Grafting latex for high-impact-resistance and high-weather-resistance ASA resin as well as preparation method and application of grafting latex
By adding a crosslinking agent in the early stage of the polymerization reaction during the preparation of ASA resin to form a shell with a gradient crosslinking structure, the problem of fragmentation of the dispersed rubber phase was solved, and the preparation of ASA resin with high impact resistance and high weather resistance was achieved.
Patent Information
- Application Number
- CN202410932532.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-12
AI Technical Summary
In the existing technology for preparing ASA resin, the problem of fragmentation of the dispersed rubber phase makes it difficult to simultaneously improve impact resistance and weather resistance.
Adding a crosslinking agent in the early stage of the graft polymerization of polybutyl acrylate latex forms a shell with a gradient crosslinking structure, ensuring the integrity of the rubber phase particles and preventing the dispersed phase from being damaged during twin-screw mixing.
It improves the impact resistance and weather resistance of ASA resin, maintains the integrity of the dispersed phase rubber particles, and enhances the impact resistance of the resin.
Smart Images

Figure BDA0004940171700000131 
Figure HDA0004940171710000011 
Figure HDA0004940171710000012
Abstract
Description
Technical Field
[0001] The invention belongs to the field of polymer preparation, and particularly relates to a polymerization method for preparing a grafted latex for high-impact and high-weatherability ASA resin. Background Art
[0002] ASA resin is often referred to as weather-resistant ABS resin. Since it uses polyacrylate (mainly butyl) rubber to replace the polybutadiene rubber in ABS, the resin does not contain a large amount of C=C, and the weather resistance of the resin is significantly improved under ultraviolet light.
[0003] As we all know, the above two resins are two-phase structure polymers, and their design concept is to use dispersed phase rubber to toughen the brittle matrix SAN resin. Since CC connected to the C=C double bond has a lower internal rotation barrier, ASA resin using polyacrylate rubber is usually less flexible than ABS resin using polybutadiene rubber, and its toughening effect on the matrix SAN resin is not good. Therefore, how to improve the impact strength of ASA resin while maintaining its weather resistance is the main product research and development direction in the industry.
[0004] At present, there are several main methods to improve the impact strength of ASA resin:
[0005] 1) Adding rubber with better impact resistance as the matrix SAN toughening dispersed phase. For example, patent CN101633769A improves the impact resistance of ASA by mixing polydiene latex into polybutyl acrylate latex and mixing powdered nitrile rubber, powdered styrene butadiene rubber and powdered polybutadiene rubber into the prepared graft copolymer. As mentioned above, this method introduces unsaturated carbon-carbon double bonds, which will cause the weather resistance of ASA to decrease.
[0006] 2) Develop new two-phase structures based on toughening mechanisms. For example, patent US4224419A uses a dispersed phase with dual-distributed particle sizes, namely polyacrylate rubber, to achieve a dual improvement in the toughening and coloring properties of SAN resin. Generally, dispersed phases of different particle sizes have different effects on the toughening mechanism of the matrix resin. Large particle sizes tend to induce silver streaks, while small particle sizes tend to induce shear bands.
[0007] 3) Improve the core-shell structure of the rubber phase. For example, patent CN105764943B uses a multilayer core-shell structure (polybutyl acrylate-polystyrene-SAN) to improve the comprehensive mechanical properties of ASA resin.
[0008] 4) Adjust the cross-linking structure of the rubber phase. For example, patents EP-A 0535456 and DE-A 4006643 propose that when DCPA is used as a cross-linking agent in the process of preparing the rubber phase, the prepared resin has improved impact resistance.
[0009] 5) Improvement is achieved by introducing other monomers into the rubber phase for copolymerization. For example, patent CN105008421B introduces N-vinyl monomers, and US5120788 introduces acrylic monomers with 8-20 carbon atoms into the rubber phase shell to improve the impact resistance of ASA resin.
[0010] However, the inventors of this application found in experimental research that in the process of preparing ASA resin by mixing the rubber dispersed phase with a core-shell structure with the matrix SAN resin, the above schemes all have the problem of dispersed phase fragmentation to varying degrees. Controlling the dispersion effect of the dispersed phase and its integrity after dispersion is the key to affecting the toughening efficiency of the SAN matrix.
