Preparation method of polyetheretherketone auditory ossicle prosthesis and polyetheretherketone auditory ossicle prosthesis

Polyether ether ketone small bone prosthesis was prepared through 3D printing technology, combining sulfonated polyether ether ketone, nano-hydroxyapatite and modified carbon nanotube composite materials to solve the stability and biological of metal materials in the prior art Compatibility issues achieve higher postoperative stability and biological activity.

CN119015496AActive Publication Date: 2024-11-26SUZHOU JENITEK MEDICAL CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202411114263.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-26
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

Existing metal materials such as pure titanium, titanium alloy, stainless steel, etc., are likely to cause metal ions release, high detachment rate, high stress shielding risk, poor MRI compatibility, and difficult human soft tissue to cling to. Influences postoperative stability.

Method used

3D printing technology is used to prepare polyether ether ketone small bone prosthesis, and by sintering on the surface to form a rough microporous structure, increasing attachment points, sulfonated polyether ether ketone and nano-hydroxyapatite are selected as the main mixed matrix, and modification is added Carbon nanotubes and glass fibers are treated with oxygen and argon plasma to form nano-scale structures, increasing surface hydrophilicity and biological activity.

Benefits of technology

It improves the postoperative stability and biocompatibility of the prosthesis, enhances mechanical properties and biological activity, promotes soft tissue growth and bone integration, reduces the risk of disengagement, and improves MRI compatibility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004993186320000152
    Figure BDA0004993186320000152
  • Figure BDA0004993186320000171
    Figure BDA0004993186320000171
  • Figure HDA0004993186330000011
    Figure HDA0004993186330000011
Patent Text Reader

Abstract

The invention relates to a preparation method of a polyether-ether-ketone auditory ossicle prosthesis. A 3D printing technology is adopted for integral forming. The preparation raw material is polyether-ether-ketone and / or a polyether-ether-ketone composite material. According to the application, excellent chemical stability and biocompatibility of the polyether-ether-ketone and / or the polyether-ether-ketone composite material are utilized, and the polyether-ether-ketone composite material is sintered on the surface of the auditory ossicle prosthesis through a 3D printing integrated technology to form a rough microporous structure, so that the problem that human body soft tissue blood vessels are difficult to climb is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of medical devices, and in particular to a preparation method of a polyetheretherketone auditory ossicular prosthesis and the polyetheretherketone auditory ossicular prosthesis. Background Art

[0002] The ossicles are the smallest bones in the human body, also known as the auditory ossicles. The three ossicles in each ear are composed of the malleus, incus and stapes. Most of them are located in the epitympanic cavity and are connected by ligaments and joints to form an ossicular chain. The malleus is connected to the incus, and the incus is connected to the stapes, thus forming a sequential mechanical system that can transmit sound waves from the eardrum to the inner ear and amplify the vibration of the sound to facilitate the induction of auditory cells. During the transmission process, the ossicular chain amplifies the sound through the principle of leverage, making it easier for auditory cells to perceive. When the ossicles are damaged due to disease or congenital reasons, it is generally necessary to surgically implant an ossicular prosthesis to replace the function of the ossicles.

[0003] Currently, most of the ossicular prostheses widely used in clinical practice are made of metal materials such as pure titanium, titanium alloy, and stainless steel. The release of metal ions after long-term implantation can easily lead to implant failure, high dislocation rate, high risk of stress shielding, and poor MRI compatibility. These problems have not been well solved. According to the above requirements, polyetheretherketone materials stand out due to their excellent mechanical properties, excellent biocompatibility, and elastic modulus similar to that of human bones. They are used as bone tissue repair substitutes in neurosurgery and orthopedics, and are widely used in the field of medical devices. However, due to the inertness of polyetheretherketone materials, it is also difficult for soft tissues and blood vessels in the human body to adhere to its surface, which greatly affects the postoperative stability of the product. At the same time, traditional machining and injection molding processes are difficult to solve this problem. Summary of the invention

[0004] In order to solve the problem that it is difficult for soft tissue blood vessels to attach, the present application provides a preparation method of a polyetheretherketone ossicular prosthesis and a polyetheretherketone ossicular prosthesis.

[0005] In a first aspect, the present application provides a method for preparing a polyetheretherketone ossicular prosthesis, using the following technical solution: The invention discloses a method for preparing a polyetheretherketone auditory ossicle prosthesis, which adopts 3D printing technology to form the prosthesis in one piece; the raw material for the preparation is polyetheretherketone and / or a polyetheretherketone composite material.

[0006] By adopting the above technical scheme, the excellent chemical stability and biocompatibility of polyetheretherketone and / or polyetheretherketone composite materials are utilized to prepare the ossicular prosthesis, and a rough microporous structure is sintered on the surface of the prosthesis through 3D printing technology, thereby increasing its surface area and providing more attachment points, so that the prosthesis is more firmly fixed in the position of the ossicular chain and is not easy to detach; at the same time, these rough microporous structures can also promote the growth of surrounding tissues, and effectively solve the problem that it is difficult for soft tissue blood vessels in the human body to attach, thereby further enhancing the postoperative stability of the prosthesis.

[0007] In a specific embodiment, the ossicular prosthesis includes at least one of a malleus prosthesis, an incus prosthesis, and a stapes prosthesis.

[0008] In a specific embodiment, the malleus prosthesis and the incus prosthesis are connected via a ball and socket joint.

[0009] By adopting the above technical solution, the malleus prosthesis and the incus prosthesis are connected by a ball and socket joint, so that the angle between the malleus prosthesis and the incus prosthesis can be conveniently and flexibly adjusted, which is suitable for buffering the shear stress of the artificial ossicle on the tympanic membrane when the middle ear pressure changes. At the same time, it can solve the problem that this feature cannot be assembled due to machining and injection molding processes.

[0010] In a specific embodiment, the polyetheretherketone composite material includes the following raw materials in weight percentage: 15-37% nano-hydroxyapatite, 55-72% sulfonated polyetheretherketone, 5-8% modified carbon nanotubes, and 3-5% glass fiber.

[0011] By adopting the above technical scheme, sulfonated polyetheretherketone and nano-hydroxyapatite are selected as the main mixed matrix of the ossicular prosthesis, among which sulfonated polyetheretherketone, as a semi-crystalline thermoplastic polymer, has excellent mechanical properties and chemical stability; nano-hydroxyapatite, as a bioactive ceramic, has a composition similar to that of living bone matrix and has excellent biocompatibility and osteoconductivity; at the same time, carbon nanotubes and glass fibers are added on the basis thereof, among which glass fibers have good affinity with polyetheretherketone, and their compatibility is improved by modifying the carbon nanotubes, so that the two are mixed with the main mixed matrix, thereby effectively improving the mechanical properties and biological activity of the composite material.

[0012] In a specific embodiment, the sulfonated polyetheretherketone is prepared as follows: Add polyetheretherketone into concentrated sulfuric acid solution and react for 60-100 minutes. After the reaction is completed, pour the mixed solution into an ice water bath for washing. After solids are precipitated, wash them several times with deionized water, filter and dry to obtain sulfonated polyetheretherketone.

[0013] By adopting the above technical scheme, since polyetheretherketone is biologically inert, resulting in poor bone integration effect, polyetheretherketone is sulfonated and modified, so that hydrophilic sulfonate groups are introduced into the surface of the modified polyetheretherketone, thereby improving its surface reactivity and promoting apatite formation and bone tissue growth.

