High-temperature-resistant and high-cold-resistant polyvinyl chloride cable material and preparation method thereof
By adding cold-resistant and high-temperature-resistant plasticizers and modified toughener to the PVC cable material, and using segmented stirring and two-step extrusion process, the insufficient performance of PVC cable material at extreme temperatures is solved, and the performance of PVC cable material is achieved. The preparation of high temperature and high cold resistance polyvinyl chloride cable materials meets the aging conditions of -60℃ and 135℃ and high temperature, ensuring the stability and safety of the cable.
Patent Information
- Application Number
- CN202411321914.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-23
- Publication Date
- 2024-11-08
AI Technical Summary
The existing PVC cable materials cannot take into account the conditions of low temperature embrittlement in -60℃ and aging of 135℃*240h, and the production and processing are difficult, resulting in poor performance in extreme temperature environments and safety hazards.
Adopt high temperature and high cold resistance polyvinyl chloride cable material formula, including 100 parts of PVC resin powder, 90-95 parts of plasticizer, 8 parts of heat stabilizer, 5-7 parts of filler, 0.2-0.4 parts of lubricant, 10-15 Parts of modified toughening agent, 1-2 parts of antioxidant and 10-15 parts of chlorinated polyethylene, and are subjected to segmented stirring and two-step extrusion process to ensure uniform dispersion and stability of the material.
It achieves good performance at low temperatures of -60℃ and high temperatures of 135℃, excellent physical and mechanical properties, strong weather resistance, and small aging rate of change, and is suitable for use in high-temperature and high-cold environments.
Smart Images

Figure BDA0005054223790000061
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of electric wires and cables, and relates to a polyvinyl chloride cable material and a preparation method thereof, and in particular to a high-temperature-resistant and high-cold-resistant polyvinyl chloride cable material and a preparation method thereof, which adjusts the low-temperature brittle temperature to below -60°C while ensuring that the PVC cable material meets basic performance, thereby preparing a high-temperature-resistant and high-cold-resistant polyvinyl chloride cable material with excellent physical and mechanical properties and good extrusion process, and meeting the production requirements of high-temperature-resistant and low-temperature-resistant cables. Background Art
[0002] With the rapid development of economy, wires and cables are widely used in various industries and fields. Polyvinyl chloride (PVC) cable materials are cheap and have excellent performance. They have long occupied an important position in the insulation and protection materials of wires and cables. However, ordinary polyvinyl chloride plastics cannot support their use in special environments.
[0003] At present, the low-temperature brittle temperature of most PVC cable materials is between -15℃ and -20℃, and the low-temperature brittle temperature of some cold-resistant PVC cable materials can reach -40℃. However, in some high-latitude areas, such as Northeast my country, Xinjiang and other places in Russia and Northern Europe, the winter temperature is generally below -55℃. Wires and cables made of ordinary PVC cable materials or low-cold-resistant PVC cable materials are very easy to be damaged. Moreover, this kind of PVC cable material has poor high temperature resistance and is easy to age under the influence of light and heat for a long time, which poses a safety hazard and leads to unnecessary economic losses. Summary of the invention
[0004] The technical problems to be solved by the present invention include that the PVC cable material of the prior art cannot take into account both -60°C low-temperature catalysis and 135°C*240h aging at the same time, and is difficult to produce and process. Therefore, the present invention provides a high-temperature-resistant and high-cold-resistant PVC cable material and a preparation method thereof. The high-temperature-resistant and high-cold-resistant PVC cable material of the present invention meets the -60°C low-temperature catalysis temperature while ensuring that the PVC cable material meets the basic performance and has the 135°C aging condition, has excellent physical and mechanical properties, and has a good extrusion process.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] The invention firstly provides a high-temperature-resistant and high-cold-resistant polyvinyl chloride cable material, which comprises the following raw materials in parts by weight: 100 parts of PVC resin powder, 90-95 parts of plasticizer, 8 parts of heat stabilizer, 5-7 parts of filler, 0.2-0.4 parts of lubricant, 10-15 parts of modified toughening agent, 1-2 parts of antioxidant and 10-15 parts of chlorinated polyethylene.
[0007] As a preferred embodiment of the present invention, the average polymerization degree of the PVC resin powder is 2500-3000.
