High-transparency fluorine film and preparation method thereof
By using nano barium sulfate compound bentonite modified double-dispense and guiding functional agent in the fluorine film, combined with twin-screw extrusion granulation and casting method, the problem of incoordination of the existing fluorine film performance is solved, and high The coordinated improvement of transparent fluorine films in light transmission, barrier and mechanical properties has expanded its scope of application.
Patent Information
- Application Number
- CN202310499231.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-06
- Publication Date
- 2024-11-08
AI Technical Summary
When the existing fluorine film improves light transmission and water resistance, it reduces the corrosion resistance and mechanical properties of the product, resulting in the inability to coordinate performance, limiting its scope of application.
Polyvinylidene fluoride resin and polybutyl methacrylate are used as base materials, and nano barium sulfate is added to bentonite modified double-adjustment, guiding functional agent and interface agent. Through the combination of antioxidants and compatibilizers, the interface of the product is optimized. High-transparent fluorine film is prepared by twin-screw extrusion granulation and casting method to simplify the process.
The coordinated improvement of the light transmission, water vapor barrier and mechanical properties of the high-transparent fluorine film are achieved, which simplifies the process and improves the overall performance stability and scope of application of the product.
Smart Images

Figure BDA0004213157920000131 
Figure BDA0004213157920000141 
Figure BDA0004213157920000151
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of fluorine films, and in particular to a highly transparent fluorine film and a preparation method thereof. Background Art
[0002] Fluorine film has excellent advantages such as weather resistance, stain resistance, chemical corrosion resistance, and high temperature resistance. It is widely used in semiconductor packaging and testing, photovoltaic composites, carbon fiber composite molding, pharmaceutical packaging, LED packaging and other fields.
[0003] Fluorine film is made of fluororesin through ingredients and processes. The fluorine film used in conjunction with photovoltaic cell modules needs to have high performance requirements of light transmittance and water resistance. In order to improve the light transmittance and water resistance in the prior art, the corrosion resistance and mechanical properties of the product are reduced, resulting in uncoordinated product performance. Based on this, the present invention coordinates and improves the performance of the product and increases the scope of application of the product. Summary of the invention
[0004] In view of the defects of the prior art, the purpose of the present invention is to provide a highly transparent fluorine film and a preparation method thereof to solve the problems raised in the above background technology.
[0005] The present invention solves the technical problem by adopting the following technical solution:
[0006] The present invention provides a highly transparent fluorine film, which comprises the following raw materials in parts by weight:
[0007] 60-70 parts of polyvinylidene fluoride resin, 20-30 parts of polybutyl methacrylate, 5-10 parts of nano-barium sulfate compounded bentonite modified double adjuster, 3-6 parts of guiding functional agent, 2-5 parts of interface agent, 1-2 parts of antioxidant, and 1-2 parts of compatibilizer.
[0008] Preferably, the highly transparent fluorine film comprises the following raw materials in parts by weight:
[0009] 65 parts of polyvinylidene fluoride resin, 25 parts of polybutyl methacrylate, 7.5 parts of nano-barium sulfate compounded bentonite modified double adjuster, 4.5 parts of guiding functional agent, 3.5 parts of interface agent, 1.5 parts of antioxidant, and 1.5 parts of compatibilizer.
[0010] Preferably, the weight average molecular weight of the polyvinylidene fluoride resin is 400,000-600,000, and the apparent density is 0.45-0.55 g / cm 2 ;
[0011] The antioxidant is 2,8-di-tert-butyl-4-methylphenol and phosphite in a weight ratio of (4-7):1; the compatibilizer is maleic anhydride grafted ethylene-propylene copolymer;
[0012] The interface agent is coupling agent KH560.
[0013] Preferably, the preparation method of the nano-barium sulfate compounded bentonite modified double adjuster is:
[0014] S11: adding tannic acid to deionized water and mixing to prepare a tannic acid solution with a mass fraction of 1-2.5%;
[0015] S12: then adding 5-10% of the total amount of the tannic acid solution to the nano-barium sulfate coordination agent, mixing evenly, to obtain a tannic acid synergistic nano-barium sulfate complexing solution;
[0016] S13: Then, the bentonite is treated with a thermal-tannic acid-synergistic nano-barium sulfate compounding solution to obtain a nano-barium sulfate-compounded bentonite modified double agent;
[0017] The specific steps of the synergistic treatment of the thermal-tannic acid-combined nano-barium sulfate compounding solution are as follows:
[0018] S102: Bentonite is first subjected to thermal reaction at 350-400°C for 5-10 minutes, then cooled to 150°C at a rate of 1-3°C / min, kept at this temperature for 10-20 minutes, and finally air-cooled to room temperature;
[0019] S112: Then add it into the tannic acid synergistic nano-barium sulfate complex solution in a weight ratio of 3:(5-9), stir and react, then wash with water and dry.
[0020] Preferably, the preparation method of the nano barium sulfate coordination and leveling agent is:
[0021] Place the nano-barium sulfate in a ball mill for ball milling modification, add 2-5% of the total amount of nano-barium sulfate in the ball milling modification liquid, wash with water, and dry after the ball milling is completed;
[0022] The ball milling modification liquid comprises the following raw materials in parts by weight: 2-5 parts of yttrium nitrate, 1-3 parts of silica sol, 5-10 parts of deionized water, 0.5-1 parts of phosphate buffer solution, and 0.2-0.5 parts of triethanolamine borate.
