Bending-resistant winding core pipe and preparation method thereof

By using glass fiber composite components and epoxy soybean oil reinforcement system in the core tube, combined with modified glass fiber and graphene oxide, the problem of deformation of the core tube during storage and transportation is solved, and the mechanical strength and stability are improved Improves the storage effect of the film.

CN118909350APending Publication Date: 2024-11-08SUZHOU TIANYU PLASTIC +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410988993.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

During the film production process, the long-rolled core tube is prone to deform during storage and transportation, affecting the storage effect of the film.

Method used

By adding glass fiber composite components and epoxy soybean oil reinforcement system to the core tube, combining silane coupling agent with oleic acid-modified glass fiber and graphene oxide with phenolic resin, the mechanical strength of the core tube is enhanced and stability.

Benefits of technology

It significantly improves the overall mechanical strength and stability of the core tube, reduces deformation, and improves the storage and transportation quality of the film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004958336490000081
    Figure BDA0004958336490000081
Patent Text Reader

Abstract

The invention relates to a bending-resistant winding core pipe and a preparation method thereof. The bending-resistant winding core pipe is prepared from the following components in parts by mass: 64 to 80 parts of polypropylene, 48 to 66 parts of silica gel powder, 64 to 80 parts of ABS (Acrylonitrile Butadiene Styrene) plastic, 440 to 700 parts of thermoplastic resin, 104 to 130 parts of polylactic acid, 40 to 50 parts of a glass fiber composite component, 24 to 28 parts of an epoxidized soybean oil reinforcing system and 16 to 20 parts of a weather-resistant agent. The glass fiber composite component comprises modified glass fiber, phenolic resin and graphene oxide. The winding core pipe has the effect of improving the bending resistance of the winding core pipe.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of core-rolling tubes, and in particular to a bending-resistant core-rolling tube and a preparation method thereof. Background Art

[0002] At present, with the development of industry, industrial film technology is applied in various fields, and the requirements for film precision are constantly increasing. In the film production process, the film usually needs to be rolled onto a reel for easy transportation and storage. Therefore, the quality of the reel is also an important factor affecting the storage and transportation quality of the prepared film after rolling.

[0003] When a wide film is rolled up, due to the quality of the film itself, especially the long winding tube, the winding tube is easily deformed during storage and transportation, thus affecting the storage effect of the film. Summary of the invention

[0004] In order to improve the stability of a winding core tube, the present application provides a bending-resistant winding core tube and a preparation method thereof.

[0005] The present application provides a bending-resistant coiled core tube and a preparation method thereof, which adopts the following technical solutions: In the first aspect, the present application provides a bending-resistant coiled core tube, which adopts the following technical solution: A bending-resistant coiled core tube comprises the following components in parts by weight: 64-80 parts of polypropylene, 48-66 parts of silica gel powder, 64-80 parts of ABS plastic, 440-700 parts of thermoplastic resin, 104-130 parts of polylactic acid, 40-50 parts of glass fiber composite components, 24-28 parts of epoxy soybean oil reinforcement system, and 16-20 parts of weathering agent; the glass fiber composite components include modified glass fiber, phenolic resin and graphene oxide.

[0006] By adopting the above technical scheme, a glass fiber composite component and an epoxy soybean oil reinforcement system are added to the core tube component, so as to compositely improve the overall mechanical strength of the prepared curved core tube. The glass fiber composite component includes modified glass fiber, phenolic resin and graphene oxide. Phenolic resin is a resin matrix with good thermal insulation performance and stability, and has good heat resistance. A large number of oxygen-containing hydrophilic functional groups are attached to the surface of graphene oxide, which plays a key role in improving the performance of the material. After combining with glass fiber, the glass fiber system can form a stable network structure, so that the components in the core tube system are more tightly connected, thereby improving the overall mechanical strength of the core tube.

[0007] Preferably, the modified glass fiber is prepared by the following method: A silane coupling agent, deionized water and anhydrous ethanol are mixed and stirred to obtain a silane coupling agent solution, glass fiber is added to the silane coupling agent solution, the temperature is increased and allowed to stand, and then the glass fiber is taken out and heated to react to obtain a silane-treated glass fiber, the silane-treated glass fiber is mixed with deionized water, stirred and oleic acid is added to react, and the modified glass fiber is obtained after filtering and washing.