[0008] As a preferred embodiment of the present invention, the plasticizer is a composition of trioctyl trimellitate, dioctyl adipate and / or triisononyl trimellitate.
[0009] As a preferred embodiment of the present invention, the heat stabilizer is a calcium zinc stabilizer.
[0010] As a preferred embodiment of the present invention, the filler includes one or more combinations of calcium carbonate, silicon dioxide, carbon black, talc, kaolin or montmorillonite.
[0011] As a preferred embodiment of the present invention, the modified toughening agent includes nitrile rubber or ethylene-acrylic acid-ethyl ester copolymer.
[0012] As a preferred embodiment of the present invention, the antioxidant is one of pentaerythritol tetrakis-(dibutyl hydroxyhydrocinnamate) and / or dilauryl thiodipropionate.
[0013] As a preferred embodiment of the present invention, the chlorine content of the chlorinated polyethylene is 30-40%.
[0014] The present invention also provides a method for preparing the above-mentioned high-temperature-resistant and high-cold-resistant polyvinyl chloride cable material, the preparation method comprising the following steps:
[0015] 1) Put PVC resin powder, heat stabilizer, filler, lubricant and antioxidant powder into a high-mixing pot, set the high-mixing temperature, put part of the plasticizer into the pot for the first time at a low speed of the main engine, increase the main engine speed, wait for the PVC resin powder to completely absorb the plasticizer, put part of the plasticizer into the pot for the second time, wait for the PVC resin powder to completely absorb the plasticizer, put the remaining plasticizer into the pot for the third time, wait for the PVC resin powder to completely absorb the plasticizer, and after the high-mixing temperature reaches the set temperature, add the modified toughening agent and chlorinated polyethylene and continue stirring to obtain a mixture;
[0016] 2) adding the mixed material into a twin-screw extruder for extrusion granulation to obtain the high-temperature-resistant and high-cold-resistant PVC cable material.
[0017] As a preferred embodiment of the present invention, in step 1), the amount of plasticizer added each time is 1 / 3 of the total amount;
[0018] In step 2), the extruder is a counter-rotating twin-screw extruder connected to a single screw extruder, and the temperatures of the counter-rotating twin-screw extruders are set to 125°C, 130°C, 145°C, 150°C, 155°C, 160°C, 160°C, 160°C, 155°C and 150°C, respectively, and the temperature of the single screw extruder is set to 120°C; the feeding rate is 20-30rpm, and the extruder speed is 400-500rpm.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] 1) The high-temperature-resistant and high-cold-resistant PVC cable material of the present invention has good physical and mechanical properties, meets the -60°C low-temperature embrittlement impact and 135°C*240h aging, and has a small aging change rate.
[0021] 2) The high-temperature-resistant and high-cold-resistant PVC cable material of the present invention has strong weather resistance and the plasticizer is not easy to precipitate.
[0022] 3) The preparation method of the present invention adopts segmented stirring, which can make the resin powder absorb the plasticizer better and ensure the uniform dispersion of the raw materials, and maintain good mechanical properties; the two-step extrusion can ensure the stability of the cable material. DETAILED DESCRIPTION
[0023] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0024] The invention firstly provides a high-temperature-resistant and high-cold-resistant polyvinyl chloride cable material, which comprises the following raw materials in parts by weight: 100 parts of PVC resin powder, 90-95 parts of plasticizer, 8 parts of heat stabilizer, 5-7 parts of filler, 0.2-0.4 parts of lubricant, 10-15 parts of modified toughening agent, 1-2 parts of antioxidant and 10-15 parts of chlorinated polyethylene.
[0025] Preferably, the average polymerization degree of the PVC resin powder is 2500-3000.
[0026] As a specific embodiment of the present invention, PVC resin powder is purchased from Formosa Plastics Corporation, model S-85, with an average degree of polymerization of 2500-3000.
[0027] Preferably, the plasticizer is a combination of trioctyl trimellitate and dioctyl adipate and / or triisononyl trimellitate.
