Flexible transparent composite material and preparation method and application thereof
By combining silver nanowires with MXene nanomaterials, an AgNW/MXene/PDMS composite material with high conductivity and excellent electromagnetic properties was prepared, which solved the shortcomings of traditional materials in flexibility and transparency, and achieved efficient electromagnetic shielding effect. Suitable for high-frequency devices in the 5G era.
Patent Information
- Application Number
- CN202411176715.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-08-26
AI Technical Summary
While existing flexible transparent electromagnetic shielding materials meet high conductivity and optical transparency, they also have problems such as mechanical brittleness, low manufacturing efficiency and high cost. Especially under the trend of high frequency and miniaturization in the 5G era, traditional indium tin oxide and Metal nanowire materials are difficult to meet the needs of flexibility and transparency.
AgNW/MXene/PDMS composite material is prepared by spraying process using silver nanowires (AgNW) and transition metal carbide/carbonitride (MXene). The high conductivity of AgNW and excellent electromagnetic properties of MXene are used to combine with PDMS flexibility. and hydrophobicity, forming an electromagnetic shielding film with high light transmittance and good mechanical properties.
Achieve high-performance flexible transparent electromagnetic shielding material, with excellent electromagnetic shielding performance, high light transmittance and good mechanical properties. It is suitable for wearable devices and intelligent detection fields, reducing the contact resistance of silver nanowires and improving The overall performance of the material.
Smart Images

Figure CN118909285A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a multi-component composite material in the field of electromagnetic functional materials, and in particular to a flexible transparent composite material and a preparation method and application thereof. Background Art
[0002] In today's society, with the continuous expansion of the application of electromagnetic technology, electromagnetic interference (EMI) problems are becoming increasingly serious, posing a threat to the performance of electronic devices, system safety and human health. Especially with the advent of the 5G era, the high frequency and miniaturization trend of electronic devices has made the EMI problem more prominent. In the fields of visual windows, transparent wearable devices and aviation equipment, flexibility and transparency have become performance requirements for EMI shielding materials. Transparent and conductive films need to have satisfactory EMI shielding performance to meet the needs of practical applications. High-performance EMI shielding films require high conductivity and reasonable optical transparency. Traditional indium tin oxide (ITO) is widely used in industrial production due to its balanced conductivity and optical transparency. However, its inherent mechanical brittleness, low manufacturing efficiency and high cost limit its application in flexible wearable devices and smart detection. Therefore, the development of flexible and transparent electromagnetic shielding materials is of great significance to modern society. They can not only meet the needs of electronic devices for visual effects and portability, improve user experience, but also provide effective electromagnetic interference protection without affecting the appearance and visual clarity of the device. The low power consumption and high efficiency characteristics of such materials help reduce energy consumption and support sustainable development goals. At the same time, their high performance and reliability are also crucial to national security and military technology, and can ensure the normal operation of communication equipment and radar systems and enhance information security. Therefore, strengthening investment in the research and development of flexible transparent electromagnetic shielding materials and promoting the improvement of their technical level are of great significance to promoting social progress and sustainable development.
[0003] To date, various conductive alternatives have been reported, including carbon nanotubes (CNTs), metal nanowires, graphene, and transition metal carbide / carbonitride (MXene) sheets. Although graphene and carbon nanotubes have high transparency and good electromagnetic shielding performance, their filling amount affects transparency when meeting EMI SE requirements. Metals such as copper (Cu) are widely used due to their good conductivity and shielding effectiveness, but they have some problems such as visual obstruction, difficulty in using in micro-size scenes, and continuity problems during the manufacturing process, which limit their application. Silver nanowires (AgNWs) have been proven to be a promising material for the preparation of transparent and reliable conductors due to their excellent aspect ratio, good electrical conductivity, and excellent mechanical flexibility. In recent years, AgNW-based conductors have been widely used in fields including flexible fuel cells, stretchable and transparent supercapacitors, transparent sensors, air filters, color-changing soft robots, and flexible transparent electromagnetic interference shielding films. MXene is a type of two-dimensional material, usually composed of transition metal carbides, and its structural basis is a hexagonal layer formed by transition metals and carbon or nitrogen; due to this special composition structure, MXene materials have excellent electromagnetic and mechanical properties, as well as great specific surface area activity and strong plasticity and flexibility. Therefore, they are widely used in the manufacture of conductive inks, flexible electrodes and transparent conductive films. However, randomly distributed silver nanowires often have problems such as low transmittance and high haze, and have large contact resistance, and their conductivity often drops sharply under stretching. Therefore, reducing the contact resistance of silver nanowires while taking into account the transmittance and conductivity of the material is of great significance for improving the overall performance of the material. Summary of the invention
[0004] The present invention is made to solve the above problems, and aims to provide a flexible transparent composite material and a preparation method and application thereof.