[0023] Preferably, the rotation speed of the ball milling modification is 1000-1500 r / min, and the ball milling time is 20-30 min.
[0024] Preferably, the pH value of the phosphate buffer solution is 4.5-5.5.
[0025] Preferably, the stirring reaction temperature of S112 is 35-40° C., the stirring time is 45-55 min, and the stirring speed is 500-1000 r / min.
[0026] Preferably, the preparation method of the targeting functional agent is:
[0027] The nanocellulose is first placed in a 3-5 times mass fraction 2-5% hydrochloric acid solution and stirred at a speed of 300-400r / min for 35-45min; then 2-5% titanate coupling agent, 1-4% octadecyltrimethylammonium chloride and 1-3% stearic acid are added to the total amount of the hydrochloric acid solution, and then stirred at a speed of 100-200r / min for 1-2h, stirred evenly, washed with water and dried to obtain a guiding functional agent.
[0028] The present invention also provides a method for preparing a highly transparent fluorine film, comprising the following steps:
[0029] Step 1: Weigh the raw materials:
[0030] Step 2: Send the nano-barium sulfate compounded with bentonite modified double adjuster, guiding functional agent, and interface agent into a mixer for stirring until the raw materials are evenly mixed;
[0031] Step 3: Then, the polyvinylidene fluoride resin and polybutyl methacrylate are mixed thoroughly, and then added into the mixer of step 2, and stirring is continued for 15-25 minutes to obtain the first product;
[0032] Step 4: Add an antioxidant and a compatibilizer to the first product and continue stirring for 1-5 minutes to obtain a second product;
[0033] Step 5: Use a twin-screw extruder granulator to granulate the second product, the processing temperature is 350-380°C, and the screw aspect ratio is 30-40; then use a casting method to prepare the particles into the fluorine film of the present invention, the process temperature is 320-380°C, the cooling roller temperature is 120-160°C, and the prepared fluorine film has a thickness of 30-40μm.
[0034] Compared with the prior art, the present invention has the following beneficial effects:
[0035] The high-transparency fluorine film of the present invention adopts polyvinylidene fluoride resin and polybutyl methacrylate as base materials, adds nano-barium sulfate compound bentonite modified double adjuster and guiding functional agent to cooperate with each other, uses interface agent to improve the interface effect between product raw materials, and adds antioxidant and compatibilizer raw materials as auxiliary agents to enhance the overall performance effect of the product system; the traditional process adopts multi-layer film stacking method to enhance the barrier and water barrier and mechanical strength performance of the product, but multi-layer lamination is easy to reduce the light transmittance of the film, and the process is complicated. The present invention is optimized and improved, does not need multi-layer lamination, and has a simple process. At the same time, the mechanical properties, barrier and light transmittance properties are coordinated and improved, and the performance of the product is coordinated and improved;
[0036] The nano-barium sulfate compounded bentonite modified double adjuster of the present invention is optimized and improved by coordinating a nano-barium sulfate coordination leveling agent with a tannic acid solution, and the bentonite is treated by a thermal reaction to expand the interlamellar spacing and improve its channel property, thereby optimizing the light transmittance of the product on the one hand and improving its accommodation space on the other hand, thereby enhancing the optimization and improvement effect of the tannic acid-coordinated nano-barium sulfate compounding liquid, and coordinating and improving the barrier, light transmittance and mechanical properties of the product; the nano-barium sulfate compounding liquid is modified by ball milling with nano-barium sulfate and then coordinating with a tannic acid solution, and the coordinating effect of the ball-milled modified nano-barium sulfate in the system is enhanced, and the coordination performance of the system is more perfect; the coordination of the tannic acid solution can enhance the dispersibility between the raw materials in the system, and promote the product system Improved effect; at the same time, tannic acid has the structure of polyphenol hydroxyl groups, and polyphenols first approach the surface of the organic molecules of the system through hydrophobic bonds, enter its hydrophobic zone, and undergo two-point hydrogen bonding. The simultaneous action of hydrophobic bonds and hydrogen bonds enables it to improve the strength performance of the system structure in a multi-point bonding manner; thereby improving the overall performance and stability of the product; at the same time, the guiding functional agent in the product adopts nanocellulose dispersed through a hydrochloric acid solution to improve its dispersion, and then is modified through the synergistic coordination of a titanate coupling agent, octadecyltrimethylammonium chloride and stearic acid. The synergistic effect of the modified nanocellulose and the nano-barium sulfate compound bentonite modified double adjuster is enhanced, thereby improving the overall coordination stability of the system and improving the performance of the product. DETAILED DESCRIPTION
[0037] The following is a clear and complete description of the technical solutions in the embodiments of the present invention in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0038] A highly transparent fluorine film of this embodiment comprises the following raw materials in parts by weight:
[0039] 60-70 parts of polyvinylidene fluoride resin, 20-30 parts of polybutyl methacrylate, 5-10 parts of nano-barium sulfate compounded bentonite modified double adjuster, 3-6 parts of guiding functional agent, 2-5 parts of interface agent, 1-2 parts of antioxidant, and 1-2 parts of compatibilizer.
[0040] The highly transparent fluorine film of this embodiment comprises the following raw materials in parts by weight:
[0041] 65 parts of polyvinylidene fluoride resin, 25 parts of polybutyl methacrylate, 7.5 parts of nano-barium sulfate compounded bentonite modified double adjuster, 4.5 parts of guiding functional agent, 3.5 parts of interface agent, 1.5 parts of antioxidant, and 1.5 parts of compatibilizer.
