Toughening aid with flame-retardant effect as well as preparation method and application of toughening aid
By modifying the surface of nano aluminum hydroxide particles and combining calcium sulfate whiskers, a toughening additive with flame retardant effect is obtained, which solves the lack of toughness of toughening additives in the prior art and the inability to resist high temperatures and flame retardant plastics in the high temperature are not resistant to flame retardant. The problem has significantly improved the flame retardant and mechanical properties of plastics.
Patent Information
- Application Number
- CN202410987723.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-23
Smart Images

Figure BDA0004957940970000121
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of plastics, and in particular to a toughening auxiliary agent with flame retardant effect and a preparation method and application thereof. Background Art
[0002] Plastic is a high molecular compound made from monomers through addition polymerization or condensation polymerization. It has a medium deformation resistance, between fiber and rubber. It is composed of synthetic resin and additives such as fillers, toughening agents, stabilizers, lubricants, and colorants.
[0003] Toughening agents refer to substances that can increase the flexibility of the adhesive film layer. Some thermosetting resin adhesives, such as epoxy resins, phenolic resins and unsaturated polyester resins, have low elongation and high brittleness after curing. When the bonding part is subjected to external force, cracks are easily generated and rapidly expand, resulting in cracking of the adhesive layer. They are not fatigue-resistant and cannot be used for structural bonding. Therefore, it is necessary to find ways to reduce brittleness, increase toughness, and increase bearing strength. Any substance that can reduce brittleness, increase toughness, and does not affect other main properties of the adhesive is a toughening agent. It can be divided into rubber toughening agents and thermoplastic elastomer toughening agents. However, common toughening agents cannot meet the increasingly stringent toughness requirements. At the same time, the shortcomings of plastics such as high temperature resistance and non-flame retardancy have also seriously restricted the widespread application of plastics. Therefore, how to effectively improve the toughening and flame retardant properties of toughening agents has become an important issue that needs to be urgently solved in my country's plastic processing industry. Summary of the invention
[0004] The purpose of the present invention is to provide a toughening auxiliary agent with flame retardant effect and its preparation method and application, which can significantly improve the flame retardant effect of plastics, and can also play a connecting buffering role between molecular chains to reduce cracks, have good toughening and impact resistance effects, can be widely used in plastics, and play a good role in flame retardancy and improving mechanical properties.
[0005] The technical solution of the present invention is achieved in this way:
[0006] The invention provides a method for preparing a toughening aid with a flame retardant effect. The surface of nano aluminum hydroxide particles doped with Ti element is modified with a silane coupling agent with amino group, reacted with thiophene-2-carboxaldehyde and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, and then blended with calcium sulfate whiskers with surface modified with polydopamine to prepare the toughening aid with a flame retardant effect.
[0007] As a further improvement of the present invention, the following steps are included:
[0008] S1. Add an aqueous solution of aluminum chloride to the alkali solution, heat and stir to react, at which time the pH value of the solution is 6.2-6.5, add an ethanol solution of tetrabutyl titanate, stir to react, centrifuge, wash, and dry to obtain nanoparticles;
[0009] S2. adding the nanoparticles and the silane coupling agent with an amino group to ethanol, heating and stirring the reaction, centrifuging, washing, and drying to obtain amino-modified nanoparticles;
[0010] S3. The amino-modified nanoparticles are added to ethanol, thiophene-2-carboxaldehyde is added, the reaction is heated and stirred, and then 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide is added, the reaction is stirred to obtain flame-retardant nanoparticles;
[0011] S4. The calcium sulfate whiskers were added to water, dopamine hydrochloride and a catalyst were added, the reaction was heated and stirred, filtered, washed, and dried to obtain modified calcium sulfate whiskers;
[0012] S5. Evenly mix the flame retardant nanoparticles and modified calcium sulfate whiskers to prepare a toughening agent with flame retardant effect.