[0005] The present invention provides a method for preparing a flexible transparent composite material, which has the following characteristics and comprises the following steps: S10, respectively preparing a transparent hydrophobic PDMS film, an AgNW dispersion and a MXene solution of a Ti3C2 material, wherein the average aspect ratio of the AgNW is about 500; S20, spraying the AgNW dispersion on the PDMS film, and then heating to obtain an AgNW / PDMS film; S30, spraying the MXene solution on the AgNW / PDMS film to obtain a MXene / AgNW / PDMS film; S40, coating another layer of PDMS on the MXene / AgNW / PDMS film, recording the newly coated layer of PDMS as an upper film, and then drying to transfer the component MXene / AgNW in the MXene / AgNW / PDMS film to the upper film; S50, peeling off the upper film, wherein the peeled-off part is an AgNW / MXene / PDMS film, i.e., a flexible transparent composite material.
[0006] In the preparation method of the flexible transparent composite material provided by the present invention, it can also have the following characteristics: wherein, step S10 includes the following sub-steps: S11, preparing a transparent hydrophobic PDMS film: mixing PDMS with a curing agent and then vacuumizing it, then mixing it with n-hexane and coating it on a substrate, drying it and washing it, and finally using 1H, 1H, 2H, 2H-perfluorodecyltrichlorosilane for modification to obtain a PDMS film; S12, preparing an AgNW dispersion: dissolving PVP in ethylene glycol, adding a metal salt solution and a silver nitrate solution, and then hydrothermally reacting to obtain AgNW, and after centrifugal separation, dispersing the AgNW in isopropanol or ethanol to obtain an AgNW dispersion; S13, preparing a solution of MXene made of Ti3C2 material: using a HCl / LiF mixed solution to etch Ti3AlC2 to obtain a Ti3C2 material MXene solution.
[0007] The method for preparing the flexible transparent composite material provided by the present invention may also have the following characteristics: wherein, in step S11, the mass of PDMS is recorded as m1, the mass of the curing agent is recorded as m2, the mass of n-hexane is recorded as m3, m1:m2=(8-12):1, (m1+m2):m3=1:(3-6), and the environment of the modification operation is vacuum heating and drying.
[0008] The method for preparing the flexible transparent composite material provided by the present invention may also have the following characteristics: wherein, in step S12, the molecular weight of PVP is 900,000 to 1,400,000, the metal salt includes any one or more of sodium chloride, ferric chloride or cupric chloride, and in the ethylene glycol solution during the hydrothermal reaction, the mass ratio of the metal salt, PVP and silver nitrate is (0.004 to 0.008):(2 to 4):1, and the concentration of silver nitrate is 0.1 to 0.15 mol / L.
[0009] The method for preparing the flexible transparent composite material provided by the present invention may also have the following characteristics: wherein the heating rate of the hydrothermal reaction is 5°C / min to 10°C / min, the reaction temperature is 140°C to 170°C, and the insulation time is 6h to 10h.
[0010] The method for preparing the flexible transparent composite material provided by the present invention may also have the following characteristics: wherein the concentration of MXene in the MXene solution is 0.2 mg / mL to 0.4 mg / mL.