[0028] In the present invention, considering aging at 135°C*240h, the present invention selects a benzene plasticizer, which has excellent high temperature resistance and aging resistance, can maintain the stability and durability of the material in a high temperature environment, can maintain the long life of the cable, and is commonly used for aging at 135°C; considering the low temperature brittle temperature of -60°C, a cold-resistant plasticizer and a cold-resistant modified toughening agent are added to the formula of the present invention.
[0029] Preferably, the heat stabilizer is a calcium zinc stabilizer.
[0030] As a specific embodiment of the present invention, the model of the calcium zinc stabilizer is German Bear Brand 92179 PVC heat stabilizer.
[0031] Preferably, the filler comprises one or more combinations of calcium carbonate, silicon dioxide, carbon black, talc, kaolin or montmorillonite.
[0032] As a specific embodiment of the present invention, the filler is calcium carbonate, with a D100 particle size of less than or equal to 10 μm and a whiteness of ≥93.
[0033] Preferably, the modified toughening agent comprises nitrile rubber or ethylene-acrylic acid-ethyl ester copolymer.
[0034] In the present invention, the molecular chain of nitrile rubber itself is soft and has good compatibility with PVC. It can be filled into the molecular gaps of PVC to form a network in the PVC matrix to modify the low-temperature impact resistance of the material. The EMA toughening agent of the American company DuPont can also be used as a non-migrating plasticizer for the material to significantly improve the low-temperature impact resistance of the material.
[0035] As a specific embodiment of the present invention, the modified toughening agent is nitrile rubber.
[0036] As another specific embodiment of the present invention, the modified toughening agent is ethylene-acrylic acid-ethyl ester copolymer (EMA modified toughening agent) produced by DuPont Company of the United States.
[0037] Preferably, the antioxidant is one of pentaerythritol tetrakis-(dibutylhydroxyhydrocinnamate) and / or dilauryl thiodipropionate.
[0038] Preferably, the chlorine content of the chlorinated polyethylene is 30-40%.
[0039] The present invention also provides a method for preparing the above-mentioned high-temperature-resistant and high-cold-resistant polyvinyl chloride cable material, the preparation method comprising the following steps:
[0040] 1) Put PVC resin powder, heat stabilizer, filler, lubricant and antioxidant powder into a high-mixing pot, set the high-mixing temperature, put part of the plasticizer into the pot for the first time at a low speed of the main engine, increase the main engine speed, wait for the PVC resin powder to completely absorb the plasticizer, put part of the plasticizer into the pot for the second time, wait for the PVC resin powder to completely absorb the plasticizer, put the remaining plasticizer into the pot for the third time, wait for the PVC resin powder to completely absorb the plasticizer, and after the high-mixing temperature reaches the set temperature, add the modified toughening agent and chlorinated polyethylene and continue stirring to obtain a mixture;
[0041] 2) adding the mixed material into a twin-screw extruder for extrusion granulation to obtain the high-temperature-resistant and high-cold-resistant PVC cable material.
[0042] Preferably, in step 1), the amount of plasticizer added each time is 1 / 3 of the total amount;
[0043] In step 2), the extruder is a counter-rotating twin-screw extruder connected to a single screw extruder, and the temperatures of the counter-rotating twin-screw extruders are set to 125°C, 130°C, 145°C, 150°C, 155°C, 160°C, 160°C, 160°C, 155°C and 150°C, respectively, and the temperature of the single screw extruder is set to 120°C; the feeding rate is 20-30rpm, and the extruder speed is 400-500rpm.
[0044] In the present invention, the cold-resistant and high-temperature resistant plasticizer and the cold-resistant modified toughening agent are used to modify the PVC resin, so that the PVC resin has high heat resistance and high cold resistance and the mechanical properties of the material are stable.
[0045] The present invention takes aging at 135°C*240h into consideration and selects a benzene plasticizer. However, since the PVC resin powder has poor absorption of the benzene plasticizer and the content of the plasticizer added in the present invention is relatively high, the present invention adopts multiple small additions of the plasticizer and adopts segmented stirring, which can make the resin powder absorb the plasticizer better and ensure the uniform dispersion of the raw materials to maintain good mechanical properties; the two-step extrusion can better ensure the stability of the cable material.
[0046] The antioxidant and calcium zinc stabilizer in the present invention can delay the aging of the polymer and increase the service life of the cable material.