[0013] As a further improvement of the present invention, the alkali solution in step S1 is a 1-2 mol / L NaOH or KOH solution, the mass ratio of the alkali solution, aluminum chloride, and tetrabutyl titanate is 100:4-7:1-2, the temperature of the heating and stirring reaction is 70-80°C, the time is 0.5-1h, and the stirring reaction time is 1-2h.
[0014] As a further improvement of the present invention, the silane coupling agent with amino group in step S2 is selected from at least one of KH550, KH602, and KH792, the mass ratio of the nanoparticles to the silane coupling agent with amino group is 10-15:2-3, the temperature of the heating and stirring reaction is 40-50°C, and the time is 2-3h.
[0015] As a further improvement of the present invention, the mass ratio of the amino-modified nanoparticles, thiophene-2-carboxaldehyde, and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide in step S3 is 10:0.7-1.2:1.5-2.4, the temperature of the heating and stirring reaction is 75-85°C, the time is 4-6h, and the stirring reaction time is 10-12h.
[0016] As a further improvement of the present invention, the mass ratio of the calcium sulfate whiskers, dopamine hydrochloride and catalyst in step S4 is 12-15:2-3:0.2-0.3, the catalyst is a Tris-HCl solution with a pH of 7.5-8.5, the temperature of the heating and stirring reaction is 40-50°C, and the time is 2-4h.
[0017] As a further improvement of the present invention, the mass ratio of the flame retardant nanoparticles to the modified calcium sulfate whiskers in step S5 is 3-5:7.
[0018] As a further improvement of the present invention, the present invention specifically comprises the following steps:
[0019] S1. Add 20 parts by weight of an aqueous solution containing 4-7 parts by weight of aluminum chloride to 100 parts by weight of a 1-2 mol / L NaOH or KOH solution, heat to 70-80°C, stir and react for 0.5-1h, at which time the pH value of the solution is 6.2-6.5, add 20 parts by weight of an ethanol solution containing 1-2 parts by weight of tetrabutyl titanate, stir and react for 1-2h, centrifuge, wash, and dry to obtain nanoparticles;
[0020] S2. 10-15 parts by weight of the nanoparticles and 2-3 parts by weight of a silane coupling agent with an amino group are added to ethanol, heated to 40-50 ° C, stirred for 2-3h, centrifuged, washed, and dried to obtain amino-modified nanoparticles;
[0021] S3. Add 10 parts by weight of amino-modified nanoparticles to ethanol, add 0.7-1.2 parts by weight of thiophene-2-carboxaldehyde, heat to 75-85 ° C, stir and react for 4-6 hours, then add 1.5-2.4 parts by weight of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, stir and react for 10-12 hours to obtain flame retardant nanoparticles;
[0022] S4. 12-15 parts by weight of calcium sulfate whiskers are added to water, 2-3 parts by weight of dopamine hydrochloride and 0.2-0.3 parts by weight of a catalyst are added, heated to 40-50 ° C, stirred for 2-4h, filtered, washed, and dried to obtain modified calcium sulfate whiskers;
[0023] The catalyst is a Tris-HCl solution with a pH of 7.5-8.5;
[0024] S5. Mix 3-5 parts by weight of flame-retardant nanoparticles and 7 parts by weight of modified calcium sulfate whiskers to obtain a toughening agent with flame retardant effect.
[0025] The present invention further protects a toughening auxiliary agent with flame retardant effect obtained by the above preparation method.
[0026] The present invention further protects the use of the above-mentioned toughening auxiliary agent with flame retardant effect in improving the flame retardancy and toughness of plastic products.
[0027] The present invention has the following beneficial effects:
[0028] The presence of nanoparticles causes microcracks to be generated in the matrix when impacted, yielding and plastic deformation occur between the particles, and further absorbing the impact energy; as the particles become finer, more cracks will be generated, thereby absorbing more energy, which can play a role in toughening. The finer the particle size of the nanoparticles, the larger its specific surface area, and the stronger the interfacial bonding force with the polymer matrix resin, so that the plastic can be further toughened. The nano aluminum hydroxide prepared by the present invention is a very good inorganic flame retardant. After adding tetrabutyl titanate to the reaction, the prepared nanoparticles can be doped with titanium. Adding it to ABS plastic can significantly improve the antibacterial, anti-aging, and anti-ultraviolet properties of the material, and also improve the flame retardancy, with a synergistic flame retardant effect.