[0011] Therefore, there is an urgent need to provide a method that can conveniently prepare ASA resins with both high impact resistance and high weather resistance. Summary of the invention
[0012] In view of this, the object of the present invention is to provide a grafted latex for ASA resin with high impact resistance and high weather resistance and a preparation method thereof. The grafted latex is prepared by adding a cross-linking agent in the early stage (the first 1 / 3 time) of the graft polymerization reaction of polybutyl acrylate latex, so that the grafted latex has a shell layer with a gradient cross-linked structure. When further dispersed into the SAN matrix, the shell layer with the gradient cross-linked structure can realize the binding effect on the dispersed phase rubber, thereby avoiding the breakage of the dispersed phase during the twin-screw mixing process and improving the impact resistance of the resin.
[0013] The present invention also aims to provide an ASA resin with high impact resistance and high weather resistance. The raw material is the above-mentioned grafted latex. In the subsequent process of preparing the ASA resin by twin-screw blending with SAN resin, the integrity of the rubber phase particles as the dispersed phase is maintained, ensuring that the cavitation effect of the rubber dispersed phase particles is not affected by the physical process of twin-screw blending. The prepared ASA resin not only ensures high weather resistance, but also has better impact strength.
[0014] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0015] In a first aspect, the present invention provides a method for preparing a grafted latex for a high-impact and high-weatherability ASA resin, wherein the method comprises mixing polybutyl acrylate latex with a comonomer under the conditions of a crosslinking agent and an initiator to carry out a polymerization reaction to obtain an ASA grafted latex;
[0016] The cross-linking agent is added within the first 1 / 3 of the polymerization reaction, for example, when the polymerization reaction is 1 / 10, 1 / 9, 1 / 8, 1 / 7, 1 / 6, 1 / 5, 1 / 4, 1 / 3, etc.; it can also be understood as the proportion of the cross-linking agent addition time to the polymerization reaction time. Usually, the cross-linking agent is added and the timing is started from the start of the polymerization reaction.
[0017] As a preferred embodiment of the present invention, the crosslinking agent is continuously added, preferably dropwise added; the crosslinking agent is added dropwise within the first 1 / 3 of the polymerization reaction, preferably within 1 / 5-1 / 3 of the polymerization reaction.
[0018] As a preferred embodiment of the present invention, the method for preparing the grafted latex for high impact and high weather resistance ASA resin comprises the following steps:
[0019] 1) Base-laying stage: adding polybutyl acrylate latex, and optional emulsifier, chain transfer agent, complexing agent, reducing agent, auxiliary reducing agent, and water into a reactor and stirring evenly, and then heating to the polymerization reaction temperature;
[0020] 2) Continuous dropwise polymerization stage: comonomer, initiator and crosslinking agent are added dropwise to the reactor for polymerization reaction, wherein the crosslinking agent is added within the first 1 / 3 of the polymerization reaction period, and after the reaction is completed, the grafted latex for ABS resin is obtained.
[0021] As a preferred embodiment of the present invention, in step 1), the polymerization reaction temperature is 40-90°C, such as 40°C, 50°C, 60°C, 70°C, 80°C, 90°C, etc., preferably 50-80°C.
[0022] As a preferred embodiment of the present invention, in step 2), the comonomer and initiator can be added separately or simultaneously after mixing; the comonomer and initiator are both added dropwise, and by controlling their concentrations in the system to be at a lower level, it is more conducive to forming a shell layer on the surface of polybutyl acrylate latex, and the comonomer and initiator are added dropwise for 1-5 hours, for example, 1 hour, 2 hours, 3 hours, 4 hours, 5 hours, etc.
[0023] As a preferred embodiment of the present invention, in step 2), the polymerization reaction time is 1-5h, such as 1h, 2h, 3h, 4h, 5h, etc., preferably 2-4h;
[0024] Preferably, the polymerization reaction is considered complete when the total conversion of the comonomers is >95%, e.g., 95.1%, 96%, 97%, 98%, 99%, 100%, etc.