[0047] Example 1
[0048] The present embodiment provides a method for preparing a high-temperature-resistant and high-cold-resistant PVC cable material. The raw materials for the preparation include, by weight, 100 parts of PVC resin powder, 90 parts of plasticizer, 8 parts of heat stabilizer, 7 parts of filler, 0.3 parts of lubricant, 15 parts of modified toughening agent, 1 part of antioxidant, and 10 parts of chlorinated polyethylene.
[0049] The PVC resin powder was purchased from Formosa Plastics Corporation, model S-85, with an average degree of polymerization of 2500.
[0050] The plasticizers are 40 parts of trioctyl trimellitate (TOTM), 40 parts of triisononyl trimellitate (UN399), and 10 parts of dioctyl adipate (DOS), all of which are commercially available.
[0051] The heat stabilizer is Xiong brand 92179 calcium zinc stabilizer.
[0052] The lubricant is commercially available PE wax.
[0053] The filler is calcium carbonate, with a D100 particle size of less than or equal to 10 μm and a whiteness of ≥93.
[0054] The modified toughening agent is nitrile rubber.
[0055] The antioxidant is one of pentaerythritol tetrakis-(dibutylhydroxyhydrocinnamate) and / or dilauryl thiodipropionate, which are commercially available.
[0056] Put PVC resin powder, heat stabilizer, filler, lubricant and antioxidant powder into a high-mixing pot, set the high-mixing temperature to 135°C, put 30 parts of plasticizer into the pot for the first time at a low speed of 8 revolutions, increase the main engine speed to 35 revolutions, wait until the PVC resin powder completely absorbs the plasticizer, put 30 parts of plasticizer into the pot for the second time, wait until the PVC resin powder almost absorbs the plasticizer, put 30 parts of plasticizer into the pot for the third time, wait until the PVC resin powder absorbs the plasticizer, and when the high-mixing temperature reaches the set temperature, add the modified toughening agent and chlorinated polyethylene and continue stirring for 1 minute to obtain a mixture;
[0057] The mixed powder is fed into a counter-rotating twin-screw extruder connected to a single-screw extruder, the feeding speed is 30 rpm, the temperature of the counter-rotating twin-screw extruder is set to 125°C, 130°C, 145°C, 150°C, 155°C, 160°C, 160°C, 160°C, 155°C and 150°C, the temperature of the single-screw extruder is set to 120°C; the feeding speed is 20-30 rpm, and the extruder speed is 425 rpm. After extrusion granulation, cutting and cooling are performed to obtain the high-temperature-resistant and high-cold-resistant PVC cable material.
[0058] Example 2
[0059] The present embodiment provides a method for preparing a high-temperature-resistant and high-cold-resistant PVC cable material. The raw materials for the preparation include, by weight, 100 parts of PVC resin powder, 95 parts of plasticizer, 8 parts of heat stabilizer, 5 parts of filler, 0.3 parts of lubricant, 10 parts of modified toughening agent, 1 part of antioxidant, and 8 parts of chlorinated polyethylene.
[0060] The PVC resin powder was purchased from Formosa Plastics Corporation, model S-85, with an average degree of polymerization of 2500.
[0061] The plasticizers are 75 parts of trioctyl trimellitate (TOTM) and 20 parts of dioctyl adipate (DOS), both of which are commercially available.
[0062] The heat stabilizer is Xiong brand 92179 calcium zinc stabilizer.
[0063] The filler is calcium carbonate, with a D100 particle size of less than or equal to 10 μm and a whiteness of ≥93.
[0064] The lubricant is commercially available PE wax.
[0065] The modified toughening agent is ethylene-acrylic acid-ethyl ester copolymer (EMA modified toughening agent) produced by DuPont Company of the United States.
[0066] The antioxidant is one of pentaerythritol tetrakis-(dibutylhydroxyhydrocinnamate) and / or dilauryl thiodipropionate, which are commercially available.
