Preparation method of lignin-based Friedel-Crafts hypercrosslinked porous material with high specific surface area

By modifying the solubility and crosslinking degree of lignin in polar aprotic solvents, the problem of low specific surface area of ​​lignin-based Friedel-Crafts hypercrosslinked porous materials was solved, and porous materials with high specific surface area were prepared, expanding their application in catalysis, energy storage and environmental protection.

CN118909292APending Publication Date: 2024-11-08KUNMING UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411124214.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing technologies have difficulty effectively dissolving lignin in polar aprotic solvents, resulting in a low specific surface area of ​​lignin-based Friedel-Crafts hypercrosslinked porous materials, which limits their application in catalysis, energy storage and other fields.

Method used

Lignin was modified with pyridine/acetic anhydride solution and crosslinked in a polar aprotic solvent via Friedel-Crafts alkylation. Combined with Lewis acid catalysts and Soxhlet extraction technology, the solubility and crosslinking degree of lignin were improved, and lignin-based porous materials with high specific surface area were prepared.

Benefits of technology

The specific surface area of ​​lignin-based porous materials has reached over 50 m²/g, expanding their application potential in catalysis, energy storage, and environmental protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004995907300000011
    Figure HDA0004995907300000011
  • Figure HDA0004995907300000012
    Figure HDA0004995907300000012
  • Figure HDA0004995907300000021
    Figure HDA0004995907300000021
Patent Text Reader

Abstract

The invention discloses a preparation method of a lignin-based Friedel-Crafts hypercrosslinked porous material with a high specific surface area, which comprises the following steps: modifying lignin to improve the solubility of the lignin in a polar aprotic solvent, and reacting the modified lignin in the polar aprotic solvent in the presence of Lewis acid as a catalyst and a Friedel-Crafts alkylation reagent as a crosslinking agent to prepare the lignin-based Friedel-Crafts hypercrosslinked porous material with high specific surface area. Performing Friedel-Crafts alkylation reaction on lignin benzene rings and a cross-linking agent, and performing super-crosslinking on lignin to obtain a lignin-based porous material; the method provided by the invention has the characteristics of wide substrate source, simple reaction operation, adjustable pore structure of the target product and the like, and the obtained lignin-based super-crosslinked product has the characteristics of hierarchical porous structure, high specific surface area and the like, and has important application value in the aspects of catalysis, energy storage, environmental protection, carbon materials and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of lignin porous materials, in particular to a method for preparing a lignin-based Friedel-Crafts hypercrosslinked porous material with a high specific surface area. Background Art

[0002] Lignin is a natural high molecular polymer with a three-dimensional network structure composed of phenylpropane structural units connected by ether bonds and carbon-carbon. It has huge reserves in the plant kingdom, second only to cellulose, and is also the only renewable aromatic polymer in nature. Compared with non-renewable petroleum-based aromatic compounds, research and utilization based on lignin-based aromatic rings have great potential. However, lignin is mainly a by-product of the pulp and paper industry and biomass refining process, and most of it is incinerated for energy or discarded as waste, resulting in a large amount of resource waste. How to use lignin resources with high added value is an urgent problem to be solved.

[0003] Friedel-Crafts hypercrosslinking is one of the effective means to construct porous materials with aromatic rings as the backbone. The process is simple, and the highly crosslinked main chain creates a high specific surface area. Through directional regulation, a rich multi-level pore structure can be achieved. The unique three-dimensional network aromatic polymer structure makes lignin a potential precursor for the synthesis of hypercrosslinked polymers. At present, there have been reports on the construction of lignin-based porous materials by imitating the synthesis process of polystyrene porous materials based on lignin as a benzene ring donor and the addition of a crosslinking agent. The commonly used solvents for Friedel-Crafts alkylation reactions are polar aprotic solvents, and lignin has poor solubility in this type of solvent, resulting in the porous materials synthesized by the reaction being mainly particle surface modification, with a low specific surface area of ​​less than 50 m 2 / g. Therefore, it is still a challenge to develop lignin-based Friedel-Crafts hypercrosslinked porous materials with high specific surface area. Summary of the invention

[0004] The present invention provides a method for preparing a lignin-based Friedel-Crafts hypercrosslinked porous material with a high specific surface area, and explores a new method for modifying and improving the solubility of lignin in polar aprotic solvents, thereby increasing the degree of alkylation crosslinking of lignin by Friedel-Crafts reaction, and realizing the construction of a lignin-based porous material with a high specific surface area.