[0025] As a preferred embodiment of the present invention, in step 1), the polybutyl acrylate latex has a particle size of 400-600nm, such as 400nm, 450nm, 500nm, 550nm, 600nm, etc., and a solid content of 30-50wt%, such as 30wt%, 35wt%, 40wt%, 45wt%, 50wt%, etc.;
[0026] The polybutyl acrylate latex is an existing product, which can be a common commercial product or prepared by itself. The preparation method is a known process in the prior art and is not specifically limited in the present invention. For example, it can be prepared with reference to the technical solution disclosed in patent GB1293791A, which will not be described in detail here.
[0027] As a preferred embodiment of the present invention, in step 2), the comonomer is selected from a mixture of vinyl cyanide and an aromatic vinyl compound; preferably, the vinyl cyanide is acrylonitrile, and the aromatic vinyl compound is styrene;
[0028] Preferably, in the mixture, the mass ratio of vinyl cyanide to aromatic vinyl compound is 1:2-5, for example, 1:2, 1:3, 1:4, 1:5, etc.
[0029] As a preferred embodiment of the present invention, in step 2), the initiator is selected from organic peroxides of C3-C18, such as organic peroxides of C3, C5, C8, C10, C15, C18, etc., preferably one or more of diisopropylbenzene peroxide, cumene hydroperoxide, and tert-butyl hydroperoxide.
[0030] As a preferred embodiment of the present invention, in step 2), the crosslinking agent is selected from one or more of aromatic compounds having two vinyl groups and acrylate compounds, preferably one or more of divinylbenzene, ethylene glycol diacrylate, ethylene glycol dimethacrylate, 1,4-butanediol dimethacrylate, and 1,6-hexanediol dimethacrylate.
[0031] As a specific embodiment of the present invention, the raw materials in step 1) also include optional emulsifiers, chain transfer agents, complexing agents, reducing agents, auxiliary reducing agents, and water, which are all conventionally selected in the field and are not particularly required by the present invention;
[0032] Preferably, the emulsifier is selected from one or more of alkyl sulfates, alkyl sulfonates, alkyl benzene sulfonates, and alkyl naphthalene sulfonates;
[0033] Preferably, the chain transfer agent is selected from one or more of n-dodecyl mercaptan, tert-dodecyl mercaptan, n-octyl mercaptan, and isooctyl mercaptan;
[0034] Preferably, the complexing agent is selected from one or more of trisodium nitrilotriacetate, disodium ethylenediaminetetraacetate, tetrasodium ethylenediaminetetraacetate, sodium pyrophosphate, and sodium hexametaphosphate, preferably disodium ethylenediaminetetraacetate;
[0035] Preferably, the reducing agent is selected from one or more of ferrous sulfate, ferrous chloride, and sodium bisulfite, preferably ferrous sulfate;
[0036] Preferably, the auxiliary reducing agent is selected from one or more of sodium dithionite, sodium formaldehyde sulfoxylate, isoascorbic acid, glucose, and lactose, preferably sodium formaldehyde sulfoxylate.
[0037] As a preferred embodiment of the present invention, the amount of the comonomer is 50-200% of the dry weight of the polybutyl acrylate latex;
[0038] Preferably, the mass ratio of the comonomer to the crosslinking agent, initiator, emulsifier, chain transfer agent, complexing agent, reducing agent, auxiliary reducing agent, and water is 100:(0.5-5):(0.1-1):(0-5):(0-1):(0-1):(0-0.01):(0-1):(0-200), for example, 100:(0.5, 1, 2, 3, 4, 5, etc.):(0.1, 0.3, 0.5, 0.7, 1, etc.):(0, 0.1, 0.5, 1, 2, 3, 4, 5, etc.):(0, 0.1, 0.3, 0.5 , 0.7, 1, etc.): (0, 0.1, 0.3, 0.5, 0.7, 1, etc.): (0, 0.001, 0.003, 0.005, 0.007, 0.01, etc.): (0, 0.1, 0.3, 0.5, 0.7, 1, etc.): (0, 1, 10, 50, 100, 150, 200, etc.), more preferably 100: (0.5-5): (0.1-1): (1-5): (0.1-1): (0.1-1): (0.001-0.01): (0.1-1): (80-200).