[0067] Put PVC resin powder, heat stabilizer, inorganic filler, lubricant and antioxidant powder into a high-mixing pot, set the high-mixing temperature to 135°C, put 30 parts of plasticizer into the pot for the first time at a low speed of 8 revolutions, increase the main engine speed to 35 revolutions, wait until the PVC resin powder completely absorbs the plasticizer, put 30 parts of plasticizer into the pot for the second time, wait until the PVC resin powder almost absorbs the plasticizer, put 30 parts of plasticizer into the pot for the third time, wait until the PVC resin powder absorbs the plasticizer, and when the high-mixing temperature reaches the set temperature, add the modified toughening agent and chlorinated polyethylene and continue stirring for 1 minute to obtain a mixture;
[0068] The mixed powder is fed into a counter-rotating twin-screw extruder connected to a single-screw extruder, the feeding speed is 30 rpm, the temperature of the counter-rotating twin-screw extruder is set to 125°C, 130°C, 145°C, 150°C, 155°C, 160°C, 160°C, 160°C, 155°C and 150°C, the temperature of the single-screw extruder is set to 120°C; the feeding speed is 20-30 rpm, and the extruder speed is 425 rpm. After extrusion granulation, cutting and cooling are performed to obtain the high-temperature-resistant and high-cold-resistant PVC cable material.
[0069] Comparative Example 1
[0070] The difference between this comparative example and Example 1 is that the heat stabilizer is German Bear Brand 90224 PVC heat stabilizer. The preparation method of PVC cable material is the same as that of Example 1.
[0071] Comparative Example 2
[0072] The difference between this comparative example and Example 2 is that the heat stabilizer is German Bear Brand 90224 PVC heat stabilizer. The preparation method of PVC cable material is the same as that of Example 2.
[0073] Comparative Example 3
[0074] The difference between this comparative example and Example 2 is that the plasticizer is 55 parts of trioctyl trimellitate, 20 parts of didecyl phthalate, and 20 parts of dioctyl adipate. The preparation method of the cable material is the same as that of Example 2.
[0075] Comparative Example 4
[0076] Compared with Example 2, the difference between this comparative example and Example 2 is that the preparation method is to put PVC resin powder, heat stabilizer, inorganic filler, lubricant, antioxidant, modified toughening agent, and chlorinated polyethylene powder into a high-mixing pot, set the high-mixing temperature to 135°C, add the plasticizer at one time at a low speed of 5 revolutions of the main engine, and obtain a mixture after the high-mixing temperature reaches the set temperature.
[0077] This preparation method adds plasticizer at one time, which results in the resin powder not being able to fully absorb the plasticizer. Adding modified toughening agent and chlorinated polyethylene too early causes the powder to gel, making production and processing difficult, thus limiting its practical application in production.
[0078] The high-temperature-resistant and high-cold-resistant PVC cable materials obtained in Example 1 and Example 2 and the cable materials obtained in Comparative Examples 1 to 4 were subjected to physical property tests, 135°C*240h aging tests, and low-temperature catalytic temperature tests. The results are shown in Table 1.
[0079] Table 1. Test results
[0080]
[0081] Referring to Table 1, Example 1 has serious oil leakage compared with Example 2. 40 parts of UN399 are added to the formula of Example 1. The large amount of plasticizer added and the large amount of plasticizer contained in the formula system are not suitable for excessive addition to the soft material, resulting in serious oil leakage of the material, affecting the operation and use of the cable.
[0082] Compared with Examples 1 and 2, the heat stabilizer in the formula of Comparative Examples 1 and 2 is replaced by Xiong brand 90224 calcium zinc stabilizer instead of Xiong brand 92179 calcium zinc stabilizer. In the thermal aging at 135°C*240h, the effect of 90224 is lower than that of Xiong brand 92179, and the aging change rate of the cable material is greater than ±20%.
[0083] In Comparative Example 3, compared with Example 2, 75 parts of TOTM are replaced by 55 parts of trioctyl trimellitate + 22 parts and 20 parts of didecyl phthalate. Under the thermal aging condition of 135°C*240h, the migration resistance and aging resistance of didecyl phthalate are not as good as those of trioctyl trimellitate.
[0084] Therefore, the high-temperature-resistant and high-cold-resistant PVC cable material provided in Example 2 of the present invention has good aging resistance, excellent mechanical properties, a low-temperature brittle temperature that can meet -60°C, and excellent cold resistance, which can meet production, processing and market needs.