[0008] By adopting the above technical scheme, the surface of the glass fiber is modified using a silane coupling agent and oleic acid, and the Si-OH after hydrolysis of the silane coupling agent reacts with the Si-OH on the surface of the glass fiber to form a stable Si-O-Si bond. After the silane-modified glass fiber is hydrolyzed, more hydroxyl groups are obtained, which form hydrogen bonds with the carboxyl groups on the oleic acid molecular chain, thereby improving the interfacial compatibility of the glass fiber and making the glass fiber distribution more uniform, thereby improving the prepared glass fiber composite component to better improve the performance of polylactic acid, so as to improve the overall stability and mechanical properties of the prepared winding core tube.

[0009] Preferably, the mass ratio of the glass fiber, the silane coupling agent and the oleic acid is 1:0.15:(1.4-1.6).

[0010] By adopting the above technical solution, the mass ratio of the glass fiber, the silane coupling agent and the oleic acid is preferably within the above range, which can further improve the overall stability of the modified glass fiber.

[0011] Preferably, the glass fiber composite component is prepared by the following method: Phenol, formaldehyde and sodium hydroxide are mixed and reacted, ultrasonically treated, and then the graphene oxide aqueous solution is added to the reaction system, and the reaction is continued to obtain a graphene oxide-phenolic resin solution. After the system is cooled, melamine and urea are added, and the temperature is increased to continue the reaction. After the reaction, ammonium sulfate is added after cooling, and a composite is obtained after stirring. The modified glass fiber is added to the composite and allowed to stand, and a glass fiber composite component is obtained after filtering.

[0012] By adopting the above technical scheme, phenolic resin is prepared by phenol and formaldehyde. After adding graphene oxide, the spacing between graphene oxide flakes is increased due to the large number of hydrophilic functional groups on the surface of graphene oxide, and the graphene oxide flakes are intercalated between the phenolic resins, so that hydrogen bonds are formed between the surface functional groups of graphene oxide and the phenolic resin, thereby enhancing the interfacial force. At the same time, the surface roughness of graphene oxide is increased, and the relative slip between graphene oxide and phenolic resin is reduced. The graphene oxide is combined with modified glass fiber to improve the overall mechanical properties and greatly improve the stability, thereby improving the stability of the prepared rolled core tube.

[0013] Preferably, the mass fraction of graphene oxide in the graphene oxide aqueous solution is 0.7-0.9%.

[0014] By adopting the above technical solution, preferably the mass fraction of graphene oxide in the graphene oxide aqueous solution is within the above range, which can further improve the overall stability of the prepared modified glass fiber composite material.

[0015] Preferably, the raw materials of the epoxy soybean oil enhancement system include epoxy soybean oil, acetylglycine and sebacic acid.

[0016] By adopting the above technical scheme, an epoxidized soybean oil reinforcement system is prepared by using epoxidized soybean oil, sebacic acid and acetylglycine. After compounding with polylactic acid, the impact resistance of polylactic acid can be improved, and its mechanical strength can be improved, thereby improving the overall strength of the core tube.

[0017] Preferably, the epoxidized soybean oil enhancement system is prepared by the following method: After mixing sebacic acid, epoxidized soybean oil and a catalyst, acetylglycine is added, and the mixture is reacted after heating in an oil bath to obtain an epoxidized soybean oil enhanced system.

[0018] By adopting the above technical scheme, the epoxy groups of epoxidized soybean oil and the double-end carboxyl groups of sebacic acid are used for ring-opening pre-curing. After adding acetylglycine, the carboxyl groups of acetylglycine undergo a ring-opening reaction on the epoxy groups of the epoxidized soybean oil, and amide groups are introduced to form hydrogen bonds, thereby preparing an epoxidized soybean oil reinforcement system. After combining with polylactic acid, the mechanical properties of polylactic acid can be effectively improved, and the compatibility between polylactic acid and other components can be improved, thereby improving the stability of the prepared roll core tube.

[0019] Preferably, the mass ratio between the epoxy soybean oil and acetylglycine is 1:(0.035-0.045).

[0020] By adopting the above technical solution, the mass ratio between the epoxy soybean oil and acetylglycine is preferably within the above range, which can effectively improve the overall stability of the epoxy soybean enhancement system.

[0021] Preferably, the catalyst is 4-dimethylaminopyridine.