[0039] In a second aspect, the present invention provides a grafted latex for high-impact and high-weatherability ASA resin prepared according to the method described above.
[0040] In a third aspect, the present invention provides the use of the high-impact and high-weatherability ASA resin emulsion in the preparation of ASA resin.
[0041] Exemplarily, the present invention provides a high-impact and high-weather-resistant ASA resin, which is prepared by coagulating and demulsifying the high-impact and high-weather-resistant ASA resin with grafted latex to obtain ASA rubber powder, and then blending and extruding it with SAN resin.
[0042] As a preferred embodiment of the present invention, the SAN resin is selected from a styrene-acrylonitrile copolymer with an acrylonitrile copolymer mass ratio of 23-25%;
[0043] Preferably, the SAN resin has a weight average molecular weight of 100,000-140,000, for example, 100,000, 110,000, 120,000, 130,000, or 140,000.
[0044] The SAN resin of the present invention can be prepared by any known method (such as bulk polymerization), or can be directly purchased from commercially available products (such as LG80HF, DQ SAN327, CHIMEIPN128), without any limitation herein.
[0045] The method for coagulation and demulsification of the grafted latex for ASA resin of the present invention is known to those skilled in the art and can be operated by referring to the existing method. The present invention is not specifically limited thereto. For example, as one preferred method, the grafted latex for ASA resin is mixed with an inorganic salt (especially salts of main group IIA elements, such as one or more of magnesium sulfate, calcium chloride, barium chloride, etc.; the amount of inorganic salt added based on the latex is preferably 2-5wt%), and then aged at high temperature (for example, aged at 65-95°C for 1-5h), and then filtered and dried to obtain ASA rubber powder.
[0046] As a preferred embodiment of the present invention, the mass ratio of the ASA rubber powder and the SAN resin is (30-50):(40-80).
[0047] As a preferred embodiment of the present invention, the temperature used for the co-extrusion is 220-260° C., and then the high-impact and high-weatherability ASA resin is obtained through cooling and granulation.
[0048] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:
[0049] By adding a cross-linking agent in the early stage of the grafting polymerization reaction of polybutyl acrylate latex, the integrity of the core-shell structure of the grafted latex in the subsequent blending and extrusion process with SAN resin is improved, so that the regularity of the dispersed phase rubber particles can be maintained, thereby improving the cavitation effect of the dispersed phase rubber particles when the resin is impacted by external force, and further improving the impact resistance of the resin. BRIEF DESCRIPTION OF THE DRAWINGS
[0050] Figure 1 This is an electron microscope image of an ASA resin prepared using the ASA grafted latex provided in Example 1 as a raw material;
[0051] Figure 2 This is an electron microscope image of the ASA resin prepared using the ASA grafted latex provided in Comparative Example 1 as raw material. DETAILED DESCRIPTION
[0052] The present invention is further described below by means of specific examples. The examples described in the present invention are only used to illustrate the present invention and do not limit the scope of the present invention.
[0053] Unless otherwise specified, the raw materials used in the following specific embodiments of the present invention can be obtained through commercial sources, including:
[0054] Polybutyl acrylate latex: prepared according to the method disclosed in patent GB1293791A, particle size 427nm, solid content 43.2%;
[0055] SAN resin: brand 80HF, purchased from LG Chemical, weight average molecular weight 123,000;
[0056] Other reagents were purchased from pharmaceutical manufacturers such as Aladdin, Merck, and Sinopharm.
