Solid-phase regenerated rubber as well as preparation method and application thereof
By using diazon compounds or reverse vulcanized copolymers in waste rubber for hot pressing vulcanization, combined with the C-H bond functionalization strategy, a solid phase regenerated rubber with high tensile strength was prepared, which solved the fracture and performance of rubber molecular chains in the prior art. The problem of decline has achieved efficient upgrading and recycling of waste rubber and environmentally friendly vulcanization processes.
Patent Information
- Application Number
- CN202410997874.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-24
AI Technical Summary
Among the existing waste rubber recycling technology, desulfurization and regeneration technology leads to the breakage of the rubber molecular chain, which reduces performance, and is accompanied by high pollution and high energy consumption, and the sulfur vulcanization network cannot be processed, resulting in a decrease in the performance of composite materials.
A specific diazonium compound or reverse vulcanized copolymer is mixed with waste rubber and heat-pressed vulcanized under specific conditions to prepare solid phase regenerated rubber with higher tensile strength, and the compound is functionalized through C-H bonds as an interface modifier , improve the tensile strength and fatigue threshold of rubber.
It significantly improves the tensile strength and fatigue threshold of solid-phase recycled rubber, provides new means of upgrading and recycling of waste rubber, overcomes the problems of performance reduction and pollution of the existing technology, and has good application prospects.
Smart Images

Figure CN118909335A_ABST
Abstract
Description
Technical Field
[0001] The embodiments of the present application relate to the technical field of waste rubber recycling, and in particular to a solid phase recycled rubber and a preparation method and application thereof. Background Art
[0002] Due to its unique high elasticity, rubber is widely used in aerospace, national defense, tires, medical elastomers and other fields, and plays a very important role in national economic construction. However, such a wide range of applications also brings huge recycling pressure. At present, there are about 4 billion waste tires discarded or idle in the world. The recycling of waste rubber around the world has a great impact on the environment, energy and climate, and has caused "black pollution" that is more difficult to control than "white pollution".
[0003] At present, the recycling method of waste rubber is mainly "downgrading", such as mechanical destruction and recycling as low-value materials for reuse. The production of recycled rubber is the main way to recycle waste rubber at a high value. However, the desulfurization regeneration technology will inevitably lead to the breakage of the main chain of the rubber molecule chain, which will reduce the performance of the recycled rubber and is accompanied by disadvantages such as high pollution and high energy consumption. In addition, due to the characteristics of the sulfur vulcanization network that cannot be reprocessed, there will be phase separation when waste rubber is used as a filler and blended with virgin rubber or other matrices, resulting in a significant reduction in the performance of the composite material. Summary of the invention
[0004] In view of this, an embodiment of the present application provides a solid-phase regenerated rubber and a preparation method and application thereof. The solid-phase regenerated rubber has better tensile strength and can effectively overcome the defects of the above-mentioned prior art.
[0005] A first aspect of an embodiment of the present application provides a solid phase regenerated rubber, comprising the following preparation raw materials calculated by weight: 1-100 parts of waste rubber and 0.1-20 parts of diazo compound / reverse vulcanization copolymer.
[0006] In some embodiments that may include the above embodiments, the following raw materials are included in the preparation, calculated by weight: 100 parts of virgin rubber, 0.1-20 parts of inverse vulcanization copolymer, 1-10 parts of zinc oxide, 1-5 parts of stearic acid, 1-5 parts of accelerator, 0.1-6 parts of sulfur, and 1-60 parts of waste rubber.
[0007] In some embodiments that may include the above embodiments, the following raw materials are included in parts by weight: 100 parts of virgin rubber, 0.1-20 parts of diazo compounds, and 1-60 parts of waste rubber.
[0008] In some embodiments that may include the above embodiments, the reverse vulcanization copolymer is at least one of a hydroxyl-based reverse vulcanization copolymer, a lipoic acid-based reverse vulcanization copolymer, and a carboxyl-based reverse vulcanization copolymer.
[0009] In some embodiments, which may include the aforementioned embodiments, the diazo compound is a diazo compound containing a dynamic disulfide bond or a covalent bond.
[0010] In some embodiments that may include the above embodiments, the virgin rubber is natural rubber or synthetic rubber; or
[0011] The virgin rubber is at least one of isoprene rubber, styrene-butadiene rubber, butadiene rubber, nitrile rubber, butyl rubber, ethylene-propylene rubber, and chloroprene rubber; or
[0012] The waste rubber is factory-grade waste rubber.