[0022] In a second aspect, the present application provides a method for preparing a bending-resistant rolled core tube, which adopts the following technical solution: A method for preparing a bending-resistant coiled core tube comprises the following steps: Polylactic acid and an epoxy soybean oil reinforcing system are vulcanized to obtain a mixture, the mixture, polypropylene, silica gel powder, ABS plastic, thermoplastic resin, modified glass fiber and a weathering agent are mixed, the mixture is heated and stirred to obtain a mixed material, the mixed material is added to a twin-screw extruder, and the mixture is cooled after extrusion to obtain a bending-resistant coiled core tube.

[0023] In summary, the present application includes at least one of the following beneficial technical effects: 1. Adding weathering agent to the core tube component can reduce the phenomenon of thermal expansion and contraction of the core tube and improve the stability of the core tube. Adding glass fiber composite component and epoxy soybean oil reinforcement system to the core tube can improve the overall mechanical strength of the prepared curved core tube. Among them, the glass fiber composite component includes modified glass fiber, phenolic resin and graphene oxide. After compounding, the three can effectively improve the stability of polylactic acid, improve the overall mechanical strength of the core tube, and reduce the occurrence of deformation of the core tube. 2. Use silane coupling agent and oleic acid to modify the glass fiber, thereby improving the interfacial compatibility of the glass fiber, making the glass fiber distribution more uniform, and further improving the stability of the prepared product; 3. Inserting graphene oxide between phenolic resins forms hydrogen bonds between the surface functional groups of graphene oxide and the phenolic resin, thereby enhancing the interfacial force and improving the roughness of the graphene oxide surface. The bonding effect between the graphene oxide and the silane-modified glass fiber is further improved, thereby enhancing the stability of the system; 4. The epoxy soybean oil reinforcement system was prepared by epoxy soybean oil, sebacic acid and acetylglycine, which improved the compatibility of polylactic acid and effectively improved the stability of the whole system, thereby improving the mechanical strength of the prepared roll core tube. DETAILED DESCRIPTION

[0024] The present application is further described in detail below with reference to the embodiments: In the embodiment of the present application, the weathering agent is the heat resistant agent MS-NB, the silane coupling agent is γ-aminopropyltriethoxysilane, and the thermoplastic resin is polypropylene.

[0025] Example 1 Preparation of modified glass fiber: 7.5 g of γ-aminopropyltriethoxysilane, 25 g of deionized water and 120 g of anhydrous ethanol were mixed, stirred and hydrolyzed for 30 min to obtain a silane coupling agent solution, 50 g of glass fiber was added to the silane coupling agent solution, the temperature was raised to 80°C and allowed to stand for 8 h, then the glass fiber was taken out, and fully reacted in a vacuum drying oven at 120°C for 1 h to obtain silane-treated glass fiber, the silane-treated glass fiber was mixed with 200 g of deionized water, stirred at a speed of 100 r / min and heated to 80°C, 70 g of oleic acid (CAS No.: 112-80-1) was added, the temperature was maintained for 8 h, and the modified glass fiber was obtained after filtering and washing.

[0026] Preparation of glass fiber composite components: 30g of phenol, 90g of formaldehyde and 7.5g of sodium hydroxide were mixed for reaction. When the reaction temperature rose to 75°C, the system was ultrasonically treated for 3h, and then 20g of a graphite oxide solution with a mass fraction of 0.7% was added to the reaction system, and the reaction was continued at 75°C for 2h to obtain a graphene oxide-phenolic resin solution. The system was cooled to 40°C, 30g of melamine and 120g of urea were added, the temperature was raised to 55°C and the reaction was continued for 40min. After cooling to 25°C, 5wt% of ammonium sulfate was added, and a composite was obtained after stirring for 30s. 50g of modified glass fiber was added to the composite and allowed to stand for 12h. The glass fiber composite component was obtained after filtration.

[0027] Preparation of epoxidized soybean oil enhanced system: After mixing 5 g of sebacic acid, 40 g of epoxidized soybean oil (CAS No.: 8013-07-8) and 0.2 g of catalyst 4-dimethylaminopyridine (CAS No.: 1122-58-3), 1.4 g of acetylglycine (CAS No.: 543-24-8) was added, the temperature was raised to 160° C. under oil bath conditions, and then under nitrogen protection, magnetic stirring was carried out for 40 minutes to obtain an epoxidized soybean oil enhanced system.