[0057] The main analysis methods used in the following specific embodiments of the present invention are as follows:
[0058] (1) Latex particle size: 1 g of latex was mixed with 100 g of deionized water, and the average particle size was measured using a Malvern Mastersizer laser particle size analyzer according to the dynamic laser scattering method;
[0059] (2) Latex solid content / conversion rate: 2 g of grafted latex was dried at 180°C using a Mettler HC103 moisture meter to obtain the solid content; the conversion rate of the grafting process can be calculated based on the feed formula, or the conversion rate of the grafting process can be calculated by testing the residual comonomer using gas chromatography;
[0060] (3) Impact performance test: The prepared ASA resin was sampled and subjected to impact performance test according to the GB / T1043 hard plastic simply supported beam impact test method;
[0061] (4) Weather resistance of resin: ASA resin samples were subjected to accelerated UV aging test according to ASTM G154 method. The UV aging test was carried out at 60°C for 500 hours (0.89 W / m 2 The change of resin color difference ΔE under irradiation of 340nm (0.300nm) is compared with the weather resistance of the samples;
[0062] (5) Electron microscopy test: The injection-molded ASA resin was frozen in liquid nitrogen and then sectioned. It was then stained with ruthenium tetroxide and observed under a transmission electron microscope.
[0063] Example 1
[0064] Preparation of grafted latex for high impact and weather resistance ASA resin:
[0065] 1) Laying the foundation
[0066] Add 118 parts of polybutyl acrylate latex (50 parts on dry basis, particle size 427 nm, solid content 43.2%), 1 part of sodium dodecyl sulfate, 0.25 parts of tert-dodecyl mercaptan, 0.3 parts of disodium ethylenediaminetetraacetate, 0.002 parts of ferrous sulfate, 0.4 parts of sodium formaldehyde sulfoxylate, and 40 parts of deionized water into a reaction kettle, stir and mix evenly, and heat to 65°C;
[0067] 2) Continuous dropwise polymerization stage
[0068] Maintaining a constant temperature of 65°C, 50 parts of a comonomer mixture (38 parts of styrene and 12 parts of acrylonitrile), 0.3 parts of isopropyl hydroperoxide and 1 part of divinylbenzene were uniformly added dropwise to the reaction system to start the polymerization reaction; the comonomer and isopropyl hydroperoxide were added dropwise for 3 hours, and the divinylbenzene was added dropwise for 1 hour; after the addition was completed, the reaction was continued at a constant temperature, and the reaction was stopped when the comonomer conversion rate of the sampling monitoring system was 97.3%. The polymerization reaction time was 5 hours in total (the cross-linking agent was added dropwise in the first 1 / 5 of the polymerization reaction period), and the temperature was lowered to obtain a grafted latex for ASA resin.
[0069] Example 2
[0070] Preparation of grafted latex for high impact and weather resistance ASA resin:
[0071] 1) Laying the foundation
[0072] Add 118 parts of polybutyl acrylate latex (50 parts on dry basis, particle size 427 nm, solid content 43.2%), 0.4 parts of sodium dodecylbenzene sulfonate, 0.05 parts of n-octyl mercaptan, 0.1 parts of trisodium nitrilotriacetate, 0.001 parts of ferrous chloride, 0.2 parts of sodium dithionite, and 15 parts of deionized water into a reaction kettle, stir and mix evenly, and heat to 75°C;
[0073] 2) Continuous dropwise polymerization stage
[0074] Maintaining a constant temperature of 75°C, 30 parts of a comonomer mixture (20 parts of styrene and 10 parts of acrylonitrile), 0.2 parts of tert-butyl hydroperoxide and 0.6 parts of ethylene glycol diacrylate were uniformly added dropwise to the reaction system to start a polymerization reaction; the comonomer and tert-butyl hydroperoxide were added dropwise over 2 hours, and the ethylene glycol diacrylate was added dropwise over 1 hour; after the addition was completed, the reaction was continued at a constant temperature, and the reaction was stopped when the comonomer conversion rate of the sampling monitoring system was 97.83%. The polymerization reaction time was 4 hours in total (the cross-linking agent was added dropwise in the first 1 / 4 of the polymerization reaction), and the temperature was lowered to obtain a grafted latex for ASA resin.