[0014] In a specific embodiment, the modified carbon nanotubes are grafted with sulfonated polyetheretherketone, and the specific processing steps are as follows: (1) Carboxylation-modified carbon nanotubes: adding multi-walled carbon nanotubes to an acid solution for reaction, adding deionized water to dilute the solution after the reaction is completed, washing and centrifuging the resulting precipitate for multiple times, and then drying and grinding the precipitate to obtain carboxylation-modified carbon nanotubes; (2) Amino modified carbon nanotubes: neutralize the carboxyl modified carbon nanotubes and N,N-dimethylformamide and mix them evenly to obtain a modified carbon nanotube solution; then add 1,6-hexanediamine and N,N-dicyclohexylcarbodiimide to react, filter and wash after the reaction, and finally dry to obtain amino modified carbon nanotubes; (3) Grafting sulfonated polyetheretherketone: Aminated modified carbon nanotubes and N,N-dimethylformamide are mixed to obtain a modified carbon nanotube solution; then sulfonated polyetheretherketone and N,N-dimethylformamide are mixed to obtain a sulfonated polyetheretherketone solution; the modified carbon nanotube solution, N,N-dicyclohexylcarbodiimide and sulfonated polyetheretherketone solution are mixed and reacted, and after the reaction is completed, the mixture is filtered, washed, and finally dried and ground to obtain modified carbon nanotubes grafted with sulfonated polyetheretherketone.

[0015] By adopting the above technical scheme, carbon nanotubes have excellent mechanical properties and surface activity, but when they are directly physically blended with sulfonated polyetheretherketone, they are prone to agglomeration due to poor interface compatibility, which is not conducive to improving the mechanical properties of the composite material; by utilizing the reaction between amino groups and sulfonate groups, sulfonated polyetheretherketone is grafted onto the modified carbon nanotubes, thereby improving the compatibility with sulfonated polyetheretherketone through their similar structures, and solving the problem that carbon nanotubes are easy to agglomerate in sulfonated polyetheretherketone; first, the carbon nanotubes are carboxylated and the carboxylated carbon nanotubes are amino-modified, thereby providing a basis for the subsequent grafting of sulfonated polyetheretherketone with amino groups on carbon nanotubes, and at the same time, it is beneficial to improve the compatibility of carbon nanotubes with sulfonated polyetheretherketone and reduce agglomeration.

[0016] Preferably, the surface of the ossicular prosthesis is treated with oxygen or argon plasma.

[0017] By adopting the above technical solution, the surface of the ossicular prosthesis is treated with oxygen and argon plasma, so that high-energy particles hit the surface of the prosthesis to form an uneven nanoscale structure, increasing the surface area of ​​the matrix material, which is conducive to better adhesion of soft tissue and blood vessels in the human body.

[0018] In a specific feasible implementation scheme, the 3D printing technology is SLS selective laser sintering technology or FDM fused deposition modeling technology; during the one-piece molding process of the SLS selective laser sintering technology, the laser temperature is 332-338°C, the temperature in the printing chamber is 310-315°C, and the temperature of the printing platform is 310-315°C; during the one-piece molding process of the FDM fused deposition modeling technology, the nozzle temperature is 377-383°C and the printing base plate temperature is 257-263°C.

[0019] By adopting the above technical solution, the ossicles produced have high strength and will not crack due to high temperature, nor will they warp due to low temperature. At the same time, the surface of the ossicles obtained by sintering has uniform rough micropores, a large surface area, and many attachment points. The ossicle prosthesis produced can be firmly attached and fixed in the human body with high stability.

[0020] In a specific possible implementation scheme, the surface of the auditory ossicular prosthesis is loaded with a polydopamine layer, which is specifically prepared as follows: dopamine is dissolved in Tris-HCl buffer to prepare a dopamine solution; the auditory ossicular prosthesis is then immersed in the dopamine solution for reaction, and after the reaction is completed, it is taken out and repeatedly rinsed with deionized water, and dried to obtain the auditory ossicular prosthesis with the surface loaded with polydopamine.

[0021] By adopting the above technical scheme, due to the breakage of the polymer chains on the surface of the matrix material caused by the plasma surface treatment, new elements and functional groups are introduced on the surface by bonding with the active particles in the plasma, which is beneficial to the deposition of dopamine; at the same time, by loading a polydopamine layer on the surface of the ossicles, the biological activity of polyetheretherketone and / or polyetheretherketone composite materials is further enhanced, thereby promoting the bone integration effect.

[0022] In a specific embodiment, the polydopamine layer is also loaded with a protein composite material, which is specifically prepared as follows: The rhBMP-2 solution is prepared by dissolving rhBMP-2 in an acetic acid solution, and then the rhBMP-2 solution is adsorbed by a collagen membrane to form a spherical shape, and then freeze-dried to form a protein composite material; The protein composite material is uniformly mixed in deionized water to prepare a suspension; the auditory ossicle loaded with the polydopamine layer is placed in the suspension to react for 4-6 hours, and freeze-dried after the reaction to obtain an auditory ossicle prosthesis still loaded with the protein composite material.

[0023] By adopting the above technical scheme, polydopamine is used as a secondary reaction platform, and the adhesion of polydopamine is utilized to fix the protein composite material on the surface of the prosthesis, wherein the protein composite material is composed of type I collagen membrane and rhBMP-2, which is beneficial to promote MSCs cell proliferation and further improve the bone bonding effect.

[0024] In a second aspect, the present application provides a polyetheretherketone ossicular prosthesis, which adopts the following technical solution: The polyetheretherketone auditory ossicular prosthesis is prepared by the preparation method of the polyetheretherketone auditory ossicular prosthesis.

[0025] In summary, the present application includes at least one of the following beneficial technical effects: 1. The present application utilizes the excellent chemical stability and biocompatibility of polyetheretherketone and / or polyetheretherketone composite materials, and sinters the surface of the ossicular prosthesis to form a rough microporous structure through 3D printing integrated technology, thereby increasing its surface area and making the prosthesis more firmly fixed in the position of the ossicular chain. At the same time, these rough microporous structures can also promote the growth of surrounding tissues, and effectively solve the problem that soft tissue blood vessels in the human body are difficult to attach, thereby further enhancing the postoperative stability of the prosthesis.

[0026] 2. When the present application adopts a polyetheretherketone composite material to prepare a polyetheretherketone ossicular prosthesis, sulfonated polyetheretherketone is selected to give the ossicular prosthesis matrix excellent mechanical properties and chemical stability, and nano-hydroxyapatite is selected to give the ossicular matrix excellent biocompatibility and osteoconductivity. The advantages of the two are combined, and modified carbon nanotubes and glass fibers are added to prepare a composite matrix material with high strength and high biological activity. BRIEF DESCRIPTION OF THE DRAWINGS Figure 1 It is a schematic diagram of the structure of the polyetheretherketone ossicular prosthesis in the embodiment of the present application.

[0028] Figure 2 It is a schematic diagram of the structure of the polyetheretherketone ossicular prosthesis in the embodiment of the present application.

[0029] Explanation of the reference numerals: 1. malleus prosthesis; 2. incus prosthesis. DETAILED DESCRIPTION

[0030] In the present application, nano hydroxyphosphate was purchased from Shanghai Aladdin; the collagen membrane is specifically type I collagen membrane, purchased from Shanghai Qisheng Biology; rhBMP-2 is specifically recombinant human bone morphogenetic protein-2, purchased from Shanghai Aimejie; other raw materials can be obtained commercially.