[0011] The method for preparing the flexible transparent composite material provided by the present invention may also have the following characteristics: wherein, in step S20 and / or step S30, the aperture of the spray gun during spraying is 0.2 mm to 0.5 mm, the spraying pressure is 2 bar to 5 bar, and the spraying distance is 8 to 15 cm.
[0012] The method for preparing the flexible transparent composite material provided by the present invention may also have the following characteristics: wherein, in step S40, the coated PDMS is mixed with a curing agent in a mass ratio of (8 to 12):1, and a vacuum treatment is performed before drying.
[0013] The present invention also provides a flexible transparent composite material, which has the following characteristics: it is prepared by any one of the above-mentioned methods for preparing the flexible transparent composite material.
[0014] The present invention also provides an application of a flexible transparent composite material in electromagnetic shielding, which has the following characteristics: wherein the shielding performance of the flexible transparent composite material is 10-40 dB, and the light transmittance of the flexible transparent composite material is 70%-85%.
[0015] Functions and Effects of the Invention
[0016] The present invention utilizes the high conductivity and high aspect ratio of silver nanowires, combined with MXene materials with excellent electromagnetic properties, to prepare an electromagnetic shielding composite material with certain mechanical properties, high light transmittance and good flexibility. This material will have broad development space in the context of huge market demand.
[0017] The present invention can prepare AgNW / MXene / PDMS thin films with high-performance flexible transparent electromagnetic shielding through simple chemical reactions and precise spraying processes. The present invention can effectively control the network structure of AgNW and regulate the shielding performance of the composite material, thereby facilitating industrial production and having important significance for the development and wide application of electromagnetic shielding materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1is a flowchart of a method for preparing a flexible transparent composite material according to an embodiment of the present invention;
[0019] Figure 2 is a SEM image of the sample, control sample 1 and control sample 2 in the test example of the present invention at a magnification of 400×;
[0020] Figure 3 It is the transmittance spectrum and actual object comparison of the sample, control sample 1 and control sample 2 in the test example of the present invention;
[0021] Figure 4 EMI performance curves of the sample, control sample 1 and control sample 2 in the test example of the present invention. DETAILED DESCRIPTION
[0022] In order to make the technical means, creative features, objectives and effects of the present invention easy to understand, the following embodiments and drawings specifically describe a flexible transparent composite material and its preparation method and application of the present invention.
[0023] <Example>
[0024] Figure 1 It is a flowchart of a method for preparing a flexible transparent composite material according to an embodiment of the present invention.
[0025] like Figure 1 As shown, this embodiment provides a method for preparing a flexible transparent composite material, comprising the following steps:
[0026] S10, preparing a transparent hydrophobic PDMS film, an AgNW dispersion, and a Ti3C2 MXene solution, respectively, specifically comprising the following sub-steps:
[0027] S11, preparation of transparent hydrophobic PDMS film:
[0028] (1) PDMS and curing agent were mixed in a mass ratio of 10:1 and then vacuum treated for 30 minutes. The mixture was then mixed with n-hexane in a mass ratio of 1:5. After the mixture was prepared, it was coated on a clean glass substrate and placed in an oven at 80°C for 3 hours;
[0029] (2) The thin film on the glass substrate was cleaned using a plasma cleaner, and then modified using 1H,1H,2H,2H-perfluorodecyltrichlorosilane in a vacuum dryer at 80°C for 3 hours to finally obtain a transparent hydrophobic PDMS film.
[0030] S12, preparing a dispersion of AgNWs having an average high aspect ratio of about 500:
[0031] (1) Dissolve 1.6 g of PVP with a molecular weight of 1,000,000 in ethylene glycol, add 1.6 mL of 1.2 mg / mL NaCl solution, and then add 0.5 g of AgNO3;
[0032] (2) Silver nanowires were prepared by a hydrothermal method at 160° C., and then deionized water was added. Pure silver nanowires were separated by a centrifuge. The prepared silver nanowires were dispersed in isopropanol or ethanol to obtain a 0.5 mg / mL AgNW dispersion.