[0029] The surface of the prepared nanoparticles is modified by a silane coupling agent with an amino group, and then thiophene-2-carboxaldehyde is reacted to form an N=C bond. The N=C bond can react with 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO) so that 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide is connected to the surface of the nanoparticles, thereby preparing nanoparticles containing organic phosphine. At the same time, the sulfur element contained plays an important role in improving the performance of the flame retardant, can inhibit the thermal decomposition reaction, thereby preventing the material from decomposing violently too early, and the sulfur element can combine with the oxygen element to slow down the propagation speed of the flame, thereby achieving a synergistic flame retardant effect.
[0030] As a needle-shaped single crystal material, calcium sulfate inorganic whiskers have neatly arranged atoms and a complete crystal structure. After being added to plastics, they can be filled in polymer materials. When subjected to stress, the stress is transmitted to the inorganic whiskers through the molecular chain, which reduces the influence of stress on subsequent molecular chains, thereby optimizing the impact strength and toughness of the composite material. After the surface of calcium sulfate inorganic whiskers is modified with polydopamine, the N content in the flame retardant is greatly increased, the flame retardant effect is improved, and the compatibility of the prepared additive in plastics is improved. It has a free radical capture function, and enhances the heat resistance, UV resistance, and aging resistance of the material. Due to its good adhesion, it can reduce the formation of cracks under stress, and can also be well compounded with flame-retardant nanoparticles to further improve mechanical properties such as toughness and impact resistance. At the same time, it has a good flame retardant effect.
[0031] The flame retardant toughening auxiliary agent prepared by the invention can significantly improve the flame retardant effect of plastics, and can also play a connecting buffering role between molecular chains to reduce cracks, has good toughening and impact resistance effects, can be widely used in plastics, and plays a good role in flame retardancy and improving mechanical properties. DETAILED DESCRIPTION
[0032] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] Example 1
[0034] This embodiment provides a method for preparing a toughening agent with flame retardant effect, which specifically comprises the following steps:
[0035] S1. Add 20 g of an aqueous solution containing 4 g of aluminum chloride to 100 g of a 1 mol / L NaOH solution, heat to 70 ° C, and stir for 0.5 h. At this time, the pH value of the solution is 6.5. Add 20 g of an ethanol solution containing 1 g of tetrabutyl titanate, stir for 1 h, centrifuge, wash, and dry to obtain nanoparticles.
[0036] S2. 10 g of nanoparticles and 2 g of silane coupling agent KH550 were added to 200 mL of ethanol, heated to 40 ° C, stirred for reaction for 2 h, centrifuged, washed, and dried to obtain amino-modified nanoparticles;
[0037] S3. 10 g of amino-modified nanoparticles were added to 200 mL of ethanol, 0.7 g of thiophene-2-carboxaldehyde was added, heated to 75 ° C, stirred for 4 h, and then 1.5 g of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide was added, stirred for 10 h, and flame-retardant nanoparticles were obtained;
[0038] S4. 12 g of calcium sulfate whiskers were added to 200 mL of water, 2 g of dopamine hydrochloride and 0.2 g of catalyst were added, heated to 40 ° C, stirred for 2 h, filtered, washed, and dried to obtain modified calcium sulfate whiskers;
[0039] The catalyst is a Tris-HCl solution with a pH of 7.5;
[0040] S5. 3 g of flame retardant nanoparticles and 7 g of modified calcium sulfate whiskers were stirred and mixed for 20 min to obtain a toughening agent with flame retardant effect.