[0042] The weight average molecular weight of the polyvinylidene fluoride resin in this embodiment is 400,000-600,000, and the apparent density is 0.45-0.55 g / cm 2 ;
[0043] The antioxidant is 2,8-di-tert-butyl-4-methylphenol and phosphite in a weight ratio of (4-7):1; the compatibilizer is maleic anhydride grafted ethylene-propylene copolymer;
[0044] The interface agent is coupling agent KH560.
[0045] The preparation method of the nano-barium sulfate compounded bentonite modified double adjuster of this embodiment is:
[0046] S11: adding tannic acid to deionized water and mixing to prepare a tannic acid solution with a mass fraction of 1-2.5%;
[0047] S12: then adding 5-10% of the total amount of the tannic acid solution to the nano-barium sulfate coordination agent, mixing evenly, to obtain a tannic acid synergistic nano-barium sulfate complexing solution;
[0048] S13: Then, the bentonite is treated with a thermal-tannic acid-synergistic nano-barium sulfate compounding solution to obtain a nano-barium sulfate-compounded bentonite modified double agent;
[0049] The specific steps of the synergistic treatment of the thermal-tannic acid-combined nano-barium sulfate compounding solution are as follows:
[0050] S102: Bentonite is first subjected to thermal reaction at 350-400°C for 5-10 minutes, then cooled to 150°C at a rate of 1-3°C / min, kept at this temperature for 10-20 minutes, and finally air-cooled to room temperature;
[0051] S112: Then add it into the tannic acid synergistic nano-barium sulfate complex solution in a weight ratio of 3:(5-9), stir and react, then wash with water and dry.
[0052] The preparation method of the nano barium sulfate coordination and leveling agent of this embodiment is:
[0053] Place the nano-barium sulfate in a ball mill for ball milling modification, add 2-5% of the total amount of nano-barium sulfate in the ball milling modification liquid, wash with water, and dry after the ball milling is completed;
[0054] The ball milling modification liquid comprises the following raw materials in parts by weight: 2-5 parts of yttrium nitrate, 1-3 parts of silica sol, 5-10 parts of deionized water, 0.5-1 parts of phosphate buffer solution, and 0.2-0.5 parts of triethanolamine borate.
[0055] The rotation speed of the ball milling modification in this embodiment is 1000-1500 r / min, and the ball milling time is 20-30 min.
[0056] The pH value of the phosphate buffer solution of this embodiment is 4.5-5.5.
[0057] In S112 of this embodiment, the stirring reaction temperature is 35-40° C., the stirring time is 45-55 min, and the stirring speed is 500-1000 r / min.
[0058] The preparation method of the guiding functional agent of this embodiment is:
[0059] The nanocellulose is first placed in a 3-5 times mass fraction 2-5% hydrochloric acid solution and stirred at a speed of 300-400r / min for 35-45min; then 2-5% titanate coupling agent, 1-4% octadecyltrimethylammonium chloride and 1-3% stearic acid are added to the total amount of the hydrochloric acid solution, and then stirred at a speed of 100-200r / min for 1-2h, stirred evenly, washed with water and dried to obtain a guiding functional agent.
[0060] A method for preparing a highly transparent fluorine film in this embodiment comprises the following steps:
[0061] Step 1: Weigh the raw materials:
[0062] Step 2: Send the nano-barium sulfate compounded with bentonite modified double adjuster, guiding functional agent, and interface agent into a mixer for stirring until the raw materials are evenly mixed;
[0063] Step 3: Then, the polyvinylidene fluoride resin and polybutyl methacrylate are mixed thoroughly, and then added into the mixer of step 2, and stirring is continued for 15-25 minutes to obtain the first product;
[0064] Step 4: Add an antioxidant and a compatibilizer to the first product and continue stirring for 1-5 minutes to obtain a second product;
[0065] Step 5: Use a twin-screw extruder granulator to granulate the second product, the processing temperature is 350-380°C, and the screw aspect ratio is 30-40; then use a casting method to prepare the particles into the fluorine film of the present invention, the process temperature is 320-380°C, the cooling roller temperature is 120-160°C, and the prepared fluorine film has a thickness of 30-40μm.
[0066] Example 1.
[0067] A highly transparent fluorine film of this embodiment comprises the following raw materials in parts by weight:
[0068] 60 parts of polyvinylidene fluoride resin, 20 parts of polybutyl methacrylate, 5 parts of nano-barium sulfate compounded bentonite modified double adjuster, 3 parts of guiding functional agent, 2 parts of interface agent, 1 part of antioxidant, and 1 part of compatibilizer.
[0069] The weight average molecular weight of the polyvinylidene fluoride resin in this embodiment is 400,000, and the apparent density is 0.45 g / cm 2 ;
[0070] The antioxidant is 2,8-di-tert-butyl-4-methylphenol and phosphite in a weight ratio of 4:1; the compatibilizer is maleic anhydride grafted ethylene-propylene copolymer;
[0071] The interface agent is coupling agent KH560.