[0033] S13, preparation of MXene solution of Ti3C2 material:
[0034] Ti3AlC2 was etched using a mixed solution of HCl / LiF to prepare a MXene solution with a concentration of 0.2 mg / mL.
[0035] S20, preparation of AgNW / PDMS film:
[0036] (1) Place the transparent hydrophobic PDMS film with a glass substrate prepared in step S11 on a 40°C heating table, then take 5 mL of the AgNW dispersion prepared in step S12 and add it to a spray pot with a spray gun (the spray gun needle aperture size is 0.4 mm, the spraying pressure is 3 bar, and the spraying distance is 10 cm) and use the spray gun to evenly spray the AgNW dispersion on the surface of the PDMS film;
[0037] (2) The heating stage was heated to 100°C and heat treated for 5 min to obtain the AgNW / PDMS film.
[0038] S30, preparation of MXene / AgNW / PDMS film:
[0039] Take 3 mL of MXene solution and spray it on the AgNW / PDMS film using a spray gun (the aperture size of the spray gun needle is 0.4 mm, the spraying pressure is 3 bar, and the spraying distance is 10 cm) to obtain a MXene / AgNW / PDMS film.
[0040] S40, transfer:
[0041] A layer of a mixture of PDMS and curing agent in a mass ratio of 10:1 was coated on the MXene / AgNW / PDMS film. The newly coated layer of PDMS was recorded as the upper film, which was then vacuum treated for 30 minutes and kept in an 80°C oven for 3 hours to transfer the MXene / AgNW components in the MXene / AgNW / PDMS film to the upper film.
[0042] S50, obtain flexible transparent composite material:
[0043] Peel off the upper film, and the peeled part is the AgNW / MXene / PDMS film, which is a flexible transparent composite material.
[0044] This embodiment also provides a flexible transparent composite material, which is prepared by the preparation method of a flexible transparent composite material provided by this embodiment.
[0045] <Comparative Example 1>
[0046] In this comparative example, a AgNW / PDMS composite material with a micro-grid structure is prepared as a comparison by referring to steps S10, S20, S40 and S50 in the method for preparing a flexible transparent composite material provided in the embodiment.
[0047] The preparation method of the AgNW / PDMS composite material with a microgrid structure in this comparative example comprises the following steps:
[0048] Step S1, preparing a transparent hydrophobic PDMS film and an AgNW dispersion respectively, specifically comprising the following sub-steps:
[0049] Step S1-1, preparing a transparent hydrophobic PDMS film, this step is the same as step S11 in the embodiment and will not be repeated.
[0050] Step S1-2, preparing a dispersion of AgNW:
[0051] (1) 1.6 g of PVP with a molecular weight of 9,000,000 was dissolved in ethylene glycol, 1.6 mL of 1.2 mg / mL FeCl3 solution was added, and then 0.5 g of AgNO3 was added;
[0052] (2) Silver nanowires were prepared by a hydrothermal method at 150° C. The prepared silver nanowires were dispersed in isopropanol or ethanol to obtain a 0.5 mg / mL AgNW dispersion.
[0053] Step S2, preparing AgNW / PDMS film:
[0054] (1) Place the transparent hydrophobic PDMS film with a glass substrate prepared in step S1-1 on a 40°C heating table, then take 5 mL of the AgNW dispersion prepared in step S1-2 and add it to a spray pot with a spray gun (the spray gun needle aperture size is 0.3 mm, the spraying pressure is 2 bar, and the spraying distance is 10 cm) and use the spray gun to evenly spray the AgNW dispersion on the surface of the PDMS film;
[0055] (2) The heating stage was heated to 100°C and heat treated for 5 min to obtain the AgNW / PDMS film.
[0056] In order to reflect the control variables, this comparative example further includes steps S3 and S4, which are used to reflect the operation of transferring the silver nanowires in the AgNW / PDMS film to the newly coated PDMS.
