Flame retardant composition for preparing pp film, pp film and preparation method thereof
By using halogen-free flame retardant compositions and antioxidants in polypropylene films, combined with high-temperature melt extrusion process, the problem of poor flame retardancy of polypropylene films is solved, and the efficient use of low-quality flame retardants and excellent mechanics are achieved. Performance, suitable for a variety of application scenarios.
Patent Information
- Application Number
- CN202410974554.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
AI Technical Summary
Polypropylene films have poor flame retardancy, the amount of traditional flame retardant is added large and the mechanical properties are reduced, making it difficult to widely use in fields requiring flame retardation.
Halogen-free flame retardant polypropylene films are prepared by high temperature melt extrusion bidirectional stretching process using a halogen-free flame retardant composition, including compounds of specific structures and cyclophosphate-based flame retardant, combining antioxidants and compatible agents. , optimize the amount of flame retardant used and mechanical properties.
It realizes the use of a low amount of flame retardant, achieves excellent flame retardant effect and good mechanical properties, while maintaining transparency, and is suitable for the wide application of polypropylene films.
Smart Images

Figure CN118909307A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of polypropylene products, and in particular to a flame retardant composition for preparing PP film, the PP film and a preparation method thereof. Background Art
[0002] Polypropylene (PP) is a non-polar linear polymer made from propylene monomers by free radical polymerization. Due to its excellent electrical insulation, easy processing and excellent tolerance to many chemicals, polypropylene is widely used in many fields such as electronic appliances, interior decoration, medical treatment, packaging materials, chemicals and automobiles, especially in the packaging field, because polypropylene film has the advantages of low price, suitable strength, abundant sources and high transparency, which can meet the requirements of materials for packaging of various items. However, PP without any modification has poor flame retardancy, with an oxygen index of only 17%. The fire hazard caused by the high flammability of PP film seriously limits its application in many fields requiring flame retardancy.
[0003] At present, in order to solve the flammability of polypropylene film, flame retardants are usually added to polypropylene, mainly including halogen flame retardants, phosphorus flame retardants and intumescent flame retardants. However, traditional flame retardants not only require large amounts of addition, but also reduce the mechanical properties of PP film, and the flame retardant effect is also poor. Therefore, how to prepare halogen-free flame-retardant PP film with excellent mechanical properties is of far-reaching significance.
[0004] The invention patent with publication number "CN109311921A" discloses an organic phosphorus compound, a flame retardant and a flame retardant product formed therefrom. The general formula of the compound is as follows:
[0005]
[0006] , and the substituents therein are defined as follows (wherein, in the formula, R2 and R5 may be the same or different, and are phenyl which may have a substituent, naphthyl which may have a substituent, anthracene which may have a substituent, or a branched or straight-chain alkyl group with 1 to 4 carbon atoms which may have an aromatic substituent, and R1, R3, R4, and R6 may be the same or different, and are hydrogen atoms, branched or straight-chain alkyl groups with 1 to 4 carbon atoms, phenyl which may have a substituent, naphthyl which may have a substituent, or anthracene which may have a substituent). The patent discloses that when the above-mentioned compound materials are applied as flame retardants for polymer materials, flame retardant products having high flame retardancy and good appearance while maintaining the original physical properties of the polymer materials can be obtained. In the specification, it is specifically applied to epoxy resin to achieve high flame retardancy and good appearance characteristics. However, its application in the field of polypropylene film products needs to be developed and improved. Summary of the invention
[0007] The purpose of the present invention is to solve the above technical problems. The present invention provides a flame retardant composition for preparing PP film, at least for polypropylene film, at least for polypropylene film, comprising at least a compound represented by Formula 1 and a compound represented by Formula 2:
[0008]
[0009] Wherein, R1 and R2 are each independently selected from substituted or unsubstituted C1-C4 straight chain or branched alkyl groups.
[0010] As a preferred embodiment of the present invention, R1 and R2 are independently selected from substituted or unsubstituted methyl, ethyl, propyl, isopropyl, n-butyl, sec-butyl, isobutyl and tert-butyl.
[0011] As a preferred embodiment of the present invention, the compound represented by Formula 1 is one of the following compounds:
[0012]
[0013]
[0014]
[0015] The present invention also provides a halogen-free flame-retardant PP film, comprising: 60-90% polypropylene, 9.8-36.5% flame retardant composition, and 0.5-1% antioxidant, wherein the flame retardant contains the composition according to any one of claims 1-6.
[0016] As a preferred solution of the present invention, the polypropylene is homopolymer polypropylene with a melt index of 8 g / 10 min.
[0017] As a preferred solution of the present invention, the compatibilizer is PP-g-MAH, and the grafting rate is 0.8-1.2%.