[0028] Preparation of bend-resistant coiled core tube: 104g of polylactic acid and 24g of epoxy soybean oil reinforcement system are vulcanized at a speed of 80r / min for 12min at 180°C to obtain a mixture; the above-prepared mixture, 48g of silica gel powder, 64g of ABS plastic, 440g of thermoplastic resin, 40g of glass fiber composite component and 16g of weathering agent are mixed, the temperature is raised to 80°C, and stirred at a speed of 800r / min for 10min to obtain a mixture; the mixture is added to a twin-screw extruder, the temperature of each zone is set at 270°C, the head temperature is 240°C, the twin-screw speed is 280r / min, the feeding speed is 40r / min, and the mixture is cooled to 25°C after extrusion to obtain a bending-resistant coil core tube.

[0029] Example 2 Preparation of modified glass fiber: 7.5 g of γ-aminopropyltriethoxysilane, 25 g of deionized water and 120 g of anhydrous ethanol were mixed, stirred and hydrolyzed for 30 min to obtain a silane coupling agent solution, 50 g of glass fiber was added to the silane coupling agent solution, the temperature was raised to 80°C and allowed to stand for 8 h, then the glass fiber was taken out, and fully reacted in a vacuum drying oven at 120°C for 1 h to obtain silane-treated glass fiber, the silane-treated glass fiber was mixed with 200 g of deionized water, stirred at a speed of 100 r / min and heated to 80°C, 80 g of oleic acid was added, the temperature was maintained for reaction for 8 h, and the modified glass fiber was obtained after filtering and washing.

[0030] Preparation of glass fiber composite components: 30g of phenol, 90g of formaldehyde and 7.5g of sodium hydroxide were mixed and reacted. When the reaction temperature rose to 75°C, the system was ultrasonically treated for 3h, and then 20g of a graphite oxide solution with a mass fraction of 0.9% was added to the reaction system, and the reaction was continued at 75°C for 2h to obtain a graphene oxide-phenolic resin solution. The system was cooled to 40°C, 30g of melamine and 120g of urea were added, the temperature was raised to 55°C and the reaction was continued for 40min. After cooling to 25°C, 5wt% of ammonium sulfate was added, and a composite was obtained after stirring for 30s. 50g of modified glass fiber was added to the composite and allowed to stand for 12h. The glass fiber composite component was obtained after filtering.

[0031] Preparation of epoxidized soybean oil enhanced system: After mixing 5 g of sebacic acid, 40 g of epoxidized soybean oil and 0.2 g of catalyst 4-dimethylaminopyridine, 1.8 g of acetylglycine was added, the temperature was raised to 160° C. in an oil bath, and then the reaction was carried out with magnetic stirring for 40 min under nitrogen protection to obtain an epoxidized soybean oil enhanced system.

[0032] Preparation of bend-resistant coiled core tube: 130g of polylactic acid and 28g of epoxy soybean oil reinforcement system are vulcanized at a speed of 80r / min for 12min at 180°C to obtain a mixture; the above-prepared mixture, 66g of silica gel powder, 80g of ABS plastic, 800g of thermoplastic resin, 50g of glass fiber composite component and 20g of weathering agent are mixed, the temperature is raised to 80°C, and stirred at a speed of 800r / min for 10min to obtain a mixture; the mixture is added to a twin-screw extruder, the temperature of each zone is set at 270°C, the head temperature is 240°C, the twin-screw speed is 280r / min, the feeding speed is 40r / min, and the mixture is cooled to 25°C after extrusion to obtain a bending-resistant coiled core tube.

[0033] Example 3 Preparation of modified glass fiber: 7.5 g of γ-aminopropyltriethoxysilane, 25 g of deionized water and 120 g of anhydrous ethanol were mixed, stirred and hydrolyzed for 30 minutes to obtain a silane coupling agent solution, 50 g of glass fiber was added to the silane coupling agent solution, the temperature was raised to 80°C and allowed to stand for 8 hours, and then the glass fiber was taken out and fully reacted in a vacuum drying oven at 120°C for 1 hour to obtain silane-treated glass fiber, the silane-treated glass fiber was mixed with 200 g of deionized water, stirred at a speed of 100 r / min and heated to 80°C, 75 g of oleic acid was added, the temperature was maintained for reaction for 8 hours, and the modified glass fiber was obtained after filtering and washing.