[0072] The preparation method of the nano-barium sulfate compounded bentonite modified double adjuster of this embodiment is:
[0073] S11: adding tannic acid into deionized water and mixing, first preparing a tannic acid solution with a mass fraction of 1%;
[0074] S12: then adding a nano-barium sulfate coordination agent of 5% of the total amount of the tannic acid solution, mixing evenly, to obtain a tannic acid synergistic nano-barium sulfate complexing solution;
[0075] S13: Then, the bentonite is treated with a thermal-tannic acid-synergistic nano-barium sulfate compounding solution to obtain a nano-barium sulfate-compounded bentonite modified double agent;
[0076] The specific steps of the synergistic treatment of the thermal-tannic acid-combined nano-barium sulfate compounding solution are as follows:
[0077] S102: The bentonite was first subjected to thermal reaction at 350°C for 5 min, then the temperature was reduced to 150°C at a rate of 1°C / min, kept at that temperature for 10 min, and finally air-cooled to room temperature;
[0078] S112: then add the mixture into the tannic acid synergistic nano-barium sulfate compounding solution in a weight ratio of 3:5, stir for reaction, and then wash with water and dry.
[0079] The preparation method of the nano barium sulfate coordination and leveling agent of this embodiment is:
[0080] Place the nano-barium sulfate in a ball mill for ball milling modification, add 2-5% of the total amount of nano-barium sulfate in the ball milling modification liquid, wash with water, and dry after the ball milling is completed;
[0081] The ball milling modification liquid includes the following raw materials in parts by weight: 2 parts of yttrium nitrate, 1 part of silica sol, 5 parts of deionized water, 0.5 parts of phosphate buffer solution, and 0.2 parts of triethanolamine borate.
[0082] The rotation speed of the ball milling modification in this embodiment is 1000 r / min, and the ball milling time is 20 min.
[0083] The pH value of the phosphate buffer solution in this example is 4.5.
[0084] In S112 of this embodiment, the stirring reaction temperature is 35° C., the stirring time is 45 min, and the stirring speed is 500 r / min.
[0085] The preparation method of the guiding functional agent of this embodiment is:
[0086] The nanocellulose is first placed in a 3-fold mass fraction 2% hydrochloric acid solution and stirred at a speed of 300 r / min for 35 minutes; then 2% of a titanate coupling agent, 1% of octadecyltrimethylammonium chloride, and 1% of stearic acid are added to the total amount of the hydrochloric acid solution, and then stirred at a speed of 100 r / min for 1 hour. The mixture is stirred evenly, washed with water, and dried to obtain a guiding functional agent.
[0087] A method for preparing a highly transparent fluorine film in this embodiment comprises the following steps:
[0088] Step 1: Weigh the raw materials:
[0089] Step 2: Send the nano-barium sulfate compounded with bentonite modified double adjuster, guiding functional agent, and interface agent into a mixer for stirring until the raw materials are evenly mixed;
[0090] Step 3: Then, the polyvinylidene fluoride resin and polybutyl methacrylate are mixed thoroughly, and then added into the mixer of step 2, and stirring is continued for 15 minutes to obtain the first product;
[0091] Step 4: Add antioxidant and compatibilizer to the first product and continue stirring for 1 minute to obtain the second product;
[0092] Step 5: Use a twin-screw extruder granulator to granulate the second product, the processing temperature is 350°C, and the screw aspect ratio is 30; then use a casting method to prepare the particles into the fluorine film of the present invention, the process temperature is 320°C, the cooling roller temperature is 120°C, and the prepared fluorine film has a thickness of 30μm.
[0093] Example 2.
[0094] A highly transparent fluorine film of this embodiment comprises the following raw materials in parts by weight:
[0095] 70 parts of polyvinylidene fluoride resin, 30 parts of polybutyl methacrylate, 10 parts of nano-barium sulfate compounded bentonite modified double adjuster, 6 parts of guiding functional agent, 5 parts of interface agent, 2 parts of antioxidant, and 2 parts of compatibilizer.
[0096] The weight average molecular weight of the polyvinylidene fluoride resin in this embodiment is 600,000, and the apparent density is 0.55 g / cm 2 ;
[0097] The antioxidant is 2,8-di-tert-butyl-4-methylphenol and phosphite in a weight ratio of 7:1; the compatibilizer is maleic anhydride grafted ethylene-propylene copolymer;
[0098] The interface agent is coupling agent KH560.
[0099] The preparation method of the nano-barium sulfate compounded bentonite modified double adjuster of this embodiment is:
[0100] S11: adding tannic acid into deionized water and mixing, first preparing a tannic acid solution with a mass fraction of 2.5%;
[0101] S12: then adding a nano-barium sulfate coordination agent of 10% of the total amount of the tannic acid solution, mixing evenly, to obtain a tannic acid synergistic nano-barium sulfate compounding solution;
[0102] S13: Then, the bentonite is treated with a thermal-tannic acid-synergistic nano-barium sulfate compounding solution to obtain a nano-barium sulfate-compounded bentonite modified double agent;
[0103] The specific steps of the synergistic treatment of the thermal-tannic acid-combined nano-barium sulfate compounding solution are as follows:
[0104] S102: Bentonite was first subjected to thermal reaction at 400°C for 10 min, then cooled to 150°C at a rate of 3°C / min, kept at that temperature for 20 min, and finally air-cooled to room temperature;
[0105] S112: Then add the mixture into the tannic acid synergistic nano-barium sulfate complex solution in a weight ratio of 1:3, stir for reaction, wash with water, and dry.