[0005] In order to achieve the above purpose, the present invention adopts the following technical means:

[0006] A method for preparing a high specific surface area lignin-based Friedel-Crafts hypercrosslinked porous material, the specific steps are as follows:

[0007] (1) dissolving lignin in a pyridine / acetic anhydride solution, stirring and reacting for 12-48 hours in the dark, pouring the reaction solution into 5-20 times the volume of ice water, collecting the precipitate, washing the precipitate with distilled water until neutral, and drying in a vacuum at 40-60° C. to obtain modified lignin;

[0008] (2) The modified lignin, the cross-linking agent and the catalyst are mixed in a solvent, and the mixture is heated to react. After the reaction is completed, a crude reactant is obtained, which is purified by Soxhlet extraction and dried to obtain a lignin-based Friedel-Crafts hyper-cross-linked porous material.

[0009] In the above step (1), the lignin is one or a mixture of any proportion of two or more of kraft lignin, alkali lignin, organic solvent lignin, enzymatic lignin, etc.

[0010] In the above step (1), the pyridine / acetic anhydride solution is obtained by mixing pyridine and acetic anhydride in a volume ratio of 1:1.

[0011] In the above step (1), the mixing ratio of the lignin to the pyridine / acetic anhydride solution is 1:20-40 (g:mL).

[0012] In the above step (2), the solvent is a polar aprotic solvent, including ethylene dichloride, acetonitrile, dimethyl sulfoxide, etc., and the mixing ratio of the modified lignin and the solvent is 1:9-45 in g:mL.

[0013] In the above step (2), the cross-linking agent is dimethylformal, benzyl dichloride, etc.

[0014] In the above step (2), the catalyst is a Lewis acid, including AlCl3, FeCl3, SnCl4, BF3, TiCl4, ZnCl2, etc.

[0015] In the above step (2), the molar ratio of the modified lignin, the cross-linking agent and the catalyst is 1:0.5-15:1-10.

[0016] In the above step (2), the atmosphere of the heating reaction is N2 atmosphere, the reaction temperature is 40-150°C, and the reaction time is 0.5-48h.

[0017] In the above step (2), the Soxhlet extraction and purification process uses a mixed solvent of one or two or more of dichloroethane and ethanol mixed in any proportion to Soxhlet extraction for more than 5 hours.

[0018] The method of the present invention uses renewable lignin as a benzene ring donor and improves its solubility in polar aprotic solvents through chemical modification, thereby solving the problem of limited Friedel-Crafts alkylation and increasing the degree of Friedel-Crafts alkylation hypercrosslinking of lignin. The specific surface area of ​​the prepared material reaches 50 m 2 / g or above, and the pore size presents a multi-level characteristic, which has important application value in catalysis, energy storage, environmental protection, carbon materials, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 is the general reaction formula of lignin modification of the present invention (acetylation reaction);

[0020] Figure 2 The general reaction formula of the modified lignin Friedel-Crafts alkylation hypercrosslinking reaction of the present invention (FDA is used as the crosslinking agent);

[0021] Figure 3 This is the BET nitrogen adsorption curve of the lignin porous material of the present invention. DETAILED DESCRIPTION

[0022] The present invention is further described in detail below in conjunction with embodiments, but the protection scope of the present invention is not limited to the described contents.

[0023] Example 1

[0024] (1) Synthesis method of modified lignin: 1.0000 g of sulfate lignin was dissolved in 20 mL of pyridine / acetic anhydride solution (pyridine and acetic anhydride were mixed in a volume ratio of 1:1), stirred in the dark for 12 h, poured the reaction solution into 5 times the volume of ice water, filtered and collected the precipitate, and washed the precipitate with distilled water until neutral, and vacuum dried to prepare modified lignin ML-1, with a yield of 34.4%;

[0025] (2) Synthesis of lignin porous material: 1.0000 g of modified lignin ML-1, 0.7407 g of catalyst AlCl3 and 0.2114 g of dimethylformal were added to 9 mL of acetonitrile, mixed evenly in a closed reactor, purged with nitrogen 4 to 5 times to exhaust the air while maintaining the nitrogen atmosphere, heated and stirred at 40°C for 0.5 hour, and then extracted with dichloroethane for 5 hours to prepare lignin porous material LP-1 with a yield of 54.5% and a specific surface area of ​​42.07 m 2 / g.

