Micron-sized polyether-ether-ketone microsphere as well as preparation method and application thereof

By dispersing nanobioceramic materials in polyether etherketone microspheres and forming porous structures, the problem of insufficient dispersion uniformity of inorganic fillers is solved, bone conductivity and biocompatibility are improved, bone tissue repair is promoted, and bone tissue repair is reduced. Risk of immune response.

CN118909293AActive Publication Date: 2024-11-08常州君华医疗科技有限公司 +1

Patent Information

Application Number
CN202411006895.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-08
Estimated Expiration
2044-07-25

AI Technical Summary

Technical Problem

In polymer matrix, the dispersion uniformity of the inorganic filler is insufficient, especially in medical implants requiring micron-sized particle size and porous structure, affecting the pore size, biological tissue growth and biocompatibility of the product.

Method used

By dispersing the nanobiocal ceramic material into a mixed solution of polyol and water, and adding azo bubble generator to form a foam structure, the polyether ether ketone solution is atomized and dispersed into the foam structure, solidifying to form a micron-scale poly Ether ether ketone microspheres have a particle size of less than 5 μm and have a porous microstructure.

Benefits of technology

The high-performance biological activity of microspheres is achieved, which promotes bone tissue growth and repair, improves the accuracy and mechanical properties of 3D printing products, reduces the risk of immune response, and ensures long-term stability and biocompatibility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909293A_ABST
    Figure CN118909293A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of polymer microspheres, in particular to micron-sized polyether-ether-ketone microspheres as well as a preparation method and application thereof.The preparation method comprises the following steps: S1, dispersing a nano biological ceramic material into a mixed solution of polyol and water to form a suspension, and then adding an azo bubble generating agent to form a dispersed mixed solution; meanwhile, dissolving polyether-ether-ketone in oxidizing inorganic acid to form a PEEK solution; s2, heating the dispersed mixed solution to be within the thermal decomposition temperature range of the bubble generating agent, immediately atomizing and dispersing a PEEK solution into the foamed dispersed mixed solution after foams begin to be formed, enabling the PEEK solution and the foamed dispersed mixed solution to be in contact with each other and then solidifying to form microspheres, and performing post-treatment to obtain the micron-sized polyether-ether-ketone microspheres. The microspheres obtained through the method are small in particle size, the surfaces of the microspheres are of a pit type porous structure, the nano biological ceramic materials are evenly dispersed on the surfaces and in the microspheres, and it is guaranteed that the microspheres have good long-term stable physical and chemical properties after being made into implants for use.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer microspheres, and in particular to micron-sized polyetheretherketone microspheres and a preparation method and application thereof. Background Art

[0002] Since its development, polyetheretherketone (PEEK), a high-performance thermoplastic polymer, has made significant progress in the field of medical implants. PEEK has excellent chemical stability in implantation and can resist erosion by body fluids and tissues. In addition, PEEK has good biocompatibility and does not cause significant inflammatory reactions or foreign body reactions when implanted in the body. At the same time, PEEK's strength, modulus and fatigue resistance make it an ideal material for mimicking human bones and soft tissues.

[0003] PEEK materials have many applications in the implant field. For example, in spinal implants, PEEK is used to manufacture spinal fusion devices and artificial intervertebral discs. Because its elastic modulus is similar to that of bones, it helps to reduce the stress shielding effect. In joint replacement, PEEK is used as a material for certain implant components, such as tibial spacers or joint heads. In bone defect repair, bone repair scaffolds or filling materials made of PEEK are used to repair bone defects and promote bone tissue regeneration.

[0004] Hydroxyapatite (HA) and tricalcium phosphate (β-TCP) are two commonly used bioceramic materials with good osteoconductivity and osteoinductivity. Combining these materials with PEEK can improve the biological activity of PEEK and promote the growth and repair of bone tissue. However, the uniformity of the dispersion of inorganic fillers in the polymer matrix has always been a difficult problem that needs to be broken through in this field.