[0013] A second aspect of the embodiment of the present application further provides a method for preparing the above-mentioned solid phase regenerated rubber, comprising the following steps:
[0014] S1. Preparation of a diazo compound: dissolving 2-hydroxyethyl disulfide (preferably bis(2-hydroxyethyl) disulfide) / ethylene glycol, pyridine, and phenylacetyl chloride in dichloromethane, reacting at room temperature for 1-12 hours, and purifying to obtain the first-step product; dissolving the first-step product, tosyl azide, and 1,8-diazabicyclo[5.4.0]undec-7-ene in dichloromethane, reacting at room temperature for 1-12 hours, and purifying to obtain a diazo compound;
[0015] S2. Preparing solid-phase regenerated rubber: mixing the diazo compound with waste rubber or mixing the diazo compound, virgin rubber, and waste rubber, and performing hot-pressing vulcanization at 100-145° C., with a vulcanization time of 15-30 min and a vulcanization pressure of 10-15 MPa to obtain solid-phase regenerated rubber.
[0016] In some embodiments that may include the above embodiments, in step S1, the molar ratio of the 2-hydroxyethyl disulfide / ethylene glycol, pyridine and phenylacetyl chloride is 1:(0.5-6):(0.5-6); the molar ratio of the first step product, tosyl azide and 1,8-diazabicyclo[5.4.0]undec-7-ene is 1:(0.5-6):(0.5-6).
[0017] The third aspect of the embodiment of the present application further provides a method for preparing the above-mentioned solid phase regenerated rubber, comprising the following steps:
[0018] S1. Preparation of inverse vulcanized copolymer: sulfur, monomer and accelerator are mixed and reacted at 130-160° C. for 3-8 hours to obtain inverse vulcanized copolymer;
[0019] Preferably, in step S1, the mass ratio of sulfur, monomer and accelerator is (0.5-5):1:(0.1-1); preferably, the monomer is at least one of Span80, lipoic acid, lipoic acid derivatives and undecylenic alcohol.
[0020] S2. Preparation of solid phase regenerated rubber: mixing the reverse vulcanized copolymer, virgin rubber, zinc oxide, stearic acid, accelerator, sulfur and waste rubber or mixing the reverse vulcanized copolymer and waste rubber, and performing hot pressing vulcanization at 100-145° C., the vulcanization time is 15-30 min, and the vulcanization pressure is 10-15 MPa to obtain solid phase regenerated rubber.
[0021] A fourth aspect of the embodiments of the present application also provides the use of the above-mentioned solid phase regenerated rubber in the preparation of gaskets, rubber blended materials or equipment for tire / bridge engineering materials.
[0022] Compared with the prior art, the embodiments of the present application have the following beneficial effects:
[0023] The present application adopts a specific compound or polymer with CH bond functionalization as an interfacial modifier, which can significantly improve the tensile strength of solid-phase recycled rubber and the tensile strength and fatigue threshold of solid-phase recycled rubber under a specific accelerator, thereby providing a new means for the upgrading and recycling of waste rubber and having good application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0025] Figure 1 is the stress-strain curve of the solid phase regenerated rubber in Example 1 of the present application;
[0026] Figure 2 This is a curve showing the relationship between the crack growth rate and G of the solid phase regenerated rubber in Example 5 of the present application. DETAILED DESCRIPTION
[0027] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0028] Unless otherwise specified, the experimental methods used in the examples of this application are all conventional methods.
[0029] In the following examples and comparative examples, unless otherwise specified, all raw materials can be obtained by commercial purchase or conventional methods.
[0030] Example 1
[0031] The method for preparing solid phase regenerated rubber in this embodiment comprises the following steps:
[0032] 9.255 g of ethylene glycol and 10.441 g of pyridine were dissolved in dichloromethane, 20.406 g of phenylacetyl chloride was added dropwise, and the mixture was stirred at room temperature for 12 h. The product was purified to obtain the first-stage product. 1 g of the first-stage product and 4.01 g of TsN 3 (toluenesulfonyl azide), 4.01 g DBU (1,8-diazabicyclo[5.4.0]undec-7-ene), stirred at room temperature for 12 h, and purified to obtain a diazo compound;
[0033] 0.48 parts of bis-diazo compound (BD) and 24 parts of waste rubber powder (i.e., powdered waste rubber) (80 mesh) were mixed in dichloromethane, and the solvent was removed by rotary evaporation to coat the surface of the waste rubber powder (i.e., powdered waste rubber). The mixture was hot-pressed and vulcanized at a temperature of 145°C, the vulcanization time was 30 minutes, and the vulcanization pressure was 15 MPa, to finally obtain a solid phase recycled rubber (sheet).