[0041] Example 2
[0042] This embodiment provides a method for preparing a toughening agent with flame retardant effect, which specifically comprises the following steps:
[0043] S1. 20 g of an aqueous solution containing 7 g of aluminum chloride was added dropwise to 100 g of a 2 mol / L NaOH solution, heated to 80 ° C, and stirred for 1 h. At this time, the pH value of the solution was 6.2. 20 g of an ethanol solution containing 2 g of tetrabutyl titanate was added dropwise, stirred for 2 h, centrifuged, washed, and dried to obtain nanoparticles;
[0044] S2. 15 g of nanoparticles and 3 g of silane coupling agent KH602 were added to 200 mL of ethanol, heated to 50 ° C, stirred for 3 h, centrifuged, washed, and dried to obtain amino-modified nanoparticles;
[0045] S3. 10 g of amino-modified nanoparticles were added to 200 mL of ethanol, 1.2 g of thiophene-2-carboxaldehyde was added, heated to 85 ° C, stirred for 6 h, and then 2.4 g of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide was added, stirred for 12 h, and flame-retardant nanoparticles were obtained;
[0046] S4. 15 g of calcium sulfate whiskers were added to 200 mL of water, 3 g of dopamine hydrochloride and 0.3 g of catalyst were added, heated to 50 ° C, stirred for 4 h, filtered, washed, and dried to obtain modified calcium sulfate whiskers;
[0047] The catalyst is a Tris-HCl solution with a pH of 8.5;
[0048] S5. Stir and mix 5 g of flame-retardant nanoparticles and 7 g of modified calcium sulfate whiskers for 20 minutes to obtain a toughening agent with flame-retardant effect.
[0049] Example 3
[0050] This embodiment provides a method for preparing a toughening agent with flame retardant effect, which specifically comprises the following steps:
[0051] S1. 20 g of an aqueous solution containing 5.5 g of aluminum chloride was added dropwise to 100 g of a 1.5 mol / L NaOH solution, heated to 75 ° C, stirred for 1 h, at which time the pH value of the solution was 6.3, 20 g of an ethanol solution containing 1.5 g of tetrabutyl titanate was added dropwise, stirred for 1.5 h, centrifuged, washed, and dried to obtain nanoparticles;
[0052] S2. 12 g of nanoparticles and 2.5 g of silane coupling agent KH792 were added to 200 mL of ethanol, heated to 45 ° C, stirred for 2.5 h, centrifuged, washed, and dried to obtain amino-modified nanoparticles;
[0053] S3. 10 g of amino-modified nanoparticles were added to 200 mL of ethanol, 1 g of thiophene-2-carboxaldehyde was added, heated to 80 ° C, stirred for 5 h, and then 2.1 g of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide was added, stirred for 11 h, and flame-retardant nanoparticles were obtained;
[0054] S4. 13.5 g of calcium sulfate whiskers were added to 200 mL of water, 2.5 g of dopamine hydrochloride and 0.25 g of catalyst were added, heated to 45 ° C, stirred for 3 h, filtered, washed, and dried to obtain modified calcium sulfate whiskers;
[0055] The catalyst is a Tris-HCl solution with a pH of 8;
[0056] S5. 4 g of flame retardant nanoparticles and 7 g of modified calcium sulfate whiskers were stirred and mixed for 20 min to obtain a toughening agent with flame retardant effect.
[0057] Comparative Example 1
[0058] Compared with Example 3, the difference is that tetrabutyl titanate is not added in step S1.
[0059] The details are as follows:
[0060] S1. Add 20 g of an aqueous solution containing 5.5 g of aluminum chloride to 100 g of a 1.5 mol / L NaOH solution, heat to 75 ° C, and stir to react for 1 h. At this time, the pH value of the solution is 6.3. Centrifuge, wash, and dry to obtain nanoparticles;
[0061] S2. 12 g of nanoparticles and 2.5 g of silane coupling agent KH792 were added to 200 mL of ethanol, heated to 45 ° C, stirred for 2.5 h, centrifuged, washed, and dried to obtain amino-modified nanoparticles;
[0062] S3. 10 g of amino-modified nanoparticles were added to 200 mL of ethanol, 1 g of thiophene-2-carboxaldehyde was added, heated to 80 ° C, stirred for 5 h, and then 2.1 g of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide was added, stirred for 11 h, and flame-retardant nanoparticles were obtained;
[0063] S4. 13.5 g of calcium sulfate whiskers were added to 200 mL of water, 2.5 g of dopamine hydrochloride and 0.25 g of catalyst were added, heated to 45 ° C, stirred for 3 h, filtered, washed, and dried to obtain modified calcium sulfate whiskers;
[0064] The catalyst is a Tris-HCl solution with a pH of 8;
[0065] S5. 4 g of flame retardant nanoparticles and 7 g of modified calcium sulfate whiskers were stirred and mixed for 20 min to obtain a toughening agent with flame retardant effect.