[0005] In addition, 3D printing is a common preparation method for implants, but the particle size of 3D printing consumables used for medical implants has an important impact on product performance. Generally speaking, microspheres with smaller particle sizes can print finer and more uniform structures, improve printing resolution and detail expression, and may have better mechanical properties; in the application of medical implants that require a specific pore structure, the particle size of the microspheres directly affects the pore size and distribution of the product, thereby affecting permeability, growth of biological tissues, biocompatibility and other behaviors. Therefore, how to make the microspheres have a smaller particle size while combining the uniformity of filler dispersion is a technical problem to be solved in the present invention. Summary of the invention

[0006] In order to solve the above technical problems, polyetheretherketone microspheres and their preparation methods and applications are provided. The micron-sized polyetheretherketone microspheres of the present invention have uniformly dispersed bioceramic materials on the surface and inside, and the microspheres have a small particle size, and the microspheres have pits on the surface, showing a porous microstructure; the microspheres of the present invention have a small particle size and can be controlled and adjusted, and also have a porous microstructure, which is conducive to cell adhesion and proliferation, and is conducive to improving the accuracy, structural uniformity, mechanical properties, biocompatibility, etc. of 3D printed products.

[0007] In order to achieve the above objectives, the present invention is implemented through the following technical solutions:

[0008] The preparation method of micron-sized polyetheretherketone microspheres comprises the following steps:

[0009] S1, dispersing the nano-bioceramic material into a mixed solution of polyol and water to form a suspension, and then adding an azo bubble generator to form a dispersed mixed solution;

[0010] Meanwhile, polyetheretherketone is dissolved in an oxidizing inorganic acid to form a PEEK solution;

[0011] S2. The dispersed mixed liquid is heated to within the thermal decomposition temperature range of the bubble generating agent to form a foam structure, and then the PEEK solution is atomized and dispersed into the formed foam structure. The atomization process allows the PEEK solution to evenly cover the foam structure in the form of small droplets. When the small droplets of the PEEK solution contact the foam structure, the PEEK will solidify rapidly. This solidification action causes the foam structure to rupture, and the nanobioceramic material is loaded on the solidified PEEK to form microspheres. After post-processing, micron-sized polyetheretherketone microspheres loaded with nanobioceramic material are obtained, and the median particle size of the microspheres is less than 5 μm.

[0012] Furthermore, the azo bubble generator is azodicarbonamide, and the thermal decomposition temperature ranges from 180 to 225°C.

[0013] Furthermore, the average particle size of the nano bioceramic material is 20-200nm, and the nano bioceramic material is selected from nano hydroxyapatite and / or nano tricalcium phosphate; the mixed solution of polyol and water is a mixed solution of glycerol and water, wherein the mass percentage of glycerol is 80-95%.

[0014] Furthermore, the mass percentage of the nano-bioceramic material in the suspension is 1-10%; the amount of the bubble generator is in the range of 0.5-4.5% of the weight of the suspension, and preferably the amount of the bubble generator is 1-3% of the weight of the suspension.

[0015] Furthermore, the oxidizing inorganic acid is selected from concentrated sulfuric acid or concentrated nitric acid, and the mass percentage of the oxidizing inorganic acid is greater than or equal to 70%; the mass percentage of the PEEK solution is 20-35%; the mass ratio of the PEEK solution to the suspension is 1:4-8, and preferably the mass ratio of the PEEK solution to the suspension is 1:5.

[0016] Furthermore, an airflow sprayer is used to atomize the PEEK solution and disperse it into the dispersed mixed liquid forming the foam, and the airflow pressure is 0.05-0.1 MPa.

[0017] Furthermore, the post-treatment includes conventional operations such as washing, filtering, and drying.

[0018] Another aspect of the present invention provides micron-sized polyetheretherketone microspheres prepared by the above preparation method.

[0019] The last aspect of the present invention provides the use of micron-sized polyetheretherketone microspheres prepared by the above preparation method in medical implant 3D printing consumables.

[0020] Beneficial technical effects:

[0021] PEEK microsphere design: Developed new polyetheretherketone (PEEK) microspheres with surface loading of hydroxyapatite (HA) or tricalcium phosphate (β-TCP), combining the advantages of high-performance polymers and bioactive ceramics;

[0022] Innovation in preparation method: The technology combining solvent spraying and foaming is introduced to form a uniform foam structure through a bubble generator, ensuring that the microspheres have controllable porosity and particle size;

[0023] Enhanced biological activity: By loading nano-HA or β-TCP on the surface, the osteoconductivity and osteoinductivity of the microspheres are improved, promoting the growth and repair of surrounding bone tissue;