[0031] The polyetheretherketone ossicular prosthesis of the present application comprises a malleus prosthesis and an incus prosthesis, wherein the malleus prosthesis and the incus prosthesis are connected via a ball-and-socket joint and are integrally formed by adopting 3D printing technology.

[0032] Preparation Example Preparation Example 1 Add polyetheretherketone into concentrated sulfuric acid solution to prepare a mixed solution with a mass ratio of 1:20, stir and react at a constant temperature of 50°C for 60 minutes, pour the mixed solution into an ice water bath for washing after the reaction is completed, and keep stirring during the pouring process. After solids are precipitated, wash them with deionized water for multiple times until the pH is about 7, filter and vacuum dry at 60°C for 16 hours to obtain sulfonated polyetheretherketone.

[0033] Preparation Example 2 Add polyetheretherketone into concentrated sulfuric acid solution to prepare a mixed solution with a mass ratio of 1:30, stir and react at a constant temperature of 70°C for 100 minutes, pour the mixed solution into an ice water bath for washing after the reaction is completed, and keep stirring during the pouring process. After solids are precipitated, wash them with deionized water for multiple times until the pH is about 7, filter and vacuum dry at 60°C for 24 hours to obtain sulfonated polyetheretherketone.

[0034] Preparation Example 3 The multi-walled carbon nanotubes were added into a concentrated sulfuric acid solution and a concentrated nitric acid solution in a mass ratio of 1:3 to react for 1 hour. After the reaction, deionized water was added to dilute it at room temperature for 24 hours. The purified multi-walled carbon nanotubes were washed with deionized water for multiple times and centrifuged at a speed of 10000 rpm for 20 minutes until the pH value was about 7. The multi-walled carbon nanotubes were filtered and dried at 50°C for 22 hours. After drying, the carbon nanotubes were ground to obtain carboxyl-modified carbon nanotubes.

[0035] N, N-dimethylformamide is added to the carboxyl modified carbon nanotubes to prepare a modified carbon nanotube solution with a mass ratio of 1:80, and ultrasonicated at 30°C for 30 minutes; after dispersion, 1,6-hexanediamine and N, N-dicyclohexylcarbodiimide with a mass ratio of 4:1 are weighed for condensation reflux, and then the modified carbon nanotube solution is added, and the reaction is carried out at 80°C for 22 hours. After the reaction is completed, it is filtered, and then anhydrous ethanol is added for washing. After washing, deionized water is added for secondary washing, and finally dried at 80°C for 24 hours to obtain amino-modified modified carbon nanotubes.

[0036] The amino-modified modified carbon nanotubes were ground, and then N, N-dimethylformamide was added and dispersed after ultrasonic treatment for 1 hour to prepare a modified carbon nanotube solution with a mass ratio of 1:40; the sulfonated polyetheretherketone in part of Preparation Example 1 was added to N, N-dimethylformamide and dispersed after ultrasonic treatment for 30 minutes to prepare a sulfonated polyetheretherketone solution with a mass ratio of 1:20; the modified carbon nanotube solution and N, N-dicyclohexylcarbodiimide with a mass ratio of 1:5 were condensed and refluxed, and then the sulfonated polyetheretherketone solution with a mass ratio of 5:1 to the modified carbon nanotube solution was added, and the reaction was carried out at 80°C for 28 hours. After the reaction was completed, the solution was filtered, and then anhydrous ethanol was added for several washings, and then deionized water was added for several washings, and finally dried at 60°C for 24 hours. After grinding, the modified carbon nanotubes grafted with sulfonated polyetheretherketone were obtained.

[0037] Preparation Example 4 The multi-walled carbon nanotubes were added into a concentrated sulfuric acid solution and a concentrated nitric acid solution in a mass ratio of 1:3 to react for 3 hours. After the reaction, deionized water was added to dilute it at room temperature for 24 hours. The purified multi-walled carbon nanotubes were washed with deionized water for multiple times and centrifuged at a speed of 10000 rpm for 20 minutes until the pH value was about 7. The multi-walled carbon nanotubes were filtered and dried at 70°C for 26 hours. After drying, the carbon nanotubes were ground to obtain carboxyl-modified carbon nanotubes.

[0038] N, N-dimethylformamide is added to the carboxyl modified carbon nanotubes to prepare a modified carbon nanotube solution with a mass ratio of 1:120, and ultrasonicated at 30°C for 90 minutes; after dispersion, 1,6-hexanediamine and N, N-dicyclohexylcarbodiimide with a mass ratio of 6:1 are weighed for condensation reflux, and then the modified carbon nanotube solution is added, and the reaction is carried out at 100°C for 26 hours. After the reaction is completed, it is filtered, and then anhydrous ethanol is added for washing. After washing, deionized water is added for secondary washing, and finally dried at 80°C for 24 hours to obtain amino-modified modified carbon nanotubes.

[0039] The amino-modified modified carbon nanotubes were ground, and then N, N-dimethylformamide was added and dispersed after ultrasonic treatment for 2 hours to prepare a modified carbon nanotube solution with a mass ratio of 1:60; the sulfonated polyetheretherketone in part of Preparation Example 1 was added to N, N-dimethylformamide and dispersed after ultrasonic treatment for 1 minute to prepare a sulfonated polyetheretherketone solution with a mass ratio of 1:20; the modified carbon nanotube solution and N, N-dicyclohexylcarbodiimide with a mass ratio of 1:5 were condensed and refluxed, and then the sulfonated polyetheretherketone solution with a mass ratio of 8:1 to the modified carbon nanotube solution was added, and the reaction was carried out at 120°C for 32 hours. After the reaction was completed, the mixture was filtered, and then anhydrous ethanol was added for several washings, and then deionized water was added for several washings, and finally dried at 60°C for 24 hours. After grinding, the modified carbon nanotubes grafted with sulfonated polyetheretherketone were obtained. Example

[0040] Example 1 The preparation method of the polyetheretherketone auditory ossicular prosthesis adopts 3D printing technology for one-piece molding. The preparation raw material is a polyetheretherketone composite material. The polyetheretherketone composite material includes the following raw materials: 15g of nano-hydroxyapatite, 72g of sulfonated polyetheretherketone, 8g of modified carbon nanotubes, and 5g of glass fiber; wherein the sulfonated polyetheretherketone is prepared by Preparation Example 1, and the modified carbon nanotubes are prepared by Preparation Example 3.

[0041] During the preparation, nano-hydroxyapatite, sulfonated polyetheretherketone, modified carbon nanotubes and glass fiber are added into N,N-dimethylformamide and mixed, and stirred continuously for 30 minutes at a stirring rate of 8000r / min. The material is discharged into a 50% ethanol solution, boiled and washed, and dried at 150°C for 24 hours to obtain a composite powder.

[0042] The composite powder was extruded through a twin-screw extruder at 300°C to obtain a 3D printing-specific filament with a wire diameter of 1.75±0.05mm and uniform thickness; the 3D printing-specific filament was dried at 150°C for 24h, and then subjected to fused deposition molding by a 3D printer with a nozzle temperature of 380°C, a printing speed of 40mm / s, a printing layer thickness of 0.2mm, a printing base plate temperature of 260°C, and a porosity of the scaffold material of 70%, to finally obtain a 3D printed ossicular prosthesis.