[0018] As a preferred embodiment of the present invention, the weight ratio of the compound represented by Formula 2 to the compound represented by Formula 1 in the flame retardant composition is 2.3%-16.6%.
[0019] As a preferred embodiment of the present invention, the antioxidant comprises at least one of the following: antioxidant 1010 and antioxidant 168, wherein the antioxidant is a mixture of antioxidant 1010 and antioxidant 168 in a ratio of 1:1.
[0020] The present invention also provides a method for preparing a halogen-free flame-retardant PP film, which is at least used to prepare the halogen-free flame-retardant PP film as claimed in claim 4, comprising the following steps:
[0021] S1. Add PP, compatibilizer, flame retardant composition and antioxidant into a high-speed mixer and mix them evenly for 5 to 10 minutes;
[0022] S2, adding the mixed material in step S1 into the hopper of a twin-screw extruder, and preparing the halogen-free flame-retardant polypropylene film by high-temperature melt extrusion and biaxial stretching process.
[0023] As a preferred embodiment of the present invention, the processing temperature of the twin-screw extruder is 120-220°C.
[0024] The compound having the structure shown in Formula 1 of the present invention has a synthesis reaction route as follows:
[0025]
[0026] Beneficial effects of the present invention:
[0027] The invention provides a flame retardant composition with a relatively low addition amount, which can achieve a good flame retardant effect, and the product has excellent mechanical properties and good transparency. DETAILED DESCRIPTION
[0028] The following further illustrates and describes embodiments of various aspects. It should be understood that the description herein is not intended to limit the claims to the specific aspects described. On the contrary, it is intended to cover substitutions, modifications and equivalents that may be included in the spirit and scope of the present disclosure defined by the appended claims.
[0029] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. If the manufacturers of the reagents or instruments are not specified, they are all conventional products that can be purchased commercially.
[0030] Example 1
[0031] A halogen-free flame-retardant PP film is composed of the following raw materials in weight percentage: 90% homopolymer PP, 9% cyclic phosphate-based flame retardant, 0.5% antioxidant 1010, and 0.5 antioxidant 168;
[0032] (1) Add homopolymer PP, cyclic phosphate flame retardant, antioxidant 1010, and antioxidant 168 into a high-speed mixer and pre-mix them evenly. Stir for 10 minutes.
[0033] (2) adding the materials uniformly mixed in step (1) into the hopper of a twin-screw extruder, and preparing the halogen-free flame-retardant polypropylene film through high-temperature melt extrusion and biaxial stretching process, wherein the processing temperature of the twin-screw extruder is 120-220°C.
[0034] Example 2
[0035] A halogen-free flame-retardant PP film is composed of the following raw materials in weight percentage: 89% homopolymer PP, 9% cyclic phosphate-based flame retardant, 1% N-alkoxyamine flame retardant (compound shown in Formula 2), 0.5% antioxidant 1010, and 0.5 antioxidant 168;
[0036] (1) Add homopolymer PP, cyclic phosphate flame retardant, N-alkoxyamine flame retardant, antioxidant 1010, and antioxidant 168 into a high-speed mixer and mix them evenly. Stir for 10 minutes.
[0037] (2) adding the materials uniformly mixed in step (1) into the hopper of a twin-screw extruder, and preparing the halogen-free flame-retardant polypropylene film through high-temperature melt extrusion and biaxial stretching process, wherein the processing temperature of the twin-screw extruder is 120-220°C.
[0038] Example 3
[0039] A halogen-free flame-retardant PP film is composed of the following raw materials in weight percentage: 87.5% homopolymer PP, 10% cyclic phosphate-based flame retardant, 1.5% N-alkoxyamine flame retardant (compound shown in Formula 2), 0.5% antioxidant 1010, and 0.5 antioxidant 168;
[0040] (1) Add homopolymer PP, cyclic phosphate flame retardant, N-alkoxyamine flame retardant, antioxidant 1010, and antioxidant 168 into a high-speed mixer and mix them evenly. Stir for 10 minutes.
[0041] (2) adding the materials uniformly mixed in step (1) into the hopper of a twin-screw extruder, and preparing the halogen-free flame-retardant polypropylene film through high-temperature melt extrusion and biaxial stretching process, wherein the processing temperature of the twin-screw extruder is 120-220°C.
[0042] Comparative Example 1
[0043] A halogen-free flame-retardant PP film is composed of the following raw materials in weight percentage: 64% homopolymer PP, 5% PP-g-MAH, 22.5% piperazine pyrophosphate, 7.5% melamine pyrophosphate, 0.5% antioxidant 1010, and 0.5 antioxidant 168;
[0044] (1) Add homopolymer PP, PP-g-MAH, piperazine pyrophosphate, melamine pyrophosphate, antioxidant 1010, and antioxidant 168 into a high-speed mixer and mix them evenly for 10 minutes.