[0026] Example 2

[0027] (1) Synthesis method of modified lignin: 1.0000 g of sulfate lignin was dissolved in 30 mL of pyridine / acetic anhydride solution (pyridine and acetic anhydride were mixed in a volume ratio of 1:1), stirred and reacted for 24 h in a dark place, the reaction solution was poured into 10 times the volume of ice water, the precipitate was collected by filtration, and the precipitate was washed with distilled water until neutral, and vacuum dried to prepare modified lignin ML-2, with a yield of 90.4%;

[0028] (2) Synthesis method of lignin porous material: 1.0000 g of modified lignin ML-2, 3.7039 g of catalyst AlCl3 and 4.2272 g of dimethylformal were added to 25 mL of acetonitrile, mixed evenly in a closed reactor, purged with nitrogen for 4 to 5 times to exhaust the air while maintaining the nitrogen atmosphere, heated and stirred at 80°C for 24 hours, and then extracted with dichloroethane for 5 hours to prepare lignin porous material LP-2 with a yield of 84.5% and a specific surface area of ​​48.12 m 2 / g.

[0029] Example 3

[0030] (1) Synthesis method of modified lignin: 1.0000 g of sulfate lignin was dissolved in 40 mL of pyridine / acetic anhydride solution (pyridine and acetic anhydride were mixed in a volume ratio of 1:1), stirred and reacted for 48 h in a dark place, the reaction solution was poured into 20 times the volume of ice water, the precipitate was collected by filtration, and the precipitate was washed with distilled water until neutral, and vacuum dried to prepare modified lignin ML-3, with a yield of 95.1%;

[0031] (2) Synthesis method of lignin porous material: 1.0000 g of modified lignin ML-3, 7.4078 g of catalyst AlCl3 and 6.3408 g of dimethylformal were added to 45 mL of acetonitrile, mixed evenly in a closed reactor, purged with nitrogen for 4 to 5 times to exhaust the air while maintaining the nitrogen atmosphere, heated and stirred at 80° C. for 48 hours, and extracted with dichloroethane for 5 hours to prepare lignin porous material LP-3 with a yield of 90.12% and a specific surface area of ​​60.45 m 2 / g.

[0032] Example 4

[0033] (1) Synthesis method of modified lignin: 1.0000 g of sulfate lignin was dissolved in 40 mL of pyridine / acetic anhydride solution (pyridine and acetic anhydride were mixed in a volume ratio of 1:1), stirred and reacted for 24 h in a dark place, the reaction solution was poured into 20 times the volume of ice water, the precipitate was collected by filtration, and the precipitate was washed with distilled water until neutral, and vacuum dried to prepare modified lignin ML-4, with a yield of 94.1%;

[0034] (2) Synthesis method of lignin porous material: 1.0000 g of modified lignin ML-4, 3.7039 g of catalyst AlCl3 and 4.2272 g of dimethylformal were added to 25 mL of dimethyl sulfoxide, mixed evenly in a closed reactor, purged with nitrogen for 4 to 5 times to exhaust the air while maintaining the nitrogen atmosphere, heated and stirred at 150° C. for 24 hours, and extracted with dichloroethane for 5 hours to prepare lignin porous material LP-4 with a yield of 73.2% and a specific surface area of ​​65.23 m2 / g.

[0035] Example 5

[0036] Synthesis method of lignin porous material: 1.0000 g of modified lignin ML-4 prepared in Example 4, 3.7039 g of catalyst AlCl3 and 0.4863 g of p-dichlorobenzyl were added to 30 mL of acetonitrile, mixed evenly in a closed reactor, purged with nitrogen 4 to 5 times to exhaust the air and maintain the nitrogen atmosphere, heated and stirred at 80°C for 24 hours, and extracted with ethanol Soxhlet for 5 hours to prepare lignin porous material LP-5 with a yield of 72.6% and a specific surface area of ​​56.58 m 2 / g.

[0037] Example 6

[0038] Synthesis method of lignin porous material: 1.0000 g of modified lignin ML-4 prepared in Example 4, 3.7039 g of catalyst AlCl3 and 14.5879 g of p-dichlorobenzyl were added to 30 mL of acetonitrile, mixed evenly in a closed reactor, purged with nitrogen 4 to 5 times to exhaust the air and maintain the nitrogen atmosphere, heated and stirred at 80°C for 24 hours, and extracted with ethanol Soxhlet for 6 hours to prepare lignin porous material LP-6, with a yield of 87.62% and a specific surface area of ​​83.10 m 2 / g.