[0024] Advantages of porous structure: The porous structure of microspheres is conducive to cell adhesion and proliferation, which enhances the biocompatibility of materials and contributes to the stability of long-term implants;

[0025] Synergistic effect of composite materials: The composite of PEEK and bioceramic materials improves the overall performance of the material, including mechanical strength, biocompatibility and bone integration ability;

[0026] Customized microsphere performance: The physical and chemical properties of microspheres can be customized by adjusting the bioceramic material loading, particle size and distribution to meet different clinical needs and application scenarios;

[0027] Reduced risk of immune response: PEEK is a material with good biocompatibility. By loading bioceramics on the surface, the risk of immune response after implantation is further reduced.

[0028] Long-term stability and lasting effect: The bioceramic material loaded on the surface ensures the long-term stability of the physical and chemical properties of the microspheres in the body, ensuring that the therapeutic effect is long-lasting and effective. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is a SEM image of polyetheretherketone microspheres loaded with nano-bioceramic materials prepared in Example 1, where the scale length is 1 μm;

[0030] Figure 2 This is a SEM image of polyetheretherketone microspheres loaded with nano-bioceramic materials prepared in Example 5, where the scale length is 1 μm;

[0031] Figure 3 This is the SEM image of the polyetheretherketone microspheres loaded with nano-bioceramic material prepared in Comparative Example 2. The scale length in the image is 2 μm. DETAILED DESCRIPTION

[0032] The technical solutions in the embodiments of the present invention will be described clearly and completely below in combination with the embodiments of the present invention and the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. All other embodiments obtained by ordinary technicians in this field without creative work based on the embodiments of the present invention are within the scope of protection of the present invention.

[0033] Unless otherwise specifically stated, the numerical value set forth in these embodiments does not limit the scope of the present invention. The technology and method known to those of ordinary skill in the relevant art may not be discussed in detail, but in appropriate cases, the technology and method should be considered as a part of the specification. In all examples shown and discussed here, any specific value should be interpreted as being merely exemplary, rather than as a limitation. Therefore, other examples of exemplary embodiments may have different values.

[0034] The experimental methods in the following examples without specifying specific conditions are usually measured in accordance with national standards; if there is no corresponding national standard, the method is carried out in accordance with the general standard requirements or general methods.

[0035] The polyetheretherketone powder model used below is PEEK5600P, which is provided by Shandong Junhao High Performance Polymer Co., Ltd.

[0036] Example 1

[0037] The preparation method of micron-sized polyetheretherketone microspheres loaded with nano-bioceramic materials comprises the following steps:

[0038] S1, 5g of nano-hydroxyapatite (HA) with an average particle size of 50nm is dispersed in 95g of a glycerol-water mixed solution (90% by weight) to form a suspension with a mass percentage of 5%, and then 2g of azodicarbonamide is added as a bubble generator to form a dispersed mixed solution, and the amount of azodicarbonamide used is 2% by weight of the suspension;

[0039] Meanwhile, 6 g of polyetheretherketone powder was dissolved in 14 g of concentrated sulfuric acid (concentration 98 wt%) to form a PEEK solution with a mass percentage of 30%;

[0040] S2. The dispersed mixed liquid is heated to 200° C. to form a foam structure, and then the PEEK solution is atomized using an airflow sprayer. The generated atomized droplets are dispersed into the formed foam structure with an airflow pressure of 0.05 MPa. After the two come into contact, they solidify to form microspheres. After washing, filtering and drying, micron-sized polyetheretherketone microspheres loaded with HA are obtained.

[0041] The microsphere sizes in this case are shown in Table 1 and Figure 1 .

[0042] Example 2

[0043] The preparation method of micron-sized polyetheretherketone microspheres loaded with nano-bioceramic materials comprises the following steps:

[0044] S1, 5g of nano-hydroxyapatite (HA) with an average particle size of 50nm is dispersed in 95g of a glycerol-water mixed solution (90% by weight) to form a suspension with a mass percentage of 5%, and then 2g of azodicarbonamide is added as a bubble generator to form a dispersed mixed solution, and the amount of azodicarbonamide used is 2% by weight of the suspension;

[0045] Meanwhile, 6 g of polyetheretherketone powder was dissolved in 14 g of concentrated sulfuric acid (concentration 98 wt%) to form a PEEK solution with a mass percentage of 30%;

[0046] S2. The dispersed mixed liquid is heated to 210° C. to form a foam structure, and then the PEEK solution is atomized using an airflow sprayer. The generated atomized droplets are dispersed into the formed foam structure with an airflow pressure of 0.05 MPa. After the two come into contact, they solidify to form microspheres. After washing, filtering and drying, micron-sized polyetheretherketone microspheres loaded with HA are obtained.