[0043] After printing, the ossicular prosthesis was ultrasonically cleaned with acetone, anhydrous ethanol and deionized water for 10 minutes in sequence to remove surface contaminants; finally, the ossicular prosthesis was dried at 70°C for 48 hours; The surface was treated with 30% oxygen and 70% argon low-temperature plasma for 5 minutes under the conditions of 400V voltage and 10Pa pressure. After the treatment, it was ultrasonically cleaned with deionized water for 5 minutes and dried to obtain the plasma-treated ossicular prosthesis.

[0044] Prepare 10mmol / L Tris-HCl buffer; dissolve dopamine in Tris-HCl buffer to prepare a dopamine solution with a pH of 8.5 and a concentration of 2g / L; then immerse the auditory ossicle prosthesis in the dopamine solution, shake and react at 37°C for 24h, take out and ultrasonically rinse with deionized water for 3min to remove the dopamine not loaded on the surface, and then dry to obtain the auditory ossicle prosthesis with polydopamine loaded on the surface.

[0045] The polydopamine-loaded ossicular prosthesis was sterilized by ethylene oxide or cobalt-60 and then stored aseptically under vacuum until use.

[0046] Example 2 The preparation method of the polyetheretherketone auditory ossicular prosthesis adopts 3D printing technology for one-piece molding. The preparation raw material is a polyetheretherketone composite material. The polyetheretherketone composite material includes the following raw materials: 26g of nano-hydroxyapatite, 63.5g of sulfonated polyetheretherketone, 6.5g of modified carbon nanotubes, and 4g of glass fiber; wherein the sulfonated polyetheretherketone is prepared by Preparation Example 1, and the modified carbon nanotubes are prepared by Preparation Example 3.

[0047] During the preparation, nano-hydroxyapatite, sulfonated polyetheretherketone, modified carbon nanotubes and glass fiber are added into N,N-dimethylformamide and mixed, and stirred continuously for 30 minutes at a stirring rate of 8000r / min. The material is discharged into a 50% ethanol solution, boiled and washed, and dried at 150°C for 24 hours to obtain a composite powder.

[0048] The composite powder was extruded through a twin-screw extruder at 300°C to obtain a 3D printing-specific filament with a wire diameter of 1.75±0.05mm and uniform thickness; the 3D printing-specific filament was dried at 150°C for 24h, and then subjected to fused deposition molding by a 3D printer with a nozzle temperature of 380°C, a printing speed of 40mm / s, a printing layer thickness of 0.2mm, a printing base plate temperature of 260°C, and a porosity of the scaffold material of 70%, to finally obtain a 3D printed ossicular prosthesis.

[0049] After printing, the ossicular prosthesis was ultrasonically cleaned with acetone, anhydrous ethanol and deionized water for 10 minutes in sequence to remove surface contaminants; finally, the ossicular prosthesis was dried at 70°C for 48 hours; The surface was treated with 30% oxygen and 70% argon low-temperature plasma for 5 minutes under the conditions of 400V voltage and 10Pa pressure. After the treatment, it was ultrasonically cleaned with deionized water for 5 minutes and dried to obtain the plasma-treated ossicular prosthesis.

[0050] Prepare 10mmol / L Tris-HCl buffer; dissolve dopamine in Tris-HCl buffer to prepare a dopamine solution with a pH of 8.5 and a concentration of 2g / L; then immerse the auditory ossicle prosthesis in the dopamine solution, shake and react at 37°C for 24h, take out and ultrasonically rinse with deionized water for 3min to remove the dopamine not loaded on the surface, and then dry to obtain the auditory ossicle prosthesis with polydopamine loaded on the surface.

[0051] The polydopamine-loaded ossicular prosthesis was sterilized by ethylene oxide or cobalt-60 and then stored aseptically under vacuum until use.

[0052] Example 3 The preparation method of the polyetheretherketone auditory ossicular prosthesis adopts 3D printing technology for one-piece molding. The preparation raw material is a polyetheretherketone composite material. The polyetheretherketone composite material includes the following raw materials: 37g of nano-hydroxyapatite, 55g of sulfonated polyetheretherketone, 5g of modified carbon nanotubes, and 3g of glass fiber; wherein the sulfonated polyetheretherketone is prepared by Preparation Example 1, and the modified carbon nanotubes are prepared by Preparation Example 3.

[0053] During the preparation, nano-hydroxyapatite, sulfonated polyetheretherketone, modified carbon nanotubes and glass fiber are added into N,N-dimethylformamide and mixed, and stirred continuously for 30 minutes at a stirring rate of 8000r / min. The material is discharged into a 50% ethanol solution, boiled and washed, and dried at 150°C for 24 hours to obtain a composite powder.

[0054] The composite powder was extruded through a twin-screw extruder at 300°C to obtain a 3D printing-specific filament with a wire diameter of 1.75±0.05mm and uniform thickness; the 3D printing-specific filament was dried at 150°C for 24h, and then subjected to fused deposition molding by a 3D printer with a nozzle temperature of 380°C, a printing speed of 40mm / s, a printing layer thickness of 0.2mm, a printing base plate temperature of 260°C, and a porosity of the scaffold material of 70%, to finally obtain a 3D printed ossicular prosthesis.

[0055] After printing, the ossicular prosthesis was ultrasonically cleaned with acetone, anhydrous ethanol and deionized water for 10 minutes in sequence to remove surface contaminants; finally, the ossicular prosthesis was dried at 70°C for 48 hours; The surface was treated with 30% oxygen and 70% argon low-temperature plasma for 5 minutes under the conditions of 400V voltage and 10Pa pressure. After the treatment, it was ultrasonically cleaned with deionized water for 5 minutes and dried to obtain the plasma-treated ossicular prosthesis.

[0056] Prepare 10mmol / L Tris-HCl buffer; dissolve dopamine in Tris-HCl buffer to prepare a dopamine solution with a pH of 8.5 and a concentration of 2g / L; then immerse the auditory ossicle prosthesis in the dopamine solution, shake and react at 37°C for 24h, take out and ultrasonically rinse with deionized water for 3min to remove the dopamine not loaded on the surface, and then dry to obtain the auditory ossicle prosthesis with polydopamine loaded on the surface.

[0057] The polydopamine-loaded ossicular prosthesis was sterilized by ethylene oxide or cobalt-60 and then stored aseptically under vacuum until use.

[0058] Example 4 The only difference between this embodiment and Embodiment 1 is that the sulfonated polyetheretherketone is prepared by Preparation Example 2.

[0059] Example 5 The only difference between this embodiment and embodiment 1 is that the modified carbon nanotubes are prepared by preparation example 4.

[0060] Example 6 The only difference between this embodiment and embodiment 1 is that the polyetheretherketone composite material includes the following raw materials: 15 g of nano-hydroxyapatite, 72 g of sulfonated polyetheretherketone, and 13 g of modified carbon nanotubes.

[0061] Example 7 The only difference between this embodiment and embodiment 1 is that the polyetheretherketone composite material includes the following raw materials: 15 g of nano-hydroxyapatite, 72 g of sulfonated polyetheretherketone, and 13 g of glass fiber.

[0062] Example 8 The only difference between this embodiment and embodiment 1 is that the polyetheretherketone composite material includes the following raw materials: 15 g of nano-hydroxyapatite and 85 g of sulfonated polyetheretherketone.

[0063] Example 9 The difference between this embodiment and embodiment 1 is that the polyetheretherketone composite material includes the following raw materials: 15 g of nano-hydroxyapatite, 72 g of sulfonated polyetheretherketone, 8 g of carbon nanotubes, and 5 g of glass fiber.