[0034] According to GB / T 528-2009, the prepared sheets were cut into dumbbell-shaped specimens, and the stress-strain curves were obtained using a high-speed rail AI-3000 tensile testing machine ( Figure 1 ), the tensile strength of the sheet is 2MPa.
[0035] The tensile strength is the stress at which the specimen breaks.
[0036] Example 2
[0037] The method for preparing solid phase regenerated rubber in this embodiment comprises the following steps:
[0038] 9.255 g of 2-hydroxyethyl disulfide and 10.441 g of pyridine were dissolved in dichloromethane, 20.406 g of phenylacetyl chloride was added dropwise, and the mixture was stirred at room temperature for 12 h. The product was purified to obtain the first-stage product. 1 g of the first-stage product and 4.01 g of TsN 3 , 4.01 g DBU, stirred at room temperature for 12 h, and purified to obtain a disulfide bond-containing diazo compound;
[0039] 0.48 parts of bis-diazo compounds with disulfidebonds (BDS) and 24 parts of waste rubber powder (i.e., powdered waste rubber) (80 mesh) were mixed in dichloromethane, and the solvent was removed by rotary evaporation to coat the surface of the waste rubber powder (i.e., powdered waste rubber). The mixture was hot-pressed and vulcanized at a temperature of 145°C, the vulcanization time was 30 minutes, and the vulcanization pressure was 15 MPa, to finally obtain a solid phase recycled rubber (sheet).
[0040] The tensile strength of the sheet was tested according to the method described in Example 1, and the tensile strength of the sheet was found to be 2.5 MPa.
[0041] The obtained sheet was cut into pieces and hot-pressed and vulcanized again at 145°C for 20 min and 15 MPa to obtain a reprocessed sheet. The tensile strength was tested again according to the method described in Example 1, and the tensile strength of the sheet was 1.7 MPa.
[0042] Example 3
[0043] The method for preparing solid phase regenerated rubber in this embodiment comprises the following steps:
[0044] Add 45g of sulfur into a three-necked flask, heat to 160°C, maintain for 5 minutes, then add 45g of Span80 and 0.9g of accelerator ZDC, react for 3-4 hours to obtain Span80 reverse vulcanized copolymer;
[0045] 1.2 parts of Span80 reverse vulcanized copolymer and 24 parts of waste rubber powder (i.e., powdered waste rubber) (80 mesh) were mixed and dissolved in tetrahydrofuran, and the solvent was removed by rotary evaporation to coat the surface of the waste rubber powder (i.e., powdered waste rubber) with the reverse vulcanized copolymer. The mixture was hot-pressed and vulcanized at a temperature of 145°C, the vulcanization time was 30 minutes, and the vulcanization pressure was 15 MPa, to finally obtain a solid phase recycled rubber (sheet).
[0046] The tensile strength of the sheet was tested according to the method described in Example 1, and the tensile strength of the sheet was found to be 4.5 MPa.
[0047] Example 4
[0048] The method for preparing solid phase regenerated rubber in this embodiment comprises the following steps:
[0049] 70 g of sulfur was added into a three-necked flask, and the temperature was raised to 150° C., and then 30 g of thioctic acid and 3 g of accelerator N-methylimidazole were added after maintaining for 5 min, and the reaction was continued for 8 h to obtain a thioctic acid reverse vulcanized copolymer;
[0050] 0.48 parts of lipoic acid reverse vulcanized copolymer and 24 parts of waste rubber powder (i.e. powdered waste rubber) (80 mesh) were mixed in tetrahydrofuran, the solvent was removed by rotary evaporation, the reverse vulcanized copolymer was coated on the surface of the waste rubber powder (i.e. powdered waste rubber), and hot-pressed vulcanized at a temperature of 145°C, the vulcanization time was 30 minutes, and the vulcanization pressure was 15 MPa, and finally a solid phase recycled rubber (sheet) was obtained.
[0051] The tensile strength of the sheet was tested according to the method described in Example 1, and the tensile strength of the sheet was found to be 3.7 MPa.
[0052] The obtained sheet was cut into pieces and hot-pressed and vulcanized again at 145°C for 20 minutes at a pressure of 15 MPa. The tensile strength of the reprocessed sheet was 2.5 MPa.