[0066] Comparative Example 2
[0067] Compared with Example 3, the difference is that steps S2 and S3 are not performed.
[0068] The details are as follows:
[0069] S1. 20 g of an aqueous solution containing 5.5 g of aluminum chloride was added dropwise to 100 g of a 1.5 mol / L NaOH solution, heated to 75 ° C, stirred for 1 h, at which time the pH value of the solution was 6.3, 20 g of an ethanol solution containing 1.5 g of tetrabutyl titanate was added dropwise, stirred for 1.5 h, centrifuged, washed, and dried to obtain nanoparticles;
[0070] S2. 13.5 g of calcium sulfate whiskers were added to 200 mL of water, 2.5 g of dopamine hydrochloride and 0.25 g of catalyst were added, heated to 45 ° C, stirred for 3 h, filtered, washed, and dried to obtain modified calcium sulfate whiskers;
[0071] The catalyst is a Tris-HCl solution with a pH of 8;
[0072] S3. 4 g of nanoparticles and 7 g of modified calcium sulfate whiskers were stirred and mixed for 20 min to obtain a toughening agent with flame retardant effect.
[0073] Comparative Example 3
[0074] Compared with Example 3, the difference is that step S3 is not performed.
[0075] The details are as follows:
[0076] S1. 20 g of an aqueous solution containing 5.5 g of aluminum chloride was added dropwise to 100 g of a 1.5 mol / L NaOH solution, heated to 75 ° C, stirred for 1 h, at which time the pH value of the solution was 6.3, 20 g of an ethanol solution containing 1.5 g of tetrabutyl titanate was added dropwise, stirred for 1.5 h, centrifuged, washed, and dried to obtain nanoparticles;
[0077] S2. 12 g of nanoparticles and 2.5 g of silane coupling agent KH792 were added to 200 mL of ethanol, heated to 45 ° C, stirred for 2.5 h, centrifuged, washed, and dried to obtain amino-modified nanoparticles;
[0078] S3. 13.5 g of calcium sulfate whiskers were added to 200 mL of water, 2.5 g of dopamine hydrochloride and 0.25 g of catalyst were added, heated to 45 ° C, stirred for 3 h, filtered, washed, and dried to obtain modified calcium sulfate whiskers;
[0079] The catalyst is a Tris-HCl solution with a pH of 8;
[0080] S4. 4 g of amino-modified nanoparticles and 7 g of modified calcium sulfate whiskers were stirred and mixed for 20 min to obtain a toughening agent with flame retardant effect.
[0081] Comparative Example 4
[0082] Compared with Example 3, the difference is that step S4 is not performed.
[0083] The details are as follows:
[0084] S1. 20 g of an aqueous solution containing 5.5 g of aluminum chloride was added dropwise to 100 g of a 1.5 mol / L NaOH solution, heated to 75 ° C, stirred for 1 h, at which time the pH value of the solution was 6.3, 20 g of an ethanol solution containing 1.5 g of tetrabutyl titanate was added dropwise, stirred for 1.5 h, centrifuged, washed, and dried to obtain nanoparticles;
[0085] S2. 12 g of nanoparticles and 2.5 g of silane coupling agent KH792 were added to 200 mL of ethanol, heated to 45 ° C, stirred for 2.5 h, centrifuged, washed, and dried to obtain amino-modified nanoparticles;
[0086] S3. 10 g of amino-modified nanoparticles were added to 200 mL of ethanol, 1 g of thiophene-2-carboxaldehyde was added, heated to 80 ° C, stirred for 5 h, and then 2.1 g of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide was added, stirred for 11 h, and flame-retardant nanoparticles were obtained;
[0087] S4. 4 g of flame retardant nanoparticles and 7 g of calcium sulfate whiskers were stirred and mixed for 20 minutes to obtain a toughening agent with flame retardant effect.