[0075] Example 3
[0076] Preparation of grafted latex for high impact and weather resistance ASA resin:
[0077] 1) Laying the foundation
[0078] Add 118 parts of polybutyl acrylate latex (50 parts on dry basis, particle size 427 nm, solid content 43.2%), 3 parts of sodium dodecylnaphthalene sulfonate, 0.5 parts of n-dodecyl mercaptan, 0.6 parts of sodium hexametaphosphate, 0.007 parts of sodium bisulfite, 0.2 parts of isoascorbic acid, and 100 parts of deionized water into a reaction kettle, stir and mix evenly, and heat to 55°C;
[0079] 2) Continuous dropwise polymerization stage
[0080] Maintaining a constant temperature of 55°C, 70 parts of a comonomer mixture (50 parts of styrene and 20 parts of acrylonitrile), 0.5 parts of diisopropylbenzene peroxide and 1 part of 1,4-butanediol dimethacrylate were uniformly added dropwise to the reaction system to start a polymerization reaction; the comonomer and diisopropylbenzene peroxide were added dropwise within 3 hours, and the 1,4-butanediol dimethacrylate was added dropwise within 1.5 hours; after the addition was completed, the reaction was continued at a constant temperature, and the reaction was stopped when the comonomer conversion rate of the sampling monitoring system reached 97.7%. The polymerization reaction time was 5 hours in total (the cross-linking agent was added dropwise in the first 1 / 3.3 time period of the polymerization reaction), and the temperature was lowered to obtain a grafted latex for ASA resin.
[0081] Example 4
[0082] Preparation of grafted latex for high impact and weather resistance ASA resin:
[0083] 1) Laying the foundation
[0084] Add 118 parts of polybutyl acrylate latex (50 parts on dry basis, particle size 427 nm, solid content 43.2%), 1.5 parts of sodium dodecyl sulfate, 0.3 parts of tert-dodecyl mercaptan, 0.3 parts of disodium ethylenediaminetetraacetate, 0.001 parts of ferrous sulfate, 0.2 parts of glucose, and 50 parts of deionized water into a reaction kettle, stir and mix evenly, and heat to 65°C;
[0085] 2) Continuous dropwise polymerization stage
[0086] Maintaining a constant temperature of 65°C, 60 parts of a comonomer mixture (40 parts of styrene and 20 parts of acrylonitrile), 0.3 parts of isopropylbenzene hydroperoxide and 1 part of ethylene glycol dimethacrylate were uniformly added dropwise to the reaction system to start the polymerization reaction; the comonomer and isopropylbenzene hydroperoxide were added dropwise within 3 hours, and the ethylene glycol dimethacrylate was added dropwise within 1 hour; after the addition was completed, the reaction was continued at a constant temperature, and the reaction was stopped when the comonomer conversion rate of the sampling monitoring system reached 97.5%. The polymerization reaction time was 5 hours in total (the cross-linking agent was added dropwise in the first 1 / 5 of the polymerization reaction period), and the temperature was lowered to obtain a grafted latex for ASA resin.
[0087] Example 5
[0088] Preparation of grafted latex for high impact and weather resistance ASA resin:
[0089] 1) Laying the foundation
[0090] Add 118 parts of polybutyl acrylate latex (50 parts on dry basis, particle size 427 nm, solid content 43.2%), 0.5 parts of sodium dodecyl sulfate, 0.2 parts of tert-dodecyl mercaptan, 0.1 parts of disodium ethylenediaminetetraacetate, 0.001 parts of ferrous sulfate, 0.1 parts of sodium formaldehyde sulfoxylate, and 27 parts of deionized water into a reaction kettle, stir and mix evenly, and heat to 70°C;
[0091] 2) Continuous dropwise polymerization stage
[0092] Maintaining a constant temperature of 70°C, 30 parts of a comonomer mixture (20 parts of α-methylstyrene and 10 parts of acrylonitrile), 0.2 parts of cumene hydroperoxide, and 0.3 parts of 1,6-hexanediol dimethacrylate were uniformly added to the reaction system to start the polymerization reaction; the comonomer and cumene hydroperoxide were added in 4 hours, and the 1,6-hexanediol dimethacrylate was added in 1 hour; after the addition was completed, the reaction was continued at a constant temperature, and the reaction was stopped when the comonomer conversion rate of the sampling monitoring system was 97.9%. The polymerization reaction time was 5 hours in total (the cross-linking agent was added in the first 1 / 5 of the polymerization reaction period), and the temperature was lowered to obtain the grafted latex for ASA resin.