[0106] The preparation method of the nano barium sulfate coordination and leveling agent of this embodiment is:
[0107] Place the nano-barium sulfate in a ball mill for ball milling modification, add 2-5% of the total amount of nano-barium sulfate in the ball milling modification liquid, wash with water, and dry after the ball milling is completed;
[0108] The ball milling modification liquid includes the following raw materials in parts by weight: 5 parts of yttrium nitrate, 3 parts of silica sol, 10 parts of deionized water, 1 part of phosphate buffer solution, and 0.5 parts of triethanolamine borate.
[0109] The rotation speed of the ball milling modification in this embodiment is 1500 r / min, and the ball milling time is 30 min.
[0110] The pH value of the phosphate buffer solution in this example is 5.5.
[0111] In S112 of this embodiment, the stirring reaction temperature is 40° C., the stirring time is 55 min, and the stirring speed is 1000 r / min.
[0112] The preparation method of the guiding functional agent of this embodiment is:
[0113] The nanocellulose is first placed in a 5-fold mass fraction of a 5% hydrochloric acid solution and stirred at a speed of 400 r / min for 45 minutes; then 5% of a titanate coupling agent, 4% of octadecyltrimethylammonium chloride, and 3% of stearic acid are added to the total amount of the hydrochloric acid solution, and then stirred at a speed of 200 r / min for 2 hours. The mixture is stirred evenly, washed with water, and dried to obtain a guiding functional agent.
[0114] A method for preparing a highly transparent fluorine film in this embodiment comprises the following steps:
[0115] Step 1: Weigh the raw materials:
[0116] Step 2: Send the nano-barium sulfate compounded with bentonite modified double adjuster, guiding functional agent, and interface agent into a mixer for stirring until the raw materials are evenly mixed;
[0117] Step 3: Then, the polyvinylidene fluoride resin and polybutyl methacrylate are mixed thoroughly, and then added into the mixer of step 2, and stirring is continued for 25 minutes to obtain the first product;
[0118] Step 4: adding an antioxidant and a compatibilizer to the first product and continuing stirring for 5 minutes to obtain a second product;
[0119] Step 5: Use a twin-screw extruder granulator to granulate the second product, the processing temperature is 380°C, and the screw aspect ratio is 40; then use a casting method to prepare the particles into the fluorine film of the present invention, the process temperature is 380°C, the cooling roller temperature is 160°C, and the prepared fluorine film has a thickness of 40μm.
[0120] Example 3.
[0121] A highly transparent fluorine film of this embodiment comprises the following raw materials in parts by weight:
[0122] 65 parts of polyvinylidene fluoride resin, 25 parts of polybutyl methacrylate, 7.5 parts of nano-barium sulfate compounded bentonite modified double adjuster, 4.5 parts of guiding functional agent, 3.5 parts of interface agent, 1.5 parts of antioxidant, and 1.5 parts of compatibilizer.
[0123] The weight average molecular weight of the polyvinylidene fluoride resin in this embodiment is 500,000 and the apparent density is 0.50 g / cm 2 ;
[0124] The antioxidant is 2,8-di-tert-butyl-4-methylphenol and phosphite in a weight ratio of 5.5:1; the compatibilizer is maleic anhydride grafted ethylene-propylene copolymer;
[0125] The interface agent is coupling agent KH560.
[0126] The preparation method of the nano-barium sulfate compounded bentonite modified double adjuster of this embodiment is:
[0127] S11: adding tannic acid to deionized water and mixing to prepare a tannic acid solution with a mass fraction of 1.5%;
[0128] S12: then adding a nano-barium sulfate coordination agent of 7.5% of the total amount of the tannic acid solution, mixing evenly, to obtain a tannic acid-coordinated nano-barium sulfate compounding solution;
[0129] S13: Then, the bentonite is treated with a thermal-tannic acid-synergistic nano-barium sulfate compounding solution to obtain a nano-barium sulfate-compounded bentonite modified double agent;
[0130] The specific steps of the synergistic treatment of the thermal-tannic acid-combined nano-barium sulfate compounding solution are as follows:
[0131] S102: The bentonite was first subjected to thermal reaction at 375°C for 7.5 min, then cooled to 150°C at a rate of 2°C / min, kept at that temperature for 15 min, and finally air-cooled to room temperature;
[0132] S112: Then add the mixture into the tannic acid synergistic nano-barium sulfate complex solution in a weight ratio of 3:7, stir for reaction, and then wash with water and dry.
[0133] The preparation method of the nano barium sulfate coordination and leveling agent of this embodiment is:
[0134] Place the nano-barium sulfate in a ball mill for ball milling modification, add 3.5% of the total amount of nano-barium sulfate in the ball milling modification liquid, wash with water, and dry after the ball milling is completed;
[0135] The ball milling modification liquid includes the following raw materials in parts by weight: 3.5 parts of yttrium nitrate, 2 parts of silica sol, 7.5 parts of deionized water, 0.75 parts of phosphate buffer solution, and 0.35 parts of triethanolamine borate.
[0136] The rotation speed of the ball milling modification in this embodiment is 1250 r / min, and the ball milling time is 25 min.
[0137] The pH value of the phosphate buffer solution in this example is 5.0.
[0138] In S112 of this embodiment, the stirring reaction temperature is 37° C., the stirring time is 50 min, and the stirring speed is 750 r / min.
[0139] The preparation method of the guiding functional agent of this embodiment is:
[0140] The nanocellulose is first placed in a 4-fold mass fraction 3.5% hydrochloric acid solution and stirred at a speed of 350 r / min for 40 minutes; then 3.5% of a titanate coupling agent, 2.5% of octadecyltrimethylammonium chloride and 2% of stearic acid are added to the total amount of the hydrochloric acid solution, and then stirred at a speed of 150 r / min for 1.5 hours. The mixture is stirred evenly, washed with water and dried to obtain a guiding functional agent.