[0039] Example 7

[0040] Synthesis method of lignin porous material: 1.0000 g of modified lignin ML-4 prepared in Example 4, 3.7039 g of catalyst AlCl3 and 9.7253 g of p-dichlorobenzyl were added to 30 mL of acetonitrile, mixed evenly in a closed reactor, purged with nitrogen for 4 to 5 times to exhaust the air and maintain the nitrogen atmosphere, heated and stirred at 80°C for 24 hours, and extracted with ethanol Soxhlet for 7 hours to prepare lignin porous material LP-7 with a yield of 89.45% and a specific surface area of ​​80.26 cm 2 / g.

[0041] Example 8

[0042] Synthesis method of lignin porous material: 1.0000 g of modified lignin ML-4 prepared in Example 4, 7.4078 g of catalyst AlCl3 and 14.5879 g of p-dichlorobenzyl were added to 30 mL of dimethyl sulfoxide, mixed evenly in a closed reactor, purged with nitrogen 4 to 5 times to exhaust the air and maintain the nitrogen atmosphere, heated and stirred at 100 ° C for 24 hours, and extracted with ethanol Soxhlet for 5 hours to prepare lignin porous material LP-8, with a yield of 78.96% and a specific surface area of ​​86.43 m2 / g.

[0043] Example 9

[0044] Synthesis method of lignin porous material: 1.0000 g of modified lignin ML-4 prepared in Example 4, 3.7039 g of catalyst AlCl3 and 9.7253 g of p-dichlorobenzyl were added to 30 mL of acetonitrile, mixed evenly in a closed reactor, purged with nitrogen 4 to 5 times to exhaust the air and maintain the nitrogen atmosphere, heated and stirred at 80°C for 36 hours, and extracted with ethanol Soxhlet for 7 hours to prepare lignin porous material LP-9 with a yield of 89.32% and a specific surface area of ​​82.73 m 2 / g.

[0045] Example 10

[0046] Synthesis method of lignin porous material: 1.0000 g of modified lignin ML-4 prepared in Example 4, 7.5831 g of catalyst ZnCl2 and 9.7253 g of p-dichlorobenzyl were added to 30 mL of acetonitrile, mixed evenly in a closed reactor, purged with nitrogen for 4 to 5 times to exhaust the air and maintain the nitrogen atmosphere, heated and stirred at 80°C for 24 hours, and extracted with ethanol Soxhlet for 5 hours to prepare lignin porous material LP-10 with a yield of 82.76% and a specific surface area of ​​65.43 m 2 / g.

[0047] Embodiment 11

[0048] Synthesis method of lignin porous material: 1.0000 g of modified lignin ML-4 prepared in Example 4, 0.7573 g of catalyst ZnCl2 and 9.7253 g of p-dichlorobenzyl were added to 30 mL of acetonitrile, mixed evenly in a closed reactor, purged with nitrogen for 4 to 5 times to exhaust the air and maintain the nitrogen atmosphere, heated and stirred at 80°C for 24 hours, and extracted with ethanol Soxhlet for 5 hours to prepare lignin porous material LP-11 with a yield of 80.49% and a specific surface area of ​​60.28 m 2 / g.

[0049] Example 12

[0050] Synthesis method of lignin porous material: 1.0000 g of modified lignin ML-4 prepared in Example 4, 3.7865 g of catalyst ZnCl2 and 9.7253 g of p-dichlorobenzyl were added to 30 mL of acetonitrile, mixed evenly in a closed reactor, purged with nitrogen 4 to 5 times to exhaust the air and maintain the nitrogen atmosphere, heated and stirred at 80°C for 24 hours, and extracted with ethanol Soxhlet for 5 hours to prepare lignin porous material LP-12 with a yield of 82.45% and a specific surface area of ​​68.76 m2 / g.

[0051] Example 13

[0052] Synthesis method of lignin porous material: 1.0000 g of modified lignin ML-4 prepared in Example 4, 3.7865 g of catalyst ZnCl2 and 9.7253 g of p-dichlorobenzyl chloride were added to 30 mL of dichloroethane, mixed evenly in a closed reactor, purged with nitrogen for 4 to 5 times to exhaust the air and maintain the nitrogen atmosphere, heated and stirred at 80°C for 24 hours, and extracted with ethanol Soxhlet for 5 hours to prepare lignin porous material LP-13, with a yield of 89.45% and a specific surface area of ​​46.72 m 2 / g.