[0088] Test Example 1
[0089] The flame retardant toughening aids prepared in Examples 1-3 and Comparative Examples 1-4 were added to polypropylene resin (PP resin, T30S, Yuyao Jinlang Trading Co., Ltd.) at a content of 2wt%, mixed at 85°C for 10min by a high-speed mixer, placed in a HAKKE torque rheometer for mixing for 10min, and the processing temperature was set to 180°C. After mixing, the sample was cooled to room temperature and then crushed by a pulverizer, and then the crushed sample was pressed into various thickness samples using a flat vulcanizer (the press setting temperature was 180°C), and cut into various test specimens.
[0090] Limiting oxygen index (LOI) test: Tested according to GB / T2406-2009, the sample size is 80mm×10mm×4mm;
[0091] Vertical burning (UL94) test: tested in accordance with GB / T2408-2021, the specimen size is 125mm×13mm×3.2mm;
[0092] Impact performance was tested according to GB / T1043-2008. The size of the specimen was 80mm×10mm×3.2mm. Three specimens were tested in each group, and the average value of each group of results was taken.
[0093] The tensile properties were tested according to GB / T1040-2006, with a tensile speed of 50 mm / min, a strip thickness of 2 mm, a narrow part width of 4 mm, and each group was tested 3 times, and the average value of the results was taken;
[0094] The bending performance was tested according to GB / T9341-2008, with the test speed set at 2 mm / min, the sample size at 80 mm × 10 mm × 4 mm, the span at 64 mm, the indenter radius at 5 mm, and each group of tests was performed 3 times, and the average value of the results was taken.
[0095] The results are shown in Tables 1 and 2.
[0096] Table 1
[0097] Group LOI(%) UL-94(4mm) grade Example 1 32.2 V-0 Example 2 32.7 V-0 Example 3 33.1 V-0 Comparative Example 1 29.4 V-1 Comparative Example 2 25.7 V-1 Comparative Example 3 21.8 V-2 Comparative Example 4 30.4 V-0
[0098] It can be seen from the above table that the toughening additives with flame retardant effect prepared in Examples 1-3 of the present invention can significantly improve the flame retardant properties of PP resin.
[0099] Table 2
[0100]
[0101] It can be seen from the above table that the toughening additives with flame retardant effect prepared in Examples 1-3 of the present invention can significantly improve the mechanical properties of PP resin.
[0102] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a flame retardant toughening agent, characterized in that: The surface of Ti-doped nano-aluminum hydroxide particles is modified with a silane coupling agent with an amino group, reacted with thiophene-2-carboxaldehyde and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, and then blended with calcium sulfate whiskers modified with surface polydopamine to obtain a flame retardant toughening agent.
2. The method for preparing the toughening aid with flame retardant effect according to claim 1, characterized in that: The following steps are involved: S1. Add an aqueous solution of aluminum chloride to the alkali solution, heat and stir to react, at which time the pH value of the solution is 6.2-6.5, add an ethanol solution of tetrabutyl titanate, stir to react, centrifuge, wash, and dry to obtain nanoparticles; S2. adding the nanoparticles and the silane coupling agent with an amino group to ethanol, heating and stirring the reaction, centrifuging, washing, and drying to obtain amino-modified nanoparticles; S3. The amino-modified nanoparticles are added to ethanol, thiophene-2-carboxaldehyde is added, the reaction is heated and stirred, and then 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide is added, the reaction is stirred to obtain flame-retardant nanoparticles; S4. The calcium sulfate whiskers were added to water, dopamine hydrochloride and a catalyst were added, the reaction was heated and stirred, filtered, washed, and dried to obtain modified calcium sulfate whiskers; S5. Evenly mix the flame retardant nanoparticles and modified calcium sulfate whiskers to prepare a toughening agent with flame retardant effect.