[0057] Step S3, transfer: a layer of a mixture of PDMS and curing agent in a mass ratio of 10:1 is coated on the AgNW / PDMS film obtained in step S2, and the newly coated layer of PDMS is recorded as the upper film. Then, the film is vacuum treated for 30 minutes and kept in an oven at 80°C for 3 hours to transfer the component AgNW in the AgNW / PDMS film to the upper film.
[0058] Step S4, obtaining the AgNW / PDMS composite material with a micro-grid structure: peeling off the upper film, the peeled-off part is the AgNW / PDMS film, that is, the AgNW / PDMS composite material with a micro-grid structure of this comparative example.
[0059] <Comparative Example 2>
[0060] In this comparative example, an AgNW / PDMS composite material without a microgrid structure is prepared as a comparison by referring to steps S10, S20, S40 and S50 in the method for preparing a flexible transparent composite material provided in the embodiment.
[0061] The preparation method of the AgNW / PDMS composite material without a microgrid structure in this comparative example comprises the following steps:
[0062] Step S1', preparing a transparent hydrophobic PDMS film and an AgNW dispersion respectively, specifically comprises the following sub-steps:
[0063] Step S1-1', preparing a transparent hydrophobic PDMS film, this step is the same as step S11 in the embodiment and will not be repeated.
[0064] Step S1-2', preparing a dispersion of AgNW:
[0065] (1) Dissolve 1.6 g of PVP with a molecular weight of 1200000 in ethylene glycol, add 1.6 mL of 1.2 mg / mL CuCl2 solution, and then add 0.5 g of AgNO3;
[0066] (2) Silver nanowires were prepared by a hydrothermal method at 170° C. The prepared silver nanowires were dispersed in isopropanol or ethanol to obtain a 0.5 mg / mL AgNW dispersion.
[0067] Step S2', preparing AgNW / PDMS film:
[0068] The transparent hydrophobic PDMS film with a glass substrate prepared in step S1-1' was placed on a 40°C heating table, and then 5 mL of the AgNW dispersion prepared in step S1-2' was added to a spray pot with a spray gun (the spray gun needle aperture size was 0.3 mm, the spraying pressure was 2 bar, and the spraying distance was 10 cm). The AgNW dispersion was evenly sprayed on the surface of the PDMS film using the spray gun to obtain an AgNW / PDMS film.
[0069] In order to reflect the control variables, this comparative example further includes steps S3' and S4', which are used to reflect the operation of transferring the silver nanowires in the AgNW / PDMS film to the newly coated PDMS.
[0070] Step S3', transfer: a layer of a mixture of PDMS and curing agent in a mass ratio of 10:1 is coated on the AgNW / PDMS film obtained in step S2', and the newly coated layer of PDMS is recorded as the upper film. Then, it is vacuum treated for 30 minutes and kept in an oven at 80°C for 3 hours to transfer the component AgNW in the AgNW / PDMS film to the upper film.
[0071] Step S4', obtaining the AgNW / PDMS composite material without micro-grid structure: peel off the upper film, and the peeled part is the AgNW / PDMS film, that is, the AgNW / PDMS composite material without micro-grid structure of this comparative example.
[0072] <Test example>
[0073] The flexible transparent composite material in the example is recorded as sample, the AgNW / PDMS composite material with microgrid structure in comparative example 1 is recorded as control sample 1, and the AgNW / PDMS composite material without microgrid structure in comparative example 2 is recorded as control sample 2.
[0074] This test example performs corresponding tests on the sample, control sample 1 and control sample 2 and provides an application of a flexible transparent composite material in electromagnetic shielding.
[0075] Figure 2 It is a SEM image of the sample, control sample 1 and control sample 2 in the test example of the present invention at a magnification of 400×.