[0064] Example 10 The only difference between this embodiment and embodiment 1 is that the surface is treated with 30% oxygen and 70% argon low-temperature plasma for 15 minutes under the conditions of 450V voltage and 15Pa pressure, and after treatment, it is ultrasonically cleaned with deionized water for 5 minutes and dried to obtain the plasma-treated ossicular prosthesis.

[0065] Embodiment 11 The only difference between this embodiment and embodiment 1 is that the surface is treated with 30% oxygen and 70% argon low-temperature plasma for 25 minutes under the conditions of 500V voltage and 20Pa pressure, and then ultrasonically cleaned with deionized water for 5 minutes and dried to obtain the plasma-treated ossicular prosthesis.

[0066] Example 12 The preparation method of the polyetheretherketone auditory ossicular prosthesis adopts 3D printing technology for one-piece molding. The preparation raw material is a polyetheretherketone composite material. The polyetheretherketone composite material includes the following raw materials: 15g of nano-hydroxyapatite, 72g of sulfonated polyetheretherketone, 8g of modified carbon nanotubes, and 5g of glass fiber; wherein the sulfonated polyetheretherketone is prepared by Preparation Example 1, and the modified carbon nanotubes are prepared by Preparation Example 3.

[0067] During the preparation, nano-hydroxyapatite, sulfonated polyetheretherketone, modified carbon nanotubes and glass fiber are added into N,N-dimethylformamide and mixed, and stirred continuously for 30 minutes at a stirring rate of 8000r / min. The material is discharged into a 50% ethanol solution, boiled and washed, and dried at 150°C for 24 hours to obtain a composite powder.

[0068] The composite powder was extruded through a twin-screw extruder at 300°C to obtain a 3D printing-specific filament with a wire diameter of 1.75±0.05mm and uniform thickness; the 3D printing-specific filament was dried at 150°C for 24h, and then subjected to fused deposition molding by a 3D printer with a nozzle temperature of 380°C, a printing speed of 40mm / s, a printing layer thickness of 0.2mm, a printing base plate temperature of 260°C, and a porosity of the scaffold material of 70%, to finally obtain a 3D printed ossicular prosthesis.

[0069] After printing, the ossicular prosthesis was ultrasonically cleaned with acetone, anhydrous ethanol and deionized water for 10 minutes in sequence to remove surface contaminants; finally, the ossicular prosthesis was dried at 70°C for 48 hours; Prepare 10mmol / L Tris-HCl buffer; dissolve dopamine in Tris-HCl buffer to prepare a dopamine solution with a pH of 8.5 and a concentration of 2g / L; then immerse the auditory ossicle prosthesis in the dopamine solution, shake and react at 37°C for 24h, take out and ultrasonically rinse with deionized water for 3min to remove the dopamine not loaded on the surface, and then dry to obtain the auditory ossicle prosthesis with polydopamine loaded on the surface.

[0070] The polydopamine-loaded ossicular prosthesis was sterilized by ethylene oxide or cobalt-60 and then stored aseptically under vacuum until use.

[0071] Embodiment 13 The preparation method of the polyetheretherketone auditory ossicular prosthesis adopts 3D printing technology for one-piece molding. The preparation raw material is a polyetheretherketone composite material. The polyetheretherketone composite material includes the following raw materials: 15g of nano-hydroxyapatite, 72g of sulfonated polyetheretherketone, 8g of modified carbon nanotubes, and 5g of glass fiber; wherein the sulfonated polyetheretherketone is prepared by Preparation Example 1, and the modified carbon nanotubes are prepared by Preparation Example 3.

[0072] During the preparation, nano-hydroxyapatite, sulfonated polyetheretherketone, modified carbon nanotubes and glass fiber are added into N,N-dimethylformamide and mixed, and stirred continuously for 30 minutes at a stirring rate of 8000r / min. The material is discharged into a 50% ethanol solution, boiled and washed, and dried at 150°C for 24 hours to obtain a composite powder.

[0073] The composite powder was extruded through a twin-screw extruder at 300°C to obtain a 3D printing-specific filament with a wire diameter of 1.75±0.05mm and uniform thickness; the 3D printing-specific filament was dried at 150°C for 24h, and then subjected to fused deposition molding by a 3D printer with a nozzle temperature of 380°C, a printing speed of 40mm / s, a printing layer thickness of 0.2mm, a printing base plate temperature of 260°C, and a porosity of the scaffold material of 70%, to finally obtain a 3D printed ossicular prosthesis.

[0074] After printing, the ossicular prosthesis was ultrasonically cleaned with acetone, anhydrous ethanol and deionized water for 10 minutes in sequence to remove surface contaminants; finally, the ossicular prosthesis was dried at 70°C for 48 hours; The surface was treated with 30% oxygen and 70% argon low-temperature plasma for 5 minutes under the conditions of 400V voltage and 10Pa pressure. After the treatment, it was ultrasonically cleaned with deionized water for 5 minutes and dried to obtain the plasma-treated ossicular prosthesis.

[0075] Prepare 10mmol / L Tris-HCl buffer; dissolve dopamine in Tris-HCl buffer to prepare a dopamine solution with a pH of 8.5 and a concentration of 2g / L; then immerse the auditory ossicle prosthesis in the dopamine solution, shake and react at 37°C for 24h, take out and ultrasonically rinse with deionized water for 3min to remove the dopamine not loaded on the surface, and then dry to obtain the auditory ossicle prosthesis with polydopamine loaded on the surface.

[0076] Dissolve rhBMP-2 in acetic acid solution to prepare a concentration of 100 μg / mL -1 The rhBMP-2 solution was then adsorbed on a 5cm×5cm×0.5cm collagen membrane to form a spherical shape with a diameter of 0.8cm, which was then freeze-dried to form a protein composite material. The protein composite material is uniformly mixed in deionized water to prepare a suspension with a mass ratio of 1:100; the ossicle loaded with the polydopamine layer is placed in the suspension for reaction for 4 hours, and freeze-dried after the reaction to obtain an ossicular prosthesis also loaded with the protein composite material. The ossicular prosthesis is sterilized with ethylene oxide or cobalt-60, and then stored aseptically under vacuum until use.

[0077] Embodiment 14 The only difference between this embodiment and embodiment 13 is that the auditory ossicles loaded with the polydopamine layer are placed in the suspension to react for 6 hours.

[0078] Embodiment 15 The preparation method of the polyetheretherketone auditory ossicular prosthesis adopts 3D printing technology for one-piece molding. The preparation raw material is a polyetheretherketone composite material. The polyetheretherketone composite material includes the following raw materials: 15g of nano-hydroxyapatite, 72g of sulfonated polyetheretherketone, 8g of modified carbon nanotubes, and 5g of glass fiber; wherein the sulfonated polyetheretherketone is prepared by Preparation Example 1, and the modified carbon nanotubes are prepared by Preparation Example 3.

[0079] During the preparation, nano-hydroxyapatite, sulfonated polyetheretherketone, modified carbon nanotubes and glass fiber are added into N,N-dimethylformamide and mixed, and stirred continuously for 30 minutes at a stirring rate of 8000r / min. The material is discharged into a 50% ethanol solution, boiled and washed, and dried at 150°C for 24 hours to obtain a composite powder.

[0080] The composite powder was extruded through a twin-screw extruder at 300°C to obtain a 3D printing-specific filament with a wire diameter of 1.75±0.05mm and uniform thickness; the 3D printing-specific filament was dried at 150°C for 24h, and then subjected to fused deposition molding by a 3D printer with a nozzle temperature of 380°C, a printing speed of 40mm / s, a printing layer thickness of 0.2mm, a printing base plate temperature of 260°C, and a porosity of the scaffold material of 70%, to finally obtain a 3D printed ossicular prosthesis.