3. The preparation method according to claim 2, characterized in that: The alkali solution in step S1 is 1-2 mol / L NaOH or KOH solution, the mass ratio of the alkali solution, aluminum chloride and tetrabutyl titanate is 100:4-7:1-2, the temperature of the heating and stirring reaction is 70-80°C, the time is 0.5-1h, and the stirring reaction time is 1-2h.
4. The preparation method according to claim 2, characterized in that: In step S2, the silane coupling agent with amino group is selected from at least one of KH550, KH602 and KH792, the mass ratio of the nanoparticles to the silane coupling agent with amino group is 10-15:2-3, the temperature of the heating and stirring reaction is 40-50° C., and the time is 2-3 hours.
5. The preparation method according to claim 2, characterized in that: In step S3, the mass ratio of the amino-modified nanoparticles, thiophene-2-carboxaldehyde, and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide is 10:0.7-1.2:1.5-2.4, the temperature of the heating and stirring reaction is 75-85° C., the time is 4-6 hours, and the stirring reaction time is 10-12 hours.
6. The preparation method according to claim 2, characterized in that: The mass ratio of the calcium sulfate whiskers, dopamine hydrochloride and catalyst in step S4 is 12-15:2-3:0.2-0.3, the catalyst is a Tris-HCl solution with a pH of 7.5-8.5, the temperature of the heating and stirring reaction is 40-50° C., and the time is 2-4 hours.
7. The preparation method according to claim 2, characterized in that: The mass ratio of the flame retardant nanoparticles to the modified calcium sulfate whiskers in step S5 is 3-5:
7.
8. The preparation method according to claim 2, characterized in that: The specific steps include: S1. Add 20 parts by weight of an aqueous solution containing 4-7 parts by weight of aluminum chloride to 100 parts by weight of a 1-2 mol / L NaOH or KOH solution, heat to 70-80°C, stir and react for 0.5-1h, at which time the pH value of the solution is 6.2-6.5, add 20 parts by weight of an ethanol solution containing 1-2 parts by weight of tetrabutyl titanate, stir and react for 1-2h, centrifuge, wash, and dry to obtain nanoparticles; S2. 10-15 parts by weight of the nanoparticles and 2-3 parts by weight of a silane coupling agent with an amino group are added to ethanol, heated to 40-50 ° C, stirred for 2-3h, centrifuged, washed, and dried to obtain amino-modified nanoparticles; S3. Add 10 parts by weight of amino-modified nanoparticles to ethanol, add 0.7-1.2 parts by weight of thiophene-2-carboxaldehyde, heat to 75-85 ° C, stir and react for 4-6 hours, then add 1.5-2.4 parts by weight of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, stir and react for 10-12 hours to obtain flame retardant nanoparticles; S4. 12-15 parts by weight of calcium sulfate whiskers are added to water, 2-3 parts by weight of dopamine hydrochloride and 0.2-0.3 parts by weight of a catalyst are added, heated to 40-50 ° C, stirred for 2-4h, filtered, washed, and dried to obtain modified calcium sulfate whiskers; The catalyst is a Tris-HCl solution with a pH of 7.5-8.5; S5. Mix 3-5 parts by weight of flame-retardant nanoparticles and 7 parts by weight of modified calcium sulfate whiskers to obtain a toughening agent with flame retardant effect.
9. A toughening aid with flame retardant effect obtained by the preparation method according to any one of claims 1 to 8.
10. Use of the toughening agent with flame retardant effect as claimed in claim 9 for improving the flame retardancy and toughness of plastic products.
Citation Information
Patent Citations
Flame-retardant thermoplastic vulcanized rubber material
CN106519460A
Novel thienyl-containing DOPO flame retardant, and synthesis method and application thereof
CN113337005A
Producing method for complex retardant
KR1020120051190A
Cited By
Flame-retardant silicone rubber heat insulation pad for lithium battery module
CN121642324A