[0093] Comparative Example 1
[0094] Preparation of grafted latex for ASA resin: Refer to the method of Example 1, except that divinylbenzene, comonomer and isopropylbenzene hydroperoxide are all added simultaneously within 3 hours, other operations and conditions remain unchanged, and the polymerization reaction time is 5 hours in total (the cross-linking agent is added in the first 3 / 5 time period of the polymerization reaction).
[0095] Comparative Example 2
[0096] Preparation of grafted latex for ASA resin: Refer to the method of Example 2, except that ethylene glycol diacrylate, comonomer and tert-butyl hydroperoxide are all added simultaneously within 2 hours, other operations and conditions remain unchanged, and the polymerization reaction time is 4 hours in total (the cross-linking agent is added in the first 1 / 2 period of the polymerization reaction).
[0097] Comparative Example 3
[0098] Preparation of grafted latex for ASA resin: Refer to the method of Example 3, except that: 1,4-butanediol dimethacrylate comonomer and diisopropylbenzene peroxide are added simultaneously within 1.7 hours, other operations and conditions remain unchanged, and the polymerization reaction time is 5 hours in total (the cross-linking agent is added in the first 1 / 2.9 time period of the polymerization reaction).
[0099] The particle size and solid content of the grafted latex for ASA resin prepared in each embodiment and comparative example were tested (see Table 1), and the grafted latex for ASA resin was used as a raw material to prepare ASA resin according to the following method:
[0100] (1) Coagulation / drying: 100 parts of the ASA grafted latex emulsion was added to a reactor, heated to 90°C, 4 parts of MgSO4 and 40 parts of deionized water were gradually added thereto, and the mixture was uniformly stirred for reaction for 1 hour. The resulting coagulated emulsion was filtered with a 200-mesh stainless steel filter cloth to obtain wet ASA rubber powder, which was dried in a fluidized bed dryer at 65°C for 1 hour to obtain ASA rubber powder with a moisture content of <1 wt%;
[0101] (2) Blending: Using a twin-screw extruder at 240° C., SAN resin (80HF) and the above-mentioned ASA rubber powder are blended in a mass ratio of 60:40, and then cooled and granulated to obtain ASA resin.
[0102] The impact strength and weather resistance of each ASA resin were tested. The test results are shown in Table 1.
[0103] Table 1. Performance test results
[0104]
[0105] Comparison of comparative examples and test data of embodiments and attached Figure 1 , 2 From the electron microscope photographs, it can be found that the integrity of the dispersed phase rubber particles of the ASA resin prepared by the present invention is maintained without large-scale damage, so that the resin can significantly improve the impact resistance while ensuring high weather resistance.
Claims
1. A method for preparing a grafted latex for high-impact and high-weather-resistant ASA resin, It is characterized in that In the presence of a crosslinking agent and an initiator, polybutyl acrylate latex is mixed with a comonomer to undergo polymerization reaction to obtain an ASA grafted latex; Wherein, the cross-linking agent is added within the first 1 / 3 period of the polymerization reaction.
2. The preparation method according to claim 1, It is characterized in that The cross-linking agent is added dropwise; More preferably, the crosslinking agent is added dropwise within 1 / 5 to 1 / 3 of the time period starting from the polymerization reaction.
3. The preparation method according to claim 1 or 2, It is characterized in that The method for preparing the grafted latex for high-impact and high-weatherability ASA resin comprises the following steps: 1) Base-laying stage: adding polybutyl acrylate latex, and optional emulsifier, chain transfer agent, complexing agent, reducing agent, auxiliary reducing agent, and water into a reactor and stirring evenly, and then heating to the polymerization reaction temperature; 2) Continuous dropwise polymerization stage: comonomer, initiator and crosslinking agent are added dropwise to the reactor for polymerization reaction, wherein the crosslinking agent is added within the first 1 / 3 of the polymerization reaction period, and after the reaction is completed, the grafted latex for ABS resin is obtained.
4. The preparation method according to claim 3, It is characterized in that In step 1), the polymerization reaction temperature is 40-90°C, preferably 50-80°C; and / or In step 2), the comonomer and initiator are added dropwise for 1-5 hours; and / or In step 2), the polymerization reaction time is 1-5h, preferably 2-4h; Preferably, the polymerization reaction is considered complete when the total conversion of the comonomers is >95%.