[0047] The microsphere sizes in this case are shown in Table 1.

[0048] Example 3

[0049] The preparation method of micron-sized polyetheretherketone microspheres loaded with nano-bioceramic materials comprises the following steps:

[0050] S1, 5g of nano-hydroxyapatite (HA) with an average particle size of 50nm is dispersed in 95g of a glycerol-water mixed solution (90% by weight) to form a suspension with a mass percentage of 5%, and then 2g of azodicarbonamide is added as a bubble generator to form a dispersed mixed solution, and the amount of azodicarbonamide used is 2% by weight of the suspension;

[0051] Meanwhile, 6 g of polyetheretherketone powder was dissolved in 14 g of concentrated sulfuric acid (concentration 98 wt%) to form a PEEK solution with a mass percentage of 30%;

[0052] S2. The dispersed mixed liquid is heated to 220° C. to form a foam structure, and then the PEEK solution is atomized using an airflow sprayer. The generated atomized droplets are dispersed into the formed foam structure with an airflow pressure of 0.05 MPa. After the two come into contact, they solidify to form microspheres. After washing, filtering and drying, micron-sized polyetheretherketone microspheres loaded with HA are obtained.

[0053] The microsphere sizes in this case are shown in Table 1.

[0054] Example 4

[0055] The preparation method of micron-sized polyetheretherketone microspheres loaded with nano-bioceramic materials comprises the following steps:

[0056] S1, 7g of nano-tricalcium phosphate (β-TCP) with an average particle size of 100nm is dispersed in 93g of a glycerol-water mixed solution (95% by weight) to form a suspension with a mass percentage of 7%, and then 1.5g of azodicarbonamide is added as a bubble generator to form a dispersed mixed solution. The amount of azodicarbonamide used is 1.5% by weight of the suspension;

[0057] Meanwhile, 5 g of polyetheretherketone powder was dissolved in 15 g of concentrated sulfuric acid (concentration 98 wt%) to form a PEEK solution with a mass percentage of 25%;

[0058] S2. The dispersed mixed liquid is heated to 195° C. to form a foam structure, and then the PEEK solution is atomized using an airflow sprayer. The generated atomized droplets are dispersed into the formed foam structure with an airflow pressure of 0.05 MPa. After the two come into contact, they solidify to form microspheres. After washing, filtering and drying, micron-sized polyetheretherketone microspheres loaded with β-TCP are obtained.

[0059] The microsphere sizes in this case are shown in Table 1.

[0060] Example 5

[0061] The preparation method of micron-sized polyetheretherketone microspheres loaded with nano-bioceramic materials comprises the following steps:

[0062] S1, dispersing 7g of nano-tricalcium phosphate (β-TCP) with an average particle size of 20nm into 93g of a glycerol-water mixed solution (95% by weight) to form a suspension with a mass percentage of 7%, and then adding 1.5g of azodicarbonamide as a bubble generator to form a dispersed mixed solution, wherein the amount of azodicarbonamide is 1.5% by weight of the suspension;

[0063] Meanwhile, 5 g of polyetheretherketone powder was dissolved in 15 g of concentrated sulfuric acid (concentration 98 wt%) to form a PEEK solution with a mass percentage of 25%;

[0064] S2. The dispersed mixed liquid is heated to 205° C. to form a foam structure, and then the PEEK solution is atomized using an airflow sprayer. The generated atomized droplets are dispersed into the formed foam structure with an airflow pressure of 0.05 MPa. After the two come into contact, they solidify to form microspheres. After washing, filtering and drying, micron-sized polyetheretherketone microspheres loaded with β-TCP are obtained.

[0065] The microsphere sizes in this case are shown in Table 1 and Figure 2 .

[0066] Comparative Example 1

[0067] The microsphere preparation process of this case is the same as that of Example 1, except that azodicarbonamide is not added. The size of the microspheres in this case is shown in Table 1.