[0141] A method for preparing a highly transparent fluorine film in this embodiment comprises the following steps:
[0142] Step 1: Weigh the raw materials:
[0143] Step 2: Send the nano-barium sulfate compounded with bentonite modified double adjuster, guiding functional agent, and interface agent into a mixer for stirring until the raw materials are evenly mixed;
[0144] Step 3: Then, the polyvinylidene fluoride resin and polybutyl methacrylate are mixed thoroughly, and then added into the mixer of step 2, and stirring is continued for 20 minutes to obtain the first product;
[0145] Step 4: adding an antioxidant and a compatibilizer to the first product and continuing stirring for 3 minutes to obtain a second product;
[0146] Step 5: Use a twin-screw extruder granulator to granulate the second product, the processing temperature is 365°C, and the screw aspect ratio is 35; then use a casting method to prepare the particles into the fluorine film of the present invention, the process temperature is 350°C, the cooling roller temperature is 140°C, and the prepared fluorine film has a thickness of 35μm.
[0147] Comparative Example 1.
[0148] The difference from Example 3 is that the nano-barium sulfate compounded bentonite modified double adjuster is not added.
[0149] Comparative Example 2.
[0150] The difference from Example 3 is that the preparation method of the nano-barium sulfate compounded bentonite modified double adjuster is: add 7.5% nano-barium sulfate to the total amount of deionized water, mix well, then add bentonite to the mixture at a weight ratio of 3:7, stir well, wash with water, and dry.
[0151] Comparative Example 3.
[0152] The difference from Example 3 is that in the preparation of the nano-barium sulfate compounded with bentonite modified double adjuster, the nano-barium sulfate is replaced by hydroxyapatite raw material, and the other process conditions are the same.
[0153] Comparative Example 4.
[0154] The difference from Example 3 is that in the preparation of the nano-barium sulfate compounded bentonite modified double adjuster, the tannic acid solution is replaced by a chitosan solution with a mass fraction of 5%.
[0155] Comparative Example 5.
[0156] The difference from Example 3 is that no nano-barium sulfate coordinating and leveling agent is added in the preparation of the nano-barium sulfate compounded bentonite modified double adjuster.
[0157] Comparative Example 6.
[0158] The difference from Example 3 is that the nano-barium sulfate coordinating and leveling agent is replaced by nano-barium sulfate.
[0159] Comparative Example 7.
[0160] The difference from Example 3 is that the specific process of the synergistic treatment of the heating-tannic acid-nano barium sulfate compounding liquid is different:
[0161] S102: The bentonite was placed at 375°C for a thermal reaction for 7.5 min and then directly air-cooled to room temperature;
[0162] S112: Then add the mixture into the tannic acid synergistic nano-barium sulfate complex solution in a weight ratio of 3:7, stir for reaction, and then wash with water and dry.
[0163] Comparative Example 8.
[0164] The difference from Example 3 is that no targeting functional agent is added.
[0165] Comparative Example 9.
[0166] The difference from Example 3 is that the guiding functional agent is replaced by nanocellulose.
[0167] Comparative Example 10.
[0168] The difference from Example 3 is that no titanate coupling agent is added in the preparation of the guiding functional agent.
[0169] Comparative Example 11.
[0170] The difference from Example 3 is that octadecyltrimethylammonium chloride is not added in the preparation of the directing functional agent.
[0171] Comparative Example 12.
[0172] The difference from Example 3 is that deionized water is used instead of hydrochloric acid solution in the preparation of the guiding functional agent. The performance measurement results of Examples 1-3 and Comparative Examples 1-12 are as follows
[0173]
[0174]
[0175] From Examples 1-3 and Comparative Examples 1-12, it can be concluded that the light transmittance of the present invention can be as high as 98%, the water vapor transmission rate can be as low as 0.28, the tensile strength MD and the elongation at break MD can reach 87MPa and 665% respectively, and the light transmittance, water vapor barrier and mechanical properties of the product can be improved in a coordinated manner;
[0176] It can be seen from Comparative Examples 1-3 and Example 3 that the mechanical properties, light transmittance and water vapor barrier properties of the product are significantly deteriorated without adding nano-barium sulfate compounded bentonite modified double adjuster; at the same time, the nano-barium sulfate compounded bentonite modified double adjuster is directly prepared with bentonite and nano-barium sulfate, and the performance of the product does not change much compared to the double adjuster without adding nano-barium sulfate compounded bentonite modified, so bentonite and nano-barium sulfate are directly prepared, and the performance improvement effect of the product is poor;
[0177] In the preparation of nano-barium sulfate compounded with bentonite modified double adjuster, nano-barium sulfate is replaced by hydroxyapatite raw material. The inventors found that the light transmittance did not change much, but the water vapor barrier and mechanical properties showed a significant deterioration trend;
[0178] It can be seen from Comparative Examples 4-7 and Example 3 that in the preparation of the nano-barium sulfate composite bentonite modified double adjuster, the tannic acid solution is replaced by a chitosan solution with a mass fraction of 5%. The mechanical, light transmittance and water vapor barrier properties of the product all have a significant deterioration trend, and the product performance deteriorates significantly when treated with chitosan solution. Only the use of tannic acid solution can promote the improvement effect of the product.