[0076] like Figure 2As shown, (1) for control sample 1, a clear silver nanowire microgrid structure can be observed. Each silver nanowire microgrid is composed of multiple silver nanowires. In this way, the high conductivity of the silver nanowires is maximized. In addition, the contact resistance between the silver nanowires is further reduced by heating treatment. At the same time, it can be observed that there are a large number of pores around the silver nanowires. The presence of these pores can greatly reduce the haze generated by the random distribution of the silver nanowires and improve the overall transparency of the material; (2) for the sample, it can be observed that there are dark MXene nanosheets around the silver nanowire microgrid structure. MXene is mainly attached to the silver nanowires without filling the pores. In this way, on the one hand, the influence of the presence of MXene nanosheets on the transmittance of the material is minimized. On the other hand, the attachment to the silver nanowires can further improve the overall conductivity of the material; (3) for control sample 2, it can be observed that the silver nanowires are randomly distributed. Therefore, compared with control sample 2 prepared in comparative example 2, the sample prepared in the embodiment has a more regular arrangement.
[0077] Figure 3 It is the transmittance spectrum and actual object comparison of the sample, control sample 1 and control sample 2 in the test example of the present invention.
[0078] like Figure 3 As shown, (1) from the transmittance spectrum, it can be seen that for control sample 1, the overall transmittance of the material is about 80%, while for the sample with added MXene, the overall transmittance of the material is about 76%. It can be seen that the addition of MXene has no significant effect on the transmittance of the sample prepared in the embodiment. For control sample 2, the overall transmittance of the material is about 67%. Compared with control sample 1 and the sample prepared in the embodiment, the overall transmittance of the material is lower. Therefore, the overall transmittance of the material with a microgrid structure will be higher. (2) For control sample 1, it can be observed that the material itself has a higher transmittance, which contrasts with the surrounding paper, and has a lower haze; (3) For the sample, it can be observed that the transmittance of the material itself is lower than that of control sample 1, but it still has a high transmittance. At the same time, Figure 3 As can be seen from the upper right corner of Figure b in the figure, the sample prepared in the embodiment has higher flexibility; (4) For the control sample 2, it can be observed that although the light transmittance of the material is acceptable, there is obvious haze, and the pattern on the paper under the material is obviously blurred. Therefore, compared with the control sample 2 prepared in the comparative example 2, the sample prepared in the embodiment has higher light transmittance and lower haze.
[0079] In this test example, the sample, control sample 1 and control sample 2 were cut into square specimens of 2.2×1.1×0.4 cm, respectively, and then the electromagnetic parameters of the three were measured using a vector network analyzer in the frequency range of 8.2 GHz to 12.4 GHz.
[0080] The electromagnetic shielding performance of the material mainly comes from the silver nanowire micro-grid structure in the material, which can greatly reduce the contact resistance between the silver nanowires and improve the overall conductivity of the material. In addition, MXene has excellent conductivity, and the selective attachment of MXene to the silver nanowire network can further improve the conductivity of the material while ensuring the light transmittance of the material.
[0081] Figure 4 EMI performance curves of the sample, control sample 1 and control sample 2 in the test example of the present invention.
[0082] like Figure 4 As shown, the shielding performance of the sample, control sample 1 and control sample 2 are 30.2dB, 24.7dB and 10.3dB respectively. Therefore, compared with the shielding performance of 10.3dB of control sample 2, the sample prepared in the embodiment and the control sample 1 prepared in comparative example 1 both obtain excellent shielding performance, which is sufficient to prove that the silver nanowire network with a micro-mesh structure can greatly improve the overall conductivity of the material; and adding a trace amount of MXene nanomaterial on the basis of control sample 1 can significantly improve the overall conductivity of the material, so that the material has excellent electromagnetic shielding performance.