[0081] After printing, the ossicular prosthesis was ultrasonically cleaned with acetone, anhydrous ethanol and deionized water for 10 minutes in sequence to remove surface contaminants; finally, the ossicular prosthesis was dried at 70°C for 48 hours; The surface was treated with 30% oxygen and 70% argon low-temperature plasma for 5 minutes under the conditions of 400V voltage and 10Pa pressure. After the treatment, it was ultrasonically cleaned with deionized water for 5 minutes and dried to obtain the plasma-treated ossicular prosthesis.

[0082] The ossicular prosthesis is sterilized by ethylene oxide or cobalt-60 and then stored aseptically under vacuum until use.

[0083] Example 16 The preparation method of the polyetheretherketone auditory ossicular prosthesis adopts 3D printing technology for one-piece molding. The preparation raw material is a polyetheretherketone composite material. The polyetheretherketone composite material includes the following raw materials: 15g of nano-hydroxyapatite, 72g of sulfonated polyetheretherketone, 8g of modified carbon nanotubes, and 5g of glass fiber; wherein the sulfonated polyetheretherketone is prepared by Preparation Example 1, and the modified carbon nanotubes are prepared by Preparation Example 3.

[0084] During the preparation, nano-hydroxyapatite, sulfonated polyetheretherketone, modified carbon nanotubes and glass fiber are added into N,N-dimethylformamide and mixed, and stirred continuously for 30 minutes at a stirring rate of 8000r / min. The material is discharged into a 50% ethanol solution, boiled and washed, and dried at 150°C for 24 hours to obtain a composite powder.

[0085] The composite powder was subjected to SLS selective laser sintering molding through a 3D printer. The laser temperature was 335°C, the temperature in the printing chamber was 310°C, the temperature of the printing base was 310°C, the scanning speed was 1200mm / s, the printing layer thickness was 0.2mm, and the porosity of the scaffold material was set to 70%, ultimately obtaining a 3D printed ossicular prosthesis.

[0086] After printing, the ossicular prosthesis was ultrasonically cleaned with acetone, anhydrous ethanol and deionized water for 10 minutes in sequence to remove surface contaminants; finally, the ossicular prosthesis was dried at 70°C for 48 hours; The surface was treated with 30% oxygen and 70% argon low-temperature plasma for 5 minutes under the conditions of 400V voltage and 10Pa pressure. After the treatment, it was ultrasonically cleaned with deionized water for 5 minutes and dried to obtain the plasma-treated ossicular prosthesis.

[0087] Prepare 10mmol / L Tris-HCl buffer; dissolve dopamine in Tris-HCl buffer to prepare a dopamine solution with a pH of 8.5 and a concentration of 2g / L; then immerse the auditory ossicle prosthesis in the dopamine solution, shake and react at 37°C for 24h, take out and ultrasonically rinse with deionized water for 3min to remove the dopamine not loaded on the surface, and then dry to obtain the auditory ossicle prosthesis with polydopamine loaded on the surface.

[0088] The polydopamine-loaded ossicular prosthesis was sterilized by ethylene oxide or cobalt-60 and then stored aseptically under vacuum until use.

[0089] Embodiment 17 The preparation method of the polyetheretherketone auditory ossicular prosthesis adopts 3D printing technology for one-piece molding. The preparation raw material is a polyetheretherketone composite material. The polyetheretherketone composite material includes the following raw materials: 15g of nano-hydroxyapatite, 72g of sulfonated polyetheretherketone, 8g of modified carbon nanotubes, and 5g of glass fiber; wherein the sulfonated polyetheretherketone is prepared by Preparation Example 1, and the modified carbon nanotubes are prepared by Preparation Example 3.

[0090] During the preparation, nano-hydroxyapatite, sulfonated polyetheretherketone, modified carbon nanotubes and glass fiber are added into N,N-dimethylformamide and mixed, and stirred continuously for 30 minutes at a stirring rate of 8000r / min. The material is discharged into a 50% ethanol solution, boiled and washed, and dried at 150°C for 24 hours to obtain a composite powder.

[0091] The composite powder was subjected to SLS selective laser sintering molding through a 3D printer. The laser temperature was 320°C, the temperature in the printing chamber was 310°C, the temperature of the printing base was 310°C, the scanning speed was 1200mm / s, the printing layer thickness was 0.2mm, and the porosity of the scaffold material was set to 70%, ultimately obtaining a 3D printed ossicular prosthesis.

[0092] After printing, the ossicular prosthesis was ultrasonically cleaned with acetone, anhydrous ethanol and deionized water for 10 minutes in sequence to remove surface contaminants; finally, the ossicular prosthesis was dried at 70°C for 48 hours; The surface was treated with 30% oxygen and 70% argon low-temperature plasma for 5 minutes under the conditions of 400V voltage and 10Pa pressure. After the treatment, it was ultrasonically cleaned with deionized water for 5 minutes and dried to obtain the plasma-treated ossicular prosthesis.

[0093] Prepare 10mmol / L Tris-HCl buffer; dissolve dopamine in Tris-HCl buffer to prepare a dopamine solution with a pH of 8.5 and a concentration of 2g / L; then immerse the auditory ossicle prosthesis in the dopamine solution, shake and react at 37°C for 24h, take out and ultrasonically rinse with deionized water for 3min to remove the dopamine not loaded on the surface, and then dry to obtain the auditory ossicle prosthesis with polydopamine loaded on the surface.

[0094] The polydopamine-loaded ossicular prosthesis was sterilized by ethylene oxide or cobalt-60 and then stored aseptically under vacuum until use.

[0095] Embodiment 18 The preparation method of the polyetheretherketone auditory ossicular prosthesis adopts 3D printing technology for one-piece molding. The preparation raw material is a polyetheretherketone composite material. The polyetheretherketone composite material includes the following raw materials: 15g of nano-hydroxyapatite, 72g of sulfonated polyetheretherketone, 8g of modified carbon nanotubes, and 5g of glass fiber; wherein the sulfonated polyetheretherketone is prepared by Preparation Example 1, and the modified carbon nanotubes are prepared by Preparation Example 3.

[0096] During the preparation, nano-hydroxyapatite, sulfonated polyetheretherketone, modified carbon nanotubes and glass fiber are added into N,N-dimethylformamide and mixed, and stirred continuously for 30 minutes at a stirring rate of 8000r / min. The material is discharged into a 50% ethanol solution, boiled and washed, and dried at 150°C for 24 hours to obtain a composite powder.

[0097] The composite powder was subjected to SLS selective laser sintering molding through a 3D printer. The laser temperature was 335°C, the temperature in the printing chamber was 300°C, the printing base temperature was 310°C, the scanning speed was 1200mm / s, the printing layer thickness was 0.2mm, and the porosity of the scaffold material was set to 70%, ultimately obtaining a 3D printed ossicular prosthesis.

[0098] After printing, the ossicular prosthesis was ultrasonically cleaned with acetone, anhydrous ethanol and deionized water for 10 minutes in sequence to remove surface contaminants; finally, the ossicular prosthesis was dried at 70°C for 48 hours; The surface was treated with 30% oxygen and 70% argon low-temperature plasma for 5 minutes under the conditions of 400V voltage and 10Pa pressure. After the treatment, it was ultrasonically cleaned with deionized water for 5 minutes and dried to obtain the plasma-treated ossicular prosthesis.