[0034] Preparation of glass fiber composite components: 30g of phenol, 90g of formaldehyde and 7.5g of sodium hydroxide were mixed for reaction. When the reaction temperature rose to 75°C, the system was ultrasonically treated for 3h, and then 20g of a graphite oxide solution with a mass fraction of 0.8% was added to the reaction system, and the reaction was continued at 75°C for 2h to obtain a graphene oxide-phenolic resin solution. The system was cooled to 40°C, 30g of melamine and 120g of urea were added, the temperature was raised to 55°C and the reaction was continued for 40min. After cooling to 25°C, 5wt% of ammonium sulfate was added, and a composite was obtained after stirring for 30s. 50g of modified glass fiber was added to the composite and allowed to stand for 12h. The glass fiber composite component was obtained after filtering.

[0035] Preparation of epoxidized soybean oil enhanced system: After mixing 5 g of sebacic acid, 40 g of epoxidized soybean oil and 0.2 g of catalyst 4-dimethylaminopyridine, 1.6 g of acetylglycine was added, the temperature was raised to 160° C. in an oil bath, and then the reaction was carried out with magnetic stirring for 40 min under nitrogen protection to obtain an epoxidized soybean oil enhanced system.

[0036] Preparation of bend-resistant coiled core tube: 118g of polylactic acid and 26g of epoxy soybean oil reinforcement system are vulcanized at a speed of 80r / min for 12min at 180°C to obtain a mixture; the above-prepared mixture, 55g of silica gel powder, 72g of ABS plastic, 650g of thermoplastic resin, 45g of glass fiber composite component and 18g of weathering agent are mixed, the temperature is raised to 80°C, and stirred at a speed of 800r / min for 10min to obtain a mixture; the mixture is added to a twin-screw extruder, the temperature of each zone is set at 270°C, the head temperature is 240°C, the twin-screw speed is 280r / min, the feeding speed is 40r / min, and the mixture is cooled to 25°C after extrusion to obtain a bending-resistant coiled core tube.

[0037] Example 4 Example 4 is based on Example 3. The only difference between Example 4 and Example 3 is that in Example 4, 55 g of oleic acid is added when preparing the modified glass fiber.

[0038] Example 5 Example 5 is based on Example 3. The only difference between Example 5 and Example 3 is that in Example 5, 95 g of oleic acid is added when preparing the modified glass fiber.

[0039] Example 6 Example 6 is based on Example 3. The only difference between Example 6 and Example 3 is that in Example 6, a graphene oxide solution with a mass fraction of 0.4% is added when preparing the glass fiber composite component.

[0040] Example 7 Example 7 is based on Example 3. The only difference between Example 7 and Example 3 is that in Example 7, a graphene oxide solution with a mass fraction of 1.2% is added when preparing the glass fiber composite component.

[0041] Example 8 Example 8 is based on Example 3. The only difference between Example 8 and Example 3 is that in Example 8, 1 g of acetylglycine is added when preparing the epoxy soybean oil enhancement system.

[0042] Example 9 Example 9 is based on Example 3. The only difference between Example 9 and Example 3 is that in Example 9, 2.2 g of acetylglycine is added when preparing the epoxy soybean oil enhancement system.

[0043] Example 10 Example 10 is based on Example 3. The only difference between Example 10 and Example 3 is that in Example 10, the epoxy soybean oil enhancement system is replaced with ordinary epoxy soybean oil.

[0044] Embodiment 11 Example 11 is based on Example 3. The only difference between Example 11 and Example 3 is that in Example 11, when preparing the modified glass fiber, γ-aminopropyltriethoxysilane is not used to treat the glass fiber.

[0045] Example 12 Example 12 is based on Example 3. The only difference between Example 12 and Example 3 is that in Example 12, oleic acid is not used to treat the glass fiber when preparing the modified glass fiber.

[0046] Comparative Example 1 Comparative Example 1 is based on Example 3. The only difference between Comparative Example 1 and Example 3 is that in Comparative Example 1, no graphene oxide solution is added when preparing the glass fiber composite component.

[0047] Comparative Example 2 Comparative Example 2 is based on Example 3. The only difference between Comparative Example 2 and Example 3 is that in Comparative Example 2, the glass fiber composite component added to the system is replaced with an equal amount of ordinary glass fiber.

[0048] Comparative Example 3 Comparative Example 3 is based on Example 3. The only difference between Comparative Example 3 and Example 3 is that in Comparative Example 3, the epoxidized soybean oil added to the system is replaced by an equal amount of thermoplastic resin.