[0068] Comparative Example 2

[0069] The preparation process of the microspheres in this case is the same as that in Example 1, except that 5.3 g of azodicarbonamide is added to form a dispersed mixed solution, and the amount of azodicarbonamide used is 5.3% of the weight of the suspension. The size of the microspheres in this case is shown in Tables 1 and Figure 3 .

[0070] The microsphere sizes for each case are shown in Table 1.

[0071] Table 1 Microsphere size in each case

[0072]

[0073] From Table 1 and Figure 1 It can be seen that the median particle size of the microspheres prepared by the method of the present invention is in the range of 0.5-5 μm, and the microspheres have a surface pit-type porous structure, and a small amount of uniformly loaded bioceramic material can be seen on the surface.

[0074] The microspheres of the present invention have a small and controllable particle size and a porous microstructure, which is beneficial to cell adhesion and proliferation, and is beneficial to improving the accuracy, structural uniformity, mechanical properties, biocompatibility, etc. of 3D printed products.

[0075] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. Preparation method of micron-sized polyetheretherketone microspheres, It is characterized in that The steps include: S1, dispersing the nano-bioceramic material into a mixed solution of polyol and water to form a suspension, and then adding an azo bubble generator to form a dispersed mixed solution; Meanwhile, polyetheretherketone is dissolved in an oxidizing inorganic acid to form a PEEK solution; S2. The dispersed mixed liquid is heated to a temperature within the thermal decomposition range of the bubble generating agent. After forming foam, the PEEK solution is atomized and dispersed into the dispersed mixed liquid forming the foam. The two solidify to form microspheres after contact. After post-treatment, micron-sized polyetheretherketone microspheres loaded with nano-bioceramic materials are obtained, and the median particle size of the microspheres is less than 5 μm.

2. The method for preparing micron-sized polyetheretherketone microspheres according to claim 1, It is characterized in that The azo bubble generator is azodicarbonamide, and the thermal decomposition temperature ranges from 180 to 225°C.

3. The method for preparing micron-sized polyetheretherketone microspheres according to claim 2, It is characterized in that The average particle size of the nano bioceramic material is 20-200nm, and the nano bioceramic material is selected from nano hydroxyapatite and / or nano tricalcium phosphate; the mixed solution of polyol and water is a mixed solution of glycerol and water, wherein the mass percentage of glycerol is 80-95%.

4. The method for preparing micron-sized polyetheretherketone microspheres according to claim 2, It is characterized in that The mass percentage of the nano bioceramic material in the suspension is 1-10%; the amount of the bubble generator is in the range of 0.5-4.5% of the weight of the suspension.

5. The method for preparing micron-sized polyetheretherketone microspheres according to claim 2, It is characterized in that The oxidizing inorganic acid is selected from concentrated sulfuric acid or concentrated nitric acid, and the mass percentage of the oxidizing inorganic acid is greater than or equal to 70%; the mass percentage of the PEEK solution is 20-35%; the mass ratio of the PEEK solution to the suspension is 1:4-8.

6. The method for preparing micron-sized polyetheretherketone microspheres according to any one of claims 1 to 5, It is characterized in that The PEEK solution is atomized and dispersed into the dispersed mixed liquid forming the foam by using an airflow sprayer, and the airflow pressure is 0.05-0.1 MPa.

7. Micron-sized polyetheretherketone microspheres prepared by the preparation method according to any one of claims 1 to 6.

8. Application of micron-sized polyetheretherketone microspheres prepared by the preparation method according to any one of claims 1 to 6 in medical implant 3D printing consumables.

Citation Information

Patent Citations

  • Heat-expandable microsphere, process for producing the same, and use

    CN101312782A

  • PEEK (Polyether-Ether-Ketone) porous microsphere with surface coated with mineralized extracellular matrix, and preparation method and application of PEEK porous microsphere

    CN112972763A

  • Porous polyether-ether-ketone-hydroxyapatite composite material as well as preparation method and application thereof

    CN113304323A

  • Porous biological ceramic modified heating structure and preparation method and application thereof

    CN117044993A

  • Method of Polyurethane foam filter coated by hydroxy apatite titanium dioxide photocatalyst

    KR1020030075888A

Cited By

  • Porous polyaryletherketone microspheres as well as preparation method and application thereof