[0099] Prepare 10mmol / L Tris-HCl buffer; dissolve dopamine in Tris-HCl buffer to prepare a dopamine solution with a pH of 8.5 and a concentration of 2g / L; then immerse the auditory ossicle prosthesis in the dopamine solution, shake and react at 37°C for 24h, take out and ultrasonically rinse with deionized water for 3min to remove the dopamine not loaded on the surface, and then dry to obtain the auditory ossicle prosthesis with polydopamine loaded on the surface.

[0100] The polydopamine-loaded ossicular prosthesis was sterilized by ethylene oxide or cobalt-60 and then stored aseptically under vacuum until use.

[0101] Embodiment 19 The polyetheretherketone auditory ossicular prosthesis is prepared by the preparation method in Example 1.

[0102] Embodiment 20 The polyetheretherketone auditory ossicular prosthesis is prepared by the preparation method in Example 2.

[0103] Embodiment 21 The polyetheretherketone auditory ossicular prosthesis is prepared by the preparation method in Example 3.

[0104] Embodiment 22 The polyetheretherketone auditory ossicular prosthesis is prepared by the preparation method in Example 4.

[0105] Embodiment 23 The polyetheretherketone auditory ossicular prosthesis is prepared by the preparation method in Example 5.

[0106] Embodiment 24 The polyetheretherketone auditory ossicular prosthesis is prepared by the preparation method in Example 6.

[0107] Embodiment 25 The polyetheretherketone auditory ossicular prosthesis is prepared by the preparation method in Example 7.

[0108] Embodiment 26 The polyetheretherketone auditory ossicular prosthesis is prepared by the preparation method in Example 8.

[0109] Embodiment 27 The polyetheretherketone auditory ossicular prosthesis is prepared by the preparation method in Example 9.

[0110] Embodiment 28 The polyetheretherketone auditory ossicular prosthesis is prepared by the preparation method in Example 10.

[0111] Embodiment 29 The polyetheretherketone auditory ossicular prosthesis is prepared by the preparation method in Example 11.

[0112] Embodiment 30 The polyetheretherketone auditory ossicular prosthesis is prepared by the preparation method in Example 12.

[0113] Embodiment 31 The polyetheretherketone auditory ossicular prosthesis is prepared by the preparation method in Example 13.

[0114] Embodiment 32 The polyetheretherketone auditory ossicular prosthesis is prepared by the preparation method in Example 14.

[0115] Embodiment 33 The polyetheretherketone auditory ossicular prosthesis is prepared by the preparation method in Example 15.

[0116] Comparative Example Comparative Example 1 The only difference between this comparative example and Example 1 is that the raw material for preparing the polyetheretherketone auditory ossicular prosthesis is titanium material.

[0117] Performance Testing The ossicular prostheses prepared in Examples 1 to 18 and Comparative Example 1 were tested.

[0118] Determination of mechanical properties of auditory ossicle prosthesis: The tensile and compressive properties of auditory ossicle prosthesis were tested using a material testing machine. The tensile speed was 5 mm / min, the compression speed was 1 mm / min, and the test was performed at room temperature. The computer automatically collected data and calculated the results.

[0119] The hardness of the ossicular prosthesis was measured by using a MTHV-1MMDT Vickers hardness tester. A 10 mm × 10 mm × 10 mm sample was selected and sanded until there were no scratches. The load F was set to 500 g. The indenter was pressed into the tested surface of the sample. The time was set to 10 s. The diagonal length d of the pressed sample was measured and its surface area S was calculated. Find the hardness value.

[0120] Wear resistance of auditory ossicular prosthesis was measured by using JB-5C roughness profiler. After friction and wear, arc-shaped grooves appeared on the surface of the sample. The cross-sectional profile could be extracted by operation. The stylus was at the end of the measuring rod of the instrument. During the measurement, the stylus was perpendicular to the measured surface and moved on the measured surface at a certain speed. The surface profile of the sample could be obtained and the wear volume value of the sample could be calculated.

[0121] Table 1 Performance measurement of ossicular prosthesis Since the composite ossicular prosthesis will contact the surface of other bones during middle ear surgery, the replaced ossicular chain system transmits vibrations and plays a guiding, gain and protective role. Therefore, the ossicular prosthesis needs to match the surgical position of the ossicular chain and meet certain mechanical performance test requirements. Referring to Table 1, according to Comparative Example 1 and Example 1-Example 3, it can be seen that the polyetheretherketone composite material has excellent mechanical properties and chemical stability. The surface of the ossicular prosthesis is sintered to form a rough microporous structure through 3D printing integrated technology, thereby increasing its surface area and providing more attachment points, so that the prosthesis is more firmly fixed in the position of the ossicular chain and is not easy to detach; at the same time, these rough microporous structures can also promote the growth of surrounding tissues, and solve the problem that soft tissue blood vessels in the human body are difficult to attach, thereby further enhancing the postoperative stability of the prosthesis. According to the experimental personnel's measurement, it was found that the 3D printing integrated technology and the non-integrated technology have different effects on sound conduction, among which the integrated technology has a better conduction effect. This is because when the vibration of the tympanic membrane is transmitted to the vestibule, it can be better transmitted to the subsequent part through the integrated structure, thereby affecting the effect of postoperative hearing recovery of the patient.

[0122] Referring to Table 1, it can be seen from Examples 1-3 and 4-8 that sulfonated polyetheretherketone and nanohydroxyapatite are selected as the main mixed matrix of the ossicular prosthesis, wherein nanohydroxyapatite, as an important inorganic component in the human bone tissue structure, has very excellent biocompatibility and osteoconductivity, and is a hard tissue repair material with great potential; however, nanohydroxyapatite itself is difficult to directly form and has low strength; polyetheretherketone, as a semi-crystalline thermoplastic polymer, has excellent mechanical properties and chemical stability, and is non-toxic and harmless to the human body; and because polyetheretherketone is biologically inert, the bone integration effect in the body is not ideal, and polyetheretherketone is sulfonated and modified, and the two are compounded at the same time, thereby preparing a high-strength and high-bioactivity composite material. Comparative Examples 6-8, the polyetheretherketone composite material is also added with carbon nanotubes and / or glass fibers, and the combination between nanohydroxyapatite and sulfonated polyetheretherketone is improved by adding carbon nanotubes and glass fibers to the system, so that the two are mixed with the main mixed matrix, effectively improving the mechanical properties and bioactivity of the composite material.

[0123] Referring to Table 1, compared with Example 9, it can be seen from Example 1 and Example 5 that carbon nanotubes have excellent mechanical properties and surface activity, and the elastic modulus of the carbon nanotubes is almost close to that of diamond, and the toughness is good and can be stretched. However, due to poor interfacial compatibility, agglomeration is easily caused when directly physically blended with sulfonated polyetheretherketone, which is not conducive to improving the mechanical properties of the composite material. By performing carboxylation modification on the carbon nanotubes, and then performing secondary modification on the carboxylation modified carbon nanotubes, and chemically grafting the sulfonated polyetheretherketone to the surface of the modified carbon nanotubes, the same structure can improve the compatibility with sulfonated polyetheretherketone, and solve the agglomeration problem of carbon nanotubes in sulfonated polyetheretherketone.