5. The preparation method according to claim 3 or 4, It is characterized in that In step 1), the polybutyl acrylate latex has a particle size of 400-600 nm and a solid content of 30-50 wt %; and / or In step 2), the comonomer is selected from a mixture of vinyl cyanide and an aromatic vinyl compound; preferably, the vinyl cyanide is acrylonitrile, and the aromatic vinyl compound is styrene; Preferably, in the mixture, the mass ratio of vinyl cyanide to aromatic vinyl compound is 1:2-5; and / or In step 2), the initiator is selected from C3-C18 organic peroxides, preferably one or more of diisopropylbenzene peroxide, cumene hydroperoxide, and tert-butyl hydroperoxide; and / or In step 2), the crosslinking agent is selected from one or more of aromatic compounds having two vinyl groups and acrylate compounds, preferably one or more of divinylbenzene, ethylene glycol diacrylate, ethylene glycol dimethacrylate, 1,4-butanediol dimethacrylate, and 1,6-hexanediol dimethacrylate.
6. The preparation method according to any one of claims 3 to 5, It is characterized in that In step 1), the emulsifier is selected from one or more of alkyl sulfates, alkyl sulfonates, alkyl benzene sulfonates, and alkyl naphthalene sulfonates; and / or The chain transfer agent is selected from one or more of n-dodecyl mercaptan, tert-dodecyl mercaptan, n-octyl mercaptan, and isooctyl mercaptan; and / or The complexing agent is selected from one or more of trisodium nitrilotriacetate, disodium ethylenediaminetetraacetate, tetrasodium ethylenediaminetetraacetate, sodium pyrophosphate, sodium hexametaphosphate, preferably disodium ethylenediaminetetraacetate; and / or The reducing agent is selected from one or more of ferrous sulfate, ferrous chloride, and sodium bisulfite, preferably ferrous sulfate; and / or The auxiliary reducing agent is selected from one or more of sodium dithionite, sodium formaldehyde sulfoxylate, isoascorbic acid, glucose, and lactose, preferably sodium formaldehyde sulfoxylate.
7. The preparation method according to any one of claims 3 to 6, It is characterized in that The amount of the comonomer is 50-200% of the dry weight of polybutyl acrylate latex; Preferably, the mass ratio of the comonomer to the crosslinking agent, initiator, emulsifier, chain transfer agent, complexing agent, reducing agent, auxiliary reducing agent and water is 100:(0.5-5):(0.1-1):(0-5):(0-1):(0-1):(0-0.01):(0-1):(0-200), more preferably 100:(0.5-5):(0.1-1):(1-5):(0.1-1):(0.1-1):(0.001-0.01):(0.1-1):(80-200).
8. A grafted latex for high-impact and high-weather-resistant ASA resin prepared by the preparation method according to any one of claims 1 to 7.
9. Use of the high-impact and high-weather-resistant ASA resin emulsion prepared by the preparation method according to any one of claims 1 to 7 in the preparation of ASA resin.
10. A high impact and weather resistant ASA resin, It is characterized in that The high-impact and high-weather-resistant ASA resin prepared by the preparation method according to any one of claims 1 to 7 is subjected to coagulation and demulsification with grafted latex to obtain ASA rubber powder, which is then blended and extruded with SAN resin to obtain the ASA powder.
Citation Information
Patent Citations
Method for preparing ASA (Acrylonitrile Styrene Acrylate) resin based on polymer agglomeration
CN116574351A
Acrylate-styrene-acrylonitrile graft copolymer having excellent impact-resistance, weather-resistance, and dyeability property, and method for preparing the same
KR1020130078379A
Cited By
Preparation method and application of ABS (Acrylonitrile Butadiene Styrene) grafted latex
CN119409896A
High-impact high-gloss ASA resin and preparation method thereof
CN119798880A
High-weather-resistance and high-heat-resistance ASA high-rubber-powder impact modifier and preparation method thereof
CN120865652A
A high weather-resistant and high heat-resistant ASA high-rubber powder impact modifier and its preparation method