[0053] Figure 1 The general reaction formula of the acetylation modification of lignin of the present invention is as follows: the hydroxyl groups in the lignin molecules, including phenolic hydroxyl groups and alcoholic hydroxyl groups, can undergo acetylation reaction with acetic anhydride under alkaline conditions, and the acetyl groups are grafted onto the lignin molecular structure, which can improve the solubility of lignin in organic solvents to a certain extent. The solubility of the acetylated lignin in solvents such as acetonitrile and tetrahydrofuran is improved.

[0054] Figure 2 The invention discloses a general formula for the hypercrosslinking reaction of modified lignin by Friedel-Crafts alkylation, wherein dimethylol formal is an external crosslinking agent and dimethylol formal, as an alkylating agent, can be subjected to Friedel-Crafts alkylation with the vacant benzene ring of lignin under acidic conditions to form a methylene bridge between adjacent benzene rings of lignin, thereby causing a crosslinked network structure of lignin to appear.

[0055] Figure 3 This is the BET nitrogen adsorption curve of the lignin porous material LP-6 synthesized in Example 6 of the present invention. From the figure, it can be concluded that the specific surface area of ​​the lignin porous material LP-6 is 83.10 cm2 / g.

Claims

1. A method for preparing a high specific surface area lignin-based Friedel-Crafts hypercrosslinked porous material, characterized in that: The specific steps are as follows: (1) dissolving lignin in a pyridine / acetic anhydride solution, stirring and reacting for 12-48 hours in a dark environment, pouring the reaction solution into 5-20 times the volume of ice water, collecting the precipitate, washing the precipitate with distilled water until neutral, and drying in a vacuum at 40-60° C. to obtain modified lignin; (2) The modified lignin, the cross-linking agent and the catalyst are mixed in a solvent, and the mixture is heated to react. After the reaction is completed, a crude reactant is obtained, which is purified by Soxhlet extraction and dried to obtain a lignin-based Friedel-Crafts hyper-cross-linked porous material.

2. The method for preparing the high specific surface area lignin-based Friedel-Crafts hypercrosslinked porous material according to claim 1, characterized in that: In step (1), the lignin is one or a mixture of kraft lignin, alkali lignin, organic solvent lignin, and enzymatic lignin.

3. The method for preparing the high specific surface area lignin-based Friedel-Crafts hypercrosslinked porous material according to claim 1, characterized in that: In step (1), the pyridine / acetic anhydride solution is obtained by mixing pyridine and acetic anhydride in a volume ratio of 1:

1.

4. The method for preparing the high specific surface area lignin-based Friedel-Crafts hypercrosslinked porous material according to claim 1, characterized in that: In step (1), the mixing ratio of the lignin to the pyridine / acetic anhydride solution (g:mL) is 1:20-40.

5. The method for preparing the high specific surface area lignin-based Friedel-Crafts hypercrosslinked porous material according to claim 1, characterized in that: In step (2), the solvent is a polar aprotic solvent, including ethylene dichloride, acetonitrile, and dimethyl sulfoxide, and the mixing ratio of the modified lignin to the solvent is 1:9-45 (g:mL).

6. The method for preparing the high specific surface area lignin-based Friedel-Crafts hypercrosslinked porous material according to claim 1, characterized in that: In step (2), the cross-linking agent is dimethylformal or benzyl dichloride.

7. The method for preparing the high specific surface area lignin-based Friedel-Crafts hypercrosslinked porous material according to claim 1, characterized in that: In step (2), the catalyst is a Lewis acid, including AlCl3, FeCl3, SnCl4, BF3, TiCl4, and ZnCl2.

8. The method for preparing the high specific surface area lignin-based Friedel-Crafts hypercrosslinked porous material according to claim 1, characterized in that: In step (2), the molar ratio of the modified lignin, the cross-linking agent and the catalyst is 1:0.5-15:1-10.

9. The method for preparing the high specific surface area lignin-based Friedel-Crafts hypercrosslinked porous material according to claim 1, characterized in that: In step (2), the atmosphere of the heating reaction is N2 atmosphere, the reaction temperature is 40-150°C, and the reaction time is 0.5-48h.

10. The method for preparing the high specific surface area lignin-based Friedel-Crafts hypercrosslinked porous material according to claim 1, characterized in that: In step (2), the Soxhlet extraction and purification process uses a mixed solvent of one or more of dichloroethane, ethanol, and acetone for Soxhlet extraction for more than 5 hours.