[0124] Referring to Table 1, and comparing Example 12, it can be seen from Example 1, Example 10-Example 11 that the surface of the ossicular prosthesis is treated with oxygen and argon plasma, so that the surface of the ossicular prosthesis treated with oxygen and argon low-temperature plasma has depressions of varying sizes, and the surface becomes rough and uneven, increasing the surface area of ​​the matrix material, which is conducive to better attachment of soft tissue and blood vessels in the human body. At the same time, the ossicular prosthesis modified with oxygen and argon low-temperature plasma successfully prepares a nano-topological structure on its surface. When argon bombards the ossicular prosthesis, the free radicals formed on its surface react quickly with oxygen, which is conducive to the functionalization of the free radicals; and the hydrophilicity of the material surface is increased, providing good conditions for the subsequent deposition of polydopamine.

[0125] Referring to Table 1, Example 1, and Examples 16-18, by setting the temperature of the molding process, the obtained ossicles are denser, less prone to warping and cracking, and have better strength performance.

[0126] Biocompatibility determination of auditory ossicular prosthesis: Mouse bone marrow mesenchymal stem cells were used to evaluate the biocompatibility of auditory ossicular prosthesis. The extract was prepared according to GB / T16886.5-2017, and the auditory ossicular prosthesis was immersed in DMEM culture medium with a ratio of 0.2 g / mL to the extract medium. The prosthesis was placed in an incubator at 37°C for 72 h.

[0127] Table 2 Biocompatibility determination of ossicular prosthesis Referring to Table 2, compared with Example 15, Example 1, Example 13-Example 14, it can be seen that by loading a polydopamine layer on the surface of the ossicular prosthesis, the biological activity of the polyetheretherketone composite material can be further enhanced, and the proliferation of MSCs cells can be promoted, thereby promoting the bone integration effect; at the same time, when polydopamine is deposited on the surface of the ossicular prosthesis, the original concave and convex morphology of the surface of the ossicular prosthesis becomes less obvious, and polydopamine particles can be observed, which increases the hydrophilicity of the material surface. Then, using polydopamine as a secondary reaction platform, the protein composite material is fixed on the surface of the prosthesis by utilizing the adhesion of polydopamine, wherein the protein composite material is composed of type I collagen collagen membrane and rhBMP-2, which is conducive to promoting the proliferation of MSCs cells and further improving the bone integration effect.

[0128] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.

Claims

1. A method for preparing a polyetheretherketone ossicular prosthesis, characterized in that: The 3D printing technology is used for one-piece molding; the raw materials are polyetheretherketone and / or polyetheretherketone composite materials.

2. The method for preparing the polyetheretherketone ossicular prosthesis according to claim 1, characterized in that: The ossicular prosthesis includes at least one of a malleus prosthesis, an incus prosthesis and a stapes prosthesis.

3. The method for preparing the polyetheretherketone ossicular prosthesis according to claim 2, characterized in that: The malleus prosthesis and the incus prosthesis are connected via a ball and socket joint.

4. The method for preparing the polyetheretherketone ossicular prosthesis according to claim 1, characterized in that: The polyetheretherketone composite material comprises the following raw materials in weight percentage: 15-37% nano-hydroxyapatite, 55-72% sulfonated polyetheretherketone, 5-8% modified carbon nanotubes, and 3-5% glass fiber.

5. The method for preparing the polyetheretherketone ossicular prosthesis according to claim 4, characterized in that: The preparation of the sulfonated polyetheretherketone is as follows: Add polyetheretherketone into concentrated sulfuric acid solution and react for 60-100 minutes. After the reaction is completed, pour the mixed solution into an ice water bath for washing. After solids are precipitated, wash them several times with deionized water, filter and dry to obtain sulfonated polyetheretherketone.

6. The method for preparing the polyetheretherketone ossicular prosthesis according to claim 4, characterized in that: The modified carbon nanotubes are grafted with sulfonated polyetheretherketone, and the specific processing steps are as follows: (1) Carboxylation-modified carbon nanotubes: multi-walled carbon nanotubes are added to an acid solution for reaction, and after the reaction is completed, deionized water is added to dilute the solution. After multiple washings and centrifugation, the resulting precipitate is filtered, dried and ground to obtain carboxylation-modified carbon nanotubes. (2) Amino modified carbon nanotubes: neutralize the carboxyl modified carbon nanotubes and N,N-dimethylformamide and mix them evenly to obtain a modified carbon nanotube solution; then add 1,6-hexanediamine and N,N-dicyclohexylcarbodiimide to react, filter and wash after the reaction, and finally dry to obtain amino modified carbon nanotubes; (3) Grafting sulfonated polyetheretherketone: Mix the amino-modified modified carbon nanotubes and N,N-dimethylformamide to obtain a modified carbon nanotube solution; then mix the sulfonated polyetheretherketone and N,N-dimethylformamide to obtain a sulfonated polyetheretherketone solution; mix the modified carbon nanotube solution, N,N-dicyclohexylcarbodiimide and the sulfonated polyetheretherketone solution and react, and after the reaction is completed, filter and wash, and finally dry and grind to obtain modified carbon nanotubes grafted with sulfonated polyetheretherketone.

7. The method for preparing the polyetheretherketone ossicular prosthesis according to claim 1, characterized in that: The 3D printing technology is SLS selective laser sintering technology or FDM fused deposition modeling technology; during the one-piece molding process of the SLS selective laser sintering technology, the laser temperature is 332-338°C, the temperature in the printing chamber is 310-315°C, and the temperature of the printing platform is 310-315°C; during the one-piece molding process of the FDM fused deposition modeling technology, the nozzle temperature is 377-383°C and the printing base plate temperature is 257-263°C.

8. The method for preparing the polyetheretherketone ossicular prosthesis according to claim 1, characterized in that: The surface of the ossicular prosthesis is loaded with a polydopamine layer, which is specifically prepared as follows: Dopamine is dissolved in Tris-HCl buffer to prepare a dopamine solution; then the auditory ossicle prosthesis is immersed in the dopamine solution for reaction, and after the reaction is completed, it is taken out and repeatedly rinsed with deionized water, and dried to obtain an auditory ossicle prosthesis with polydopamine loaded on the surface.

9. The method for preparing the polyetheretherketone ossicular prosthesis according to claim 8, characterized in that: The polydopamine layer is also loaded with a protein composite material, which is specifically prepared as follows: The rhBMP-2 solution is prepared by dissolving rhBMP-2 in an acetic acid solution, and then the rhBMP-2 solution is adsorbed by a collagen membrane to form a spherical shape, and then freeze-dried to form a protein composite material; The protein composite material is uniformly mixed in deionized water to prepare a suspension; the auditory ossicle loaded with the polydopamine layer is placed in the suspension to react for 4-6 hours, and freeze-dried after the reaction to obtain an auditory ossicle prosthesis still loaded with the protein composite material.

10. Polyetheretherketone ossicular prosthesis, characterized in that: The polyetheretherketone ossicular prosthesis is prepared by the preparation method of any one of claims 1 to 9.

Citation Information

Patent Citations

  • Modified hydroxyapatite / carbon nanotube / polyetheretherketon composite material and preparation method thereof

    CN106421922A

  • Polyether ether ketone-based artificial bone composite material and preparation method thereof

    CN111184913A

  • Polyether-ether-ketone composite membrane made of modified carbon nanotube and metal organic framework composite material as well as preparation method and application of composite membrane

    CN112221358A

  • Preparation method of personalized customized polyether-ether-ketone implant prosthesis with high biological activity

    CN114392392A

  • Bone-induced polyaryletherketone interbody fusion cage and preparation method thereof

    CN116785032A