[0053] Example 5
[0054] The method for preparing solid phase regenerated rubber in this embodiment comprises the following steps:
[0055] 21g of sulfur was added into a three-necked flask, and the temperature was raised to 150°C. After maintaining the temperature for 5 minutes, 9g of lipoic acid and 0.9g of accelerator NMI were added, and the reaction was continued for 6-8 hours to obtain a lipoic acid reverse vulcanized copolymer;
[0056] On an open mixing mill, 2 parts of thioctic acid reverse vulcanization copolymer, 5 parts of zinc oxide, 1 part of stearic acid, 1.5 parts of accelerator CZ, 0.5 parts of accelerator DM, 1.5 parts of sulfur, and 20 parts of waste rubber powder (i.e. powdered waste rubber) (80 mesh) were added to 100 parts of isoprene rubber, and the mixture was evenly mixed and then vulcanized at a vulcanization temperature of 145°C, a vulcanization time of 30 min, and a vulcanization pressure of 15 MPa to finally obtain a solid phase recycled rubber (sheet).
[0057] The tensile strength of the sheet was tested according to the method described in Example 1, and the tensile strength of the sheet was found to be 25 MPa.
[0058] The sheet was prepared into a sample with a width of 100 mm, a height of 20 mm, and a thickness of 1 mm. A crack was prefabricated in the middle of the sample according to the GB / T 41941-2022 test standard, and the fatigue threshold of the sample was tested. The fatigue threshold of the sheet was expected to be 500 J / m 2 .
[0059] The fatigue threshold is the minimum energy required for crack extension under cyclic load. According to the formula G = W(λ)·H0 (G is the energy release rate, W(λ) is the elastic energy stored in the sample, and H0 is the initial length of the sample), the relationship curve between the crack growth rate and G is plotted ( Figure 2 ), and obtain the fatigue threshold.
[0060] Example 6
[0061] The method for preparing solid phase regenerated rubber in this embodiment comprises the following steps:
[0062] Add 45g of sulfur into a three-necked flask, heat to 160°C, maintain for 5 minutes, then add 45g of Span80 and 0.9g of accelerator ZDC, react for 3-4 hours to obtain Span80 reverse vulcanized copolymer;
[0063] On an open mixing mill, 2 parts of Span80 inverse vulcanization copolymer, 5 parts of zinc oxide, 1 part of stearic acid, 1.5 parts of accelerator CZ, 0.5 parts of accelerator DM, 1.5 parts of sulfur, and 20 parts of waste rubber powder (i.e. powdered waste rubber) (80 mesh) were added to 100 parts of isoprene rubber, and the mixture was evenly mixed and then vulcanized at a vulcanization temperature of 145°C, a vulcanization time of 30 min, and a vulcanization pressure of 15 MPa to finally obtain solid phase recycled rubber (sheet).
[0064] The tensile strength of the sheet was tested according to the method described in Example 1, and the tensile strength of the sheet was estimated to be 25 MPa. The fatigue threshold of the sheet was tested according to the method described in Example 5, and the fatigue threshold of the sheet was estimated to be 500 J / m 2 .
[0065] Comparative Example 1
[0066] 24 parts of waste rubber powder (i.e., powdered waste rubber) (80 mesh) were hot-pressed and vulcanized at 145°C, with a vulcanization time of 30 min and a vulcanization pressure of 15 MPa. The samples were cut according to the method described in Example 1, but a complete dumbbell-shaped sample could not be obtained, and the sample did not have the reprocessing capability. The results show that the interface effect and performance of the solid-phase regenerated rubber prepared based on the CH bond functionalization strategy are greatly improved.
[0067] Comparative Example 2
[0068] On an open mill, add 5 parts of zinc oxide, 1 part of stearic acid, 1.5 parts of accelerator CZ, 0.5 parts of accelerator DM, 1.5 parts of sulfur, and 20 parts of waste rubber powder (i.e. powdered waste rubber) (80 mesh) to 100 parts of isoprene rubber, mix well and then vulcanize. The vulcanization temperature is 145°C, the vulcanization time is 30 minutes, and the vulcanization pressure is 15MPa.
[0069] The tensile strength of the sheet was tested according to the method described in Example 1, and the tensile strength of the sheet was 3.7 MPa. The fatigue threshold of the sheet was tested according to the method described in Example 5, and the fatigue threshold of the sheet was about 50 J / m 2 The test results show that the tensile strength and fatigue threshold of the solid phase recycled rubber (sheet) prepared based on the CH bond functionalization strategy obtained in this application are significantly increased compared with traditional vulcanized rubber.
[0070] In summary, the present application provides a method for preparing solid-phase regenerated rubber based on a CH bond functionalization strategy. The present application adopts a specific CH bond functionalized compound as an interfacial modifier, which can significantly improve the interfacial effect between solid-phase regenerated rubbers and the tensile strength of solid-phase regenerated rubbers under general rubber vulcanization conditions, providing a new means for the upgrading and recycling of waste rubber and having good application scenarios.