[0179] In the preparation of the nano-barium sulfate compounded bentonite modified double adjuster, no nano-barium sulfate coordination and leveling agent was added, the nano-barium sulfate coordination and leveling agent was replaced by nano-barium sulfate, and the performance of the product tended to deteriorate. In the specific process of thermal-tannic acid synergistic nano-barium sulfate compounding liquid synergistic treatment S102: bentonite was placed at 375°C for thermal reaction for 7.5 minutes, and then directly air-cooled to room temperature, the performance of the product tended to deteriorate. Only the nano-barium sulfate compounded bentonite modified double adjuster prepared by the method of the present invention has the most significant effect on the performance of the product, and other methods are not as good as the effect produced by the method of the present invention;
[0180] It can be seen from Comparative Examples 8-12 and Example 3 that the performance of the products deteriorated to varying degrees when no guiding functional agent was added, when the guiding functional agent was replaced by nanocellulose, and when the guiding functional agent was prepared by different methods. Only when the guiding functional agent was prepared by the method of the present invention, the performance effect of the product was the most significant.
[0181] In addition, it was found in Comparative Examples 8-9 that the performance of the product was worse when nanocellulose was added than when no guiding functional agent was added. This may be because the nanocellulose was used directly without being optimized by the method of the present invention, and the nanocellulose had a high degree of aggregation, which affected the overall performance of the product.
[0182] It is found from Comparative Examples 1-2, Comparative Example 8 and Example 3 that
[0183] The present invention does not add one of the nano-barium sulfate compounded bentonite modified double adjuster and the guiding functional agent, or directly uses nano-barium sulfate and bentonite for preparation, and the performance of the product has an obvious deterioration trend. Nano-barium sulfate compounded bentonite modified double adjuster and the guiding functional agent are used for compounding, and the two are synergistically enhanced to jointly enhance the performance effect of the product, and coordinately improve the mechanical properties, water vapor barrier and light transmission properties of the product.
[0184] The product of the present invention was placed in a 2% by mass hydrochloric acid solution for 1 hour, and the performance was tested;
[0185]
[0186]
[0187] The products of Examples 1-3 of the present invention have stable performance in a corrosive environment. As can be seen from Comparative Examples 1-12, without adding nano-barium sulfate compounded bentonite modified double adjuster and guiding functional agent, the stability of corrosion resistance performance has a significant trend of deterioration;
[0188] At the same time, from Comparative Example 3, the present invention found that in the preparation of the nano-barium sulfate compounded bentonite modified double adjuster, the nano-barium sulfate was replaced by hydroxyapatite raw material, and the light transmittance changed significantly, and the water vapor barrier and mechanical properties showed a significant deterioration trend;
[0189] In summary, nano-barium sulfate is proprietary and cannot be replaced by hydroxyapatite raw materials. The use of nano-barium sulfate not only provides excellent light transmittance for the product, but also the performance of the product remains stable under acid corrosion conditions;
[0190] It is found from Comparative Examples 5-6 and Example 3 that when the nano-barium sulfate coordinating and leveling agent is replaced by nano-barium sulfate, the performance of the product also changes greatly under the acid-corrosion conditions of the product, and the stability of the product performance is significantly reduced.
[0191] The present invention further explores the performance of nano-barium sulfate coordination and leveling agent:
[0192] The preparation method of nano barium sulfate coordination and leveling agent is as follows:
[0193] Place the nano-barium sulfate in a ball mill for ball milling modification, add 3.5% of the total amount of nano-barium sulfate in the ball milling modification liquid, wash with water, and dry after the ball milling is completed;
[0194] The ball milling modification liquid includes the following raw materials in parts by weight: 3.5 parts of yttrium nitrate, 2 parts of silica sol, 7.5 parts of deionized water, 0.75 parts of phosphate buffer solution, and 0.35 parts of triethanolamine borate.
[0195] The rotation speed of the ball milling modification in this embodiment is 1250 r / min, and the ball milling time is 25 min.
[0196] The pH value of the phosphate buffer solution in this example is 5.0.
[0197] Experimental Example 1
[0198] The raw materials of the product are the same as those of Example 3, except that the rotation speed of the ball milling modification treatment in the nano-barium sulfate coordination and leveling agent is 500 r / min, and the ball milling is 10 minutes.
[0199] Experimental Example 2
[0200] The raw materials are the same as those of the product in Example 3, except that yttrium nitrate is not added to the ball milling modification liquid.
[0201] Experimental Example 3
[0202] The raw materials are the same as those of the product in Example 3, except that no silica sol is added to the ball milling modified liquid.
[0203] Experimental Example 4
[0204] The raw materials are the same as those of the product in Example 3, except that triethanolamine borate is not added to the ball milling modification liquid.
[0205] Experimental Example 5
[0206] The raw materials are the same as those of the product in Example 3, except that no phosphate buffer solution is added to the ball milling modification solution.
[0207] The test is based on the test condition that the product is placed in a 2% hydrochloric acid solution for 1 hour:
[0208]
[0209]
[0210] In the preparation of the nano-barium sulfate coordination and leveling agent, the ball milling speed conditions and the components of the ball milling modification liquid in the nano-barium sulfate coordination and leveling agent have an impact on the performance of the product. Yttrium nitrate has the greatest impact, followed by silica sol. When silica sol, triethanolamine borate and phosphate buffer solution are used as auxiliary compounding agents, combined with yttrium nitrate and ball milling conditions, the performance effect of the product is the best. The nano-barium sulfate coordination and leveling agent prepared by other methods is not as significant as the method of the present invention.