[0049] Comparative Example 4 Comparative Example 4 is based on Example 3. The only difference between Comparative Example 4 and Example 3 is that in Comparative Example 4, the weathering agent added to the system is replaced by an equal amount of thermoplastic resin.

[0050] Performance testing The samples of Examples 1-12 and Comparative Examples 1-4 were sampled and the following performance tests were performed: (1) Impact resistance test Based on GBT1043.1-2008 as the testing standard, the impact strength performance test was carried out on the samples. Each sample was tested three times, the average value was taken, and the test results were filled in Table 1.

[0051] (2) Tensile performance test Taking "GBT1040.1-2006 Determination of Tensile Properties of Plastics" as the test standard, the tensile properties of the samples were tested. Each sample was tested three times, the average value was taken, and the test results were filled in Table 1; the test environment was heated to 80℃ and the temperature was maintained for 30 minutes. The tensile properties of the samples were tested. Each test was tested three times, the average value was taken, and the test results were filled in Table 1.

[0052] Table 1 Performance test results of Examples 1-12 and Comparative Examples 1-4 It can be seen from Table 1 that the impact strength of Examples 1-3 is only 15.5 KJ / m 2 And above, it shows that the roll core tube prepared by the present application has good impact resistance, the tensile strength of Examples 1-3 is 88.0MPa and above, which shows that the roll core tube prepared by the present application has good tensile resistance, and at 80°C, the tensile strength change rate of Examples 1-3 is less than 4%, which shows that the present application has good temperature resistance.

[0053] In Example 4 and Example 5, when preparing modified glass fibers, the mass ratios of the silane coupling agent, the glass fiber and oleic acid are not within the range specified in the present application. When the oleic acid content is too little, the coating effect on the surface of the glass fiber is reduced, resulting in a decrease in the content of functional groups on the surface of the glass fiber, and a decrease in the subsequent connection performance with the phenolic resin and graphene. At the same time, the dispersion performance of the glass fiber in the system is reduced. When the oleic acid content is too high, the overall stability of the glass fiber is affected, thereby reducing the overall performance of the glass fiber. Therefore, the various performances of Example 4 and Example 5 are reduced.

[0054] When preparing the glass fiber composite components in Examples 6 and 7, the concentrations of the added graphene oxide solution are not within the range specified in the present application. When the concentration of graphene oxide is too low, it is difficult to form a continuous nano-network structure, and it is difficult to improve the thermal stability of the system, and it is difficult to significantly improve the mechanical properties of the system. When the concentration of graphene oxide is too high, graphene oxide will agglomerate in the system, thereby affecting the stability of the system. Therefore, the performance of Examples 6 and 7 are all reduced.

[0055] In Example 8 and Example 9, when preparing the epoxy soybean oil enhanced system, the mass ratio between the epoxy soybean oil and acetylglycine is not within the range specified in the present application. When the content of acetylglycine is too little, the ductility improvement between the epoxy soybean oil and polylactic acid is reduced, so it is difficult to further improve the comprehensive performance of the system. When the content of acetylglycine is too much, the carboxyl group of acetylglycine competes with the ring-opening reaction between sebacic acid and the epoxy soybean oil, thereby affecting the crosslinking degree of the system and thus affecting the strength of the system.

[0056] In Example 10, the epoxy soybean oil enhancement system is replaced with ordinary epoxy soybean oil. Ordinary epoxy soybean does not introduce acetylglycine and is difficult to form hydrogen bonds. Therefore, the bonding effect between the systems is difficult to improve, so the performance of Example 10 is reduced.

[0057] In Example 11, γ-aminopropyltriethoxysilane was not used to treat the glass fiber, and in Example 12, oleic acid was not used to treat the glass fiber. It is difficult to increase the group content on the surface of the glass fiber through a single modification, and it is difficult to further enhance the compatibility improvement effect in the system. Therefore, the performance of Examples 11 and 12 are reduced.

[0058] In Comparative Example 1, no graphene oxide solution was added. It is difficult to further improve the thermal stability of the system without adding the graphene oxide solution, and it is difficult to further improve the high temperature resistance of the system, and it is difficult to form a stable network structure, and it is difficult to improve the overall mechanical properties.