[0071] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.
Claims
1. A solid phase regenerated rubber, characterized in that: The preparation method comprises the following raw materials calculated by weight: 1-100 parts of waste rubber and 0.1-20 parts of diazo compound / reverse vulcanization copolymer.
2. The solid phase regenerated rubber according to claim 1, characterized in that: The preparation method comprises the following raw materials calculated by weight: 100 parts of virgin rubber, 0.1-20 parts of inverse vulcanized copolymer, 1-10 parts of zinc oxide, 1-5 parts of stearic acid, 1-5 parts of accelerator, 0.1-6 parts of sulfur and 1-60 parts of waste rubber.
3. The solid phase regenerated rubber according to claim 1, characterized in that: The preparation method comprises the following raw materials calculated by weight: 100 parts of virgin rubber, 0.1-20 parts of diazo compounds and 1-60 parts of waste rubber.
4. The solid phase regenerated rubber according to claim 1 or 2, characterized in that: The reverse vulcanization copolymer is at least one of a hydroxyl reverse vulcanization copolymer, a lipoic acid reverse vulcanization copolymer, and a carboxyl reverse vulcanization copolymer.
5. The solid phase regenerated rubber according to claim 1 or 3, characterized in that: The diazo compound is a diazo compound containing a dynamic disulfide bond or a covalent bond.
6. The solid phase regenerated rubber according to claim 2 or 3, characterized in that: The virgin rubber is natural rubber or synthetic rubber; or The virgin rubber is at least one of isoprene rubber, styrene-butadiene rubber, butadiene rubber, nitrile rubber, butyl rubber, ethylene-propylene rubber, and chloroprene rubber; or The waste rubber is factory-grade waste rubber.
7. A method for preparing solid phase regenerated rubber according to claim 1 or 3, characterized in that: The following steps are involved: S1. Preparation of diazo compounds: dissolving 2-hydroxyethyl disulfide / ethylene glycol, pyridine, and phenylacetyl chloride in dichloromethane, reacting at room temperature, and purifying to obtain the first-step product; dissolving the first-step product, tosyl azide, and 1,8-diazabicyclo[5.4.0]undec-7-ene in dichloromethane, reacting at room temperature, and purifying to obtain a diazo compound; S2. Preparing solid-phase regenerated rubber: mixing the diazo compound with waste rubber or mixing the diazo compound, virgin rubber, and waste rubber, and performing hot-pressing vulcanization at 100-145° C., with a vulcanization time of 15-30 min and a vulcanization pressure of 10-15 MPa to obtain solid-phase regenerated rubber.
8. The preparation method according to claim 7, characterized in that: In step S1, the molar ratio of the 2-hydroxyethyl disulfide / ethylene glycol, pyridine and phenylacetyl chloride is 1:(0.5-6):(0.5-6); the molar ratio of the first step product, toluenesulfonyl azide and 1,8-diazabicyclo[5.4.0]undec-7-ene is 1:(0.5-6):(0.5-6).
9. A method for preparing solid phase regenerated rubber according to claim 1 or 2, characterized in that: The following steps are involved: S1. Preparation of inverse vulcanized copolymer: sulfur, monomer and accelerator are mixed and reacted at 130-160° C. for 3-8 hours to obtain inverse vulcanized copolymer; Wherein, in step S1, the mass ratio of sulfur, monomer and accelerator is (0.5-5):1:(0.1-1); S2. Preparation of solid phase regenerated rubber: mixing the reverse vulcanized copolymer, virgin rubber, zinc oxide, stearic acid, accelerator, sulfur and waste rubber or mixing the reverse vulcanized copolymer and waste rubber, and performing hot pressing vulcanization at 100-145° C., the vulcanization time is 15-30 min, and the vulcanization pressure is 10-15 MPa to obtain solid phase regenerated rubber.
10. Use of the solid phase regenerated rubber according to any one of claims 1 to 6 in the preparation of gaskets, rubber blending materials or equipment for tire / bridge engineering materials.
Citation Information
Patent Citations
Composition based on natural rubber and carbon black comprising hydrazide, hydrazone and polyamine
CN103261300A
Reclaiming agent, reclaimed rubber prepared therefrom, and preparation method of reclaimed rubber
CN103435843A
Recycled rubber product
CN107857916A
Solid-phase regenerated rubber and preparation method thereof
CN111454484A
Recycled rubber
CN112812358A