[0083] Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A method for preparing a flexible transparent composite material, characterized in that: The following steps are involved: S10, preparing a transparent hydrophobic PDMS film, an AgNW dispersion, and a Ti3C2 MXene solution, respectively, wherein the average aspect ratio of the AgNW is about 500; S20, spraying the AgNW dispersion onto the PDMS film, and then heating to obtain an AgNW / PDMS film; S30, spraying the MXene solution onto the AgNW / PDMS film to obtain a MXene / AgNW / PDMS film; S40, coating another layer of PDMS on the MXene / AgNW / PDMS film, recording the newly coated layer of PDMS as an upper film, and then drying so that the components MXene / AgNW in the MXene / AgNW / PDMS film are transferred to the upper film; S50, peeling off the upper film, the peeled portion is the AgNW / MXene / PDMS film, that is, the flexible transparent composite material.
2. The method for preparing the flexible transparent composite material according to claim 1, characterized in that: in, Step S10 includes the following sub-steps: S11, preparing a transparent hydrophobic PDMS film: mixing PDMS with a curing agent, vacuumizing the mixture, mixing the mixture with n-hexane, coating the mixture on a substrate, drying the substrate, and washing the mixture; and finally modifying the mixture with 1H,1H,2H,2H-perfluorodecyltrichlorosilane to obtain the PDMS film; S12, preparing an AgNW dispersion: dissolving PVP in ethylene glycol, adding a metal salt solution and a silver nitrate solution to obtain AgNW by hydrothermal reaction, and dispersing the AgNW in isopropanol or ethanol after centrifugation to obtain the AgNW dispersion; S13, preparing a solution of MXene made of Ti3C2 material: etching Ti3AlC2 with a HCl / LiF mixed solution to prepare the MXene solution made of Ti3C2 material.
3. The method for preparing the flexible transparent composite material according to claim 2, characterized in that: in, In step S11, the mass of PDMS is recorded as m1, the mass of the curing agent is recorded as m2, and the mass of n-hexane is recorded as m3. m1:m2=(8~12):1,(m1+m2):m3=1:(3~6), The environment for the modification operation is vacuum heating and drying.
4. The method for preparing the flexible transparent composite material according to claim 2, characterized in that: in, In step S12, the molecular weight of PVP is 900,000 to 1,400,000. The metal salt includes any one or more of sodium chloride, ferric chloride or copper chloride. In the ethylene glycol solution during the hydrothermal reaction, the mass ratio of the metal salt, PVP and silver nitrate is (0.004-0.008):(2-4):1, and the concentration of silver nitrate is 0.1-0.15 mol / L.
5. The method for preparing the flexible transparent composite material according to claim 2 or 4, characterized in that: in, The heating rate of the hydrothermal reaction is 5°C / min to 10°C / min, the reaction temperature is 140°C to 170°C, and the insulation time is 6h to 10h.
6. The method for preparing the flexible transparent composite material according to claim 1 or 2, characterized in that: in, The concentration of MXene in the MXene solution is 0.2 mg / mL to 0.4 mg / mL.
7. The method for preparing the flexible transparent composite material according to claim 1, characterized in that: in, In step S20 and / or step S30, the aperture of the spray gun during spraying is 0.2 mm to 0.5 mm, the spraying pressure is 2 bar to 5 bar, and the spraying distance is 8 to 15 cm.
8. The method for preparing the flexible transparent composite material according to claim 1, characterized in that: in, In step S40, the coated PDMS is mixed with a curing agent in a mass ratio of (8-12):
1. Vacuum before drying.
9. A flexible transparent composite material, characterized in that: The flexible transparent composite material is prepared by the preparation method of any one of claims 1 to 8.
10. Use of the flexible transparent composite material according to claim 9 in electromagnetic shielding, in, The shielding performance of the flexible transparent composite material is 10 to 40 dB. The light transmittance of the flexible transparent composite material is 70% to 85%.
Citation Information
Patent Citations
Flexible high-strength MXene-based electromagnetic shielding composite film and preparation method thereof
CN111809439A
Preparation method of silver nanowire / MXene high-conductivity multifunctional heating and temperature sensing device
CN114220602A
Preparation method of PDMS-AgNW / MXene / AgNW composite membrane
CN117021716A
KR20220097770A