[0211] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.
[0212] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A highly transparent fluorine film, characterized in that: The highly transparent fluorine film comprises the following raw materials in parts by weight: 60-70 parts of polyvinylidene fluoride resin, 20-30 parts of polybutyl methacrylate, 5-10 parts of nano-barium sulfate compounded bentonite modified double adjuster, 3-6 parts of guiding functional agent, 2-5 parts of interface agent, 1-2 parts of antioxidant, and 1-2 parts of compatibilizer.
2. A highly transparent fluorine film according to claim 1, characterized in that: The highly transparent fluorine film comprises the following raw materials in parts by weight: 65 parts of polyvinylidene fluoride resin, 25 parts of polybutyl methacrylate, 7.5 parts of nano-barium sulfate compounded bentonite modified double adjuster, 4.5 parts of guiding functional agent, 3.5 parts of interface agent, 1.5 parts of antioxidant, and 1.5 parts of compatibilizer.
3. A highly transparent fluorine film according to claim 1, characterized in that: The polyvinylidene fluoride resin has a weight average molecular weight of 400,000-600,000 and an apparent density of 0.45-0.55 g / cm²; The antioxidant is 2,8-di-tert-butyl-4-methylphenol and phosphite in a weight ratio of (4-7):1; the compatibilizer is maleic anhydride grafted ethylene-propylene copolymer; The interface agent is coupling agent KH560.
4. A highly transparent fluorine film according to claim 3, characterized in that: The preparation method of the nano-barium sulfate compounded bentonite modified double adjuster is: S11: adding tannic acid to deionized water and mixing to prepare a tannic acid solution having a mass fraction of 1-2.5%; S12: Then, a nano-barium sulfate coordination agent is added thereto, which accounts for 5-10% of the total amount of the tannic acid solution, and the mixture is mixed evenly to obtain a tannic acid-coordinated nano-barium sulfate compounding solution; S13: Then, the bentonite is treated with a thermal-tannic acid-synergistic nano-barium sulfate compounding solution to obtain a nano-barium sulfate-compounded bentonite modified double agent; The specific steps of the synergistic treatment of the thermal-tannic acid-combined nano-barium sulfate compounding solution are as follows: S102: Bentonite is first subjected to thermal reaction at 350-400°C for 5-10 minutes, then cooled to 150°C at a rate of 1-3°C / min, kept at this temperature for 10-20 minutes, and finally air-cooled to room temperature; S112: Then add it into the tannic acid synergistic nano-barium sulfate complex solution in a weight ratio of 3: (5-9), stir and react, then wash with water and dry.
5. A highly transparent fluorine film according to claim 4, characterized in that: The preparation method of the nano barium sulfate coordination and leveling agent is as follows: Place the nano-barium sulfate in a ball mill for ball milling modification, add 2-5% of the total amount of nano-barium sulfate in the ball milling modification liquid, wash with water, and dry after the ball milling is completed; The ball milling modification liquid comprises the following raw materials in parts by weight: 2-5 parts of yttrium nitrate, 1-3 parts of silica sol, 5-10 parts of deionized water, 0.5-1 parts of phosphate buffer solution, and 0.2-0.5 parts of triethanolamine borate.
6. A highly transparent fluorine film according to claim 5, characterized in that: The rotation speed of the ball milling modification is 1000-1500r / min, and the ball milling time is 20-30min.
7. The highly transparent fluorine film according to claim 5, characterized in that: The pH value of the phosphate buffer solution is 4.5-5.
5.
8. The highly transparent fluorine film according to claim 4, characterized in that: The stirring reaction temperature of S112 is 35-40°C, the stirring time is 45-55min, and the stirring speed is 500-1000r / min.
9. The highly transparent fluorine film according to claim 1, characterized in that: The preparation method of the guiding functional agent is: The nanocellulose is first placed in a 3-5 times mass fraction 2-5% hydrochloric acid solution and stirred at a speed of 300-400r / min for 35-45min; then 2-5% titanate coupling agent, 1-4% octadecyltrimethylammonium chloride and 1-3% stearic acid are added to the total amount of the hydrochloric acid solution, and then stirred at a speed of 100-200r / min for 1-2h, stirred evenly, washed with water and dried to obtain a guiding functional agent.
10. A method for preparing a highly transparent fluorine film according to any one of claims 1 to 9, characterized in that: The following steps are involved: Step 1: Weigh the raw materials: Step 2: Send the nano barium sulfate compounded with bentonite modified double adjuster, guiding functional agent and interface agent into a mixer for stirring until the raw materials are evenly mixed; Step 3: Then, the polyvinylidene fluoride resin and polybutyl methacrylate are mixed thoroughly, and then added into the mixer of step 2, and stirring is continued for 15-25 minutes to obtain the first product; Step 4: Add an antioxidant and a compatibilizer to the first product and continue stirring for 1-5 minutes to obtain a second product; Step 5: Use a twin-screw extruder granulator to granulate the second product, the processing temperature is 350-380°C, and the screw aspect ratio is 30-40; then use a casting method to prepare the particles into the fluorine film of the present invention, the process temperature is 320-380°C, the cooling roller temperature is 120-160°C, and the prepared fluorine film has a thickness of 30-40μm.