[0045] (2) adding the materials uniformly mixed in step (1) into the hopper of a twin-screw extruder, and preparing the halogen-free flame-retardant polypropylene film through high-temperature melt extrusion and biaxial stretching process, wherein the processing temperature of the twin-screw extruder is 120-220°C.
[0046] Comparative Example 2
[0047] A halogen-free flame-retardant PP film is composed of the following raw materials in weight percentage: 56% homopolymer PP, 8% PP-g-MAH, 26.25% piperazine pyrophosphate, 8.75% melamine pyrophosphate, 0.5% antioxidant 1010, and 0.5 antioxidant 168;
[0048] (1) Add homopolymer PP, PP-g-MAH, piperazine pyrophosphate, melamine pyrophosphate, antioxidant 1010, and antioxidant 168 into a high-speed mixer and mix them evenly for 10 minutes.
[0049] (2) adding the materials uniformly mixed in step (1) into the hopper of a twin-screw extruder, and preparing the halogen-free flame-retardant polypropylene film through high-temperature melt extrusion and biaxial stretching process, wherein the processing temperature of the twin-screw extruder is 120-220°C.
[0050] The materials prepared in Examples 1-3 and Comparative Examples 1-2 were subjected to performance tests, and the test methods were as follows:
[0051] (1) Flame retardant performance: vertical combustion test is carried out in accordance with ANSL-UL94-2009 standard.
[0052] (2) Tensile strength: Tested in accordance with ISO 527 standard
[0053] The performance test is shown in Table 1:
[0054] Table 1
[0055] Comparative Example 1 Comparative Example 2 Example 1 Example 2 Example 3 Tensile strength / MPa 21.3 20.0 32.6 31.7 31.5 Elongation at break / % 14.6 12.3 31.2 26.7 25.4 UL-94(0.5mm) V-2 V-2 NR V-2 V-0
[0056] It can be seen from Table 1 that the flame retardant grade of Example 3 is V-0, while the flame retardant grades of Comparative Examples 1 and 2 are only V-2. The compound use of cyclic phosphate-based flame retardant and N-alkoxyamine flame retardant not only has a small addition amount, but also can maintain excellent mechanical properties.
[0057] The above experiments show that the halogen-free flame-retardant PP film of the present invention not only requires less flame retardant, but also has excellent flame retardancy and mechanical properties. The composition of the present invention is applied to polypropylene film products and has broad application prospects.
[0058] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the claims of the present invention.
Claims
1. A flame retardant composition for preparing PP film, at least for polypropylene film, characterized in that: At least comprising a compound represented by Formula 1 and a compound represented by Formula 2: Wherein, R1 and R2 are each independently selected from substituted or unsubstituted C1-C4 straight chain or branched alkyl groups.
2. A flame retardant composition for preparing PP film according to claim 1, characterized in that: R1 and R2 are each independently selected from substituted or unsubstituted methyl, ethyl, propyl, isopropyl, n-butyl, sec-butyl, isobutyl and tert-butyl.
3. The flame retardant composition for preparing PP film according to claim 1, characterized in that: The compound shown in Formula 1 is one of the following structural compounds:
4. A halogen-free flame-retardant PP film, characterized in that: include: Polypropylene 60-90%, flame retardant composition 9.8-36.5%, antioxidant 0.5-1%, the flame retardant contains the compound according to any one of claims 1-6.
5. The halogen-free flame-retardant PP film according to claim 4, characterized in that: The polypropylene is homopolymer polypropylene, and the melt index is 8g / 10min.
6. The halogen-free flame-retardant PP film according to claim 4, characterized in that: The compatibilizer is PP-g-MAH.
7. The halogen-free flame-retardant PP film according to claim 4, characterized in that: The weight ratio of the compound represented by Formula 2 to the compound represented by Formula 1 in the flame retardant composition is 2.3%-16.6%.
8. The halogen-free flame-retardant PP film according to claim 4, characterized in that: The antioxidant includes at least one of the following: antioxidant 1010 and antioxidant 168.
9. A method for preparing a halogen-free flame-retardant PP film, at least for preparing the halogen-free flame-retardant PP film as claimed in claim 4, characterized in that: The following steps are involved: S1. Add PP, compatibilizer, flame retardant composition and antioxidant into a high-speed mixer and mix them evenly for 5 to 10 minutes; S2, adding the materials uniformly mixed in step S1 into the hopper of a twin-screw extruder, and preparing the halogen-free flame-retardant polypropylene film through high-temperature melt extrusion and biaxial stretching process.
10. The halogen-free flame-retardant PP film according to claim 9, characterized in that: The processing temperature of the twin-screw extruder is 120-220°C.
Citation Information
Patent Citations
Organophosphorus compound, flame retardant, and flame-retardant product including same
CN109311921A