[0059] In Comparative Example 2, the glass fiber composite component is replaced with an equal amount of ordinary glass fiber. Ordinary glass fiber is difficult to further improve the connection performance between the components in the system, so the overall mechanical properties of the system are reduced. The lack of graphene oxide in the system is also difficult to promote the improvement of thermal stability.

[0060] In Comparative Example 3, the epoxy soybean oil reinforcement system was not added, the compatibility of the system was reduced, and there was no further cross-linking effect with polylactic acid, which would also affect the overall thermal stability.

[0061] In Comparative Example 4, no weathering agent was added, which reduced the system's adaptability to temperature changes, so the tensile strength changed significantly after the temperature rose.

[0062] This specific embodiment is only an explanation of the present application, and it is not a limitation of the present application. Through the above description, relevant staff can make various changes and modifications without deviating from the technical idea of ​​the present application. The technical scope of the present application is not limited to the content in the specification, and its technical scope must be determined according to the scope of the claims.

Claims

1. A bending-resistant coiled core tube, characterized in that: The composition comprises the following components in parts by weight: Polypropylene 64-80 parts, silica gel powder 48-66 parts, ABS plastic 64-80 parts, thermoplastic resin 440-700 parts, polylactic acid 104-130 parts, glass fiber composite component 40-50 parts, epoxy soybean oil reinforcement system 24-28 parts, weathering agent 16-20 parts; The glass fiber composite component comprises modified glass fiber, phenolic resin and graphene oxide.

2. The bending-resistant rolled core tube according to claim 1, characterized in that: The modified glass fiber is prepared by the following method: A silane coupling agent, deionized water and anhydrous ethanol are mixed and stirred to obtain a silane coupling agent solution, glass fiber is added to the silane coupling agent solution, the temperature is increased and allowed to stand, and then the glass fiber is taken out and heated to react to obtain a silane-treated glass fiber, the silane-treated glass fiber is mixed with deionized water, stirred and oleic acid is added to react, and the modified glass fiber is obtained after filtering and washing.

3. The bending-resistant rolled core tube according to claim 1, characterized in that: The mass ratio of the glass fiber, the silane coupling agent and the oleic acid is 1:0.15:(1.4-1.6).

4. The bending-resistant rolled core tube according to claim 1, characterized in that: The glass fiber composite component is prepared by the following method: Phenol, formaldehyde and sodium hydroxide are mixed and reacted, ultrasonically treated, and then the graphene oxide aqueous solution is added to the reaction system, and the reaction is continued to obtain a graphene oxide-phenolic resin solution. After the system is cooled, melamine and urea are added, and the temperature is increased to continue the reaction. After the reaction, ammonium sulfate is added after cooling, and a composite is obtained after stirring. The modified glass fiber is added to the composite and allowed to stand, and a glass fiber composite component is obtained after filtering.

5. The bending-resistant rolled core tube according to claim 1, characterized in that: The mass fraction of graphene oxide in the graphene oxide aqueous solution is 0.7-0.9%.

6. The bending-resistant rolled core tube according to claim 1, characterized in that: The raw materials of the epoxy soybean oil enhancement system include epoxy soybean oil, acetylglycine and sebacic acid.

7. The bending-resistant rolled core tube according to claim 1, characterized in that: The epoxidized soybean oil enhanced system is prepared by the following method: After mixing sebacic acid, epoxidized soybean oil and a catalyst, acetylglycine is added, and the mixture is reacted after heating in an oil bath to obtain an epoxidized soybean oil enhanced system.

8. The bending-resistant rolled core tube according to claim 1, characterized in that: The mass ratio between the epoxidized soybean oil and acetylglycine is 1:(0.035-0.045).

9. The bending-resistant rolled core tube according to claim 1, characterized in that: The catalyst is 4-dimethylaminopyridine.

10. A method for preparing the bending-resistant rolled core tube according to claim 1, characterized in that: The steps include: Polylactic acid and an epoxy soybean oil reinforcing system are vulcanized to obtain a mixture, the mixture, polypropylene, silica gel powder, ABS plastic, thermoplastic resin, modified glass fiber and a weathering agent are mixed, the mixture is heated and stirred to obtain a mixed material, the mixed material is added to a twin-screw extruder, and the mixture is cooled after extrusion to obtain a bending-resistant coiled core tube.

Citation Information

Cited By

  • Preparation method of anti-cracking high-temperature-resistant cable material