[0085] The above is only a preferred embodiment of the present invention, and is not any formal or substantial limitation of the present invention. It should be pointed out that ordinary technicians in this technical field can make several improvements and supplements without departing from the method of the present invention, and these improvements and supplements should also be regarded as the protection scope of the present invention. Any technician familiar with this profession, without departing from the spirit and scope of the present invention, can make some changes, modifications and evolutions of the technical content disclosed above, which are equivalent embodiments of the present invention; at the same time, any changes, modifications and evolutions of any equivalent changes made to the above embodiments based on the essential technology of the present invention are still within the scope of the technical solution of the present invention.
Claims
1. A high temperature and cold resistance polyvinyl chloride cable material, characterized in that: The high-temperature-resistant and high-cold-resistant polyvinyl chloride cable material comprises the following raw materials in parts by weight: 100 parts of PVC resin powder, 90-95 parts of plasticizer, 8 parts of heat stabilizer, 5-7 parts of filler, 0.2-0.4 parts of lubricant, 10-15 parts of modified toughening agent, 1-2 parts of antioxidant and 10-15 parts of chlorinated polyethylene.
2. The high temperature and cold resistance polyvinyl chloride cable material according to claim 1, characterized in that: The average polymerization degree of the PVC resin powder is 2500-3000.
3. The high temperature and cold resistance polyvinyl chloride cable material according to claim 1, characterized in that: The plasticizer is a composition of trioctyl trimellitate, dioctyl adipate and / or triisononyl trimellitate.
4. The high temperature and cold resistance polyvinyl chloride cable material according to claim 1, characterized in that: The heat stabilizer is a calcium zinc stabilizer.
5. The high temperature and cold resistance polyvinyl chloride cable material according to claim 1, characterized in that: The filler includes one or more combinations of calcium carbonate, silicon dioxide, carbon black, talc, kaolin or montmorillonite.
6. The high-temperature-resistant and high-cold-resistant polyvinyl chloride cable material according to claim 1, characterized in that: The modified toughening agent includes nitrile rubber or ethylene-acrylic acid-ethyl ester copolymer.
7. The high temperature and cold resistance polyvinyl chloride cable material according to claim 1, characterized in that: The antioxidant is one of tetrakis-(dibutyl hydroxyhydrocinnamic acid) pentaerythritol ester and / or dilauryl thiodipropionate.
8. The high-temperature-resistant and high-cold-resistant polyvinyl chloride cable material according to claim 1, characterized in that: The chlorine content of the chlorinated polyethylene is 30-40%.
9. A method for preparing a high-temperature-resistant and high-cold-resistant polyvinyl chloride cable material according to any one of claims 1 to 8, characterized in that: The preparation method comprises the following steps: 1) Put PVC resin powder, heat stabilizer, filler, lubricant and antioxidant powder into a high-mixing pot, set the high-mixing temperature, put part of the plasticizer into the pot for the first time at a low speed of the main engine, increase the main engine speed, wait for the PVC resin powder to completely absorb the plasticizer, put part of the plasticizer into the pot for the second time, wait for the PVC resin powder to completely absorb the plasticizer, put the remaining plasticizer into the pot for the third time, wait for the PVC resin powder to completely absorb the plasticizer, and after the high-mixing temperature reaches the set temperature, add the modified toughening agent and chlorinated polyethylene and continue stirring to obtain a mixture; 2) adding the mixed material into a twin-screw extruder for extrusion granulation to obtain the high-temperature-resistant and high-cold-resistant PVC cable material.
10. The method for preparing the high-temperature-resistant and high-cold-resistant polyvinyl chloride cable material according to claim 9, characterized in that: In step 1), the amount of plasticizer added each time is 1 / 3 of the total amount; In step 2), the extruder is a counter-rotating twin-screw extruder connected to a single screw extruder, and the temperatures of the counter-rotating twin-screw extruders are set to 125°C, 130°C, 145°C, 150°C, 155°C, 160°C, 160°C, 160°C, 155°C and 150°C, respectively, and the temperature of the single screw extruder is set to 120°C; the feeding rate is 20-30rpm, and the extruder speed is 400-500rpm.
Citation Information
Cited By
Cold-resistant insulated cable material and production equipment and method thereof
CN120363435A
Low-temperature-resistant cable material and preparation method thereof
CN120757940A