Filler composition capable of reducing rolling resistance of tire, low-rolling-resistance tire rubber material, preparation method of low-rolling-resistance tire rubber material and tire
By combining modified graphene oxide masterbatch with silica, and leveraging the synergistic effect of polysulfide compounds and silane coupling agents, the problem of poor reinforcing effect of silica and graphene oxide fillers was solved, achieving efficient dispersion and low rolling resistance in tire rubber materials.
Patent Information
- Application Number
- CN202411174627.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-08-26
AI Technical Summary
In existing technologies, the actual reinforcing effect of using silica and graphene oxide as fillers is not good. The compatibility modification strategy of graphene oxide with rubber matrix has poor controllability, making it difficult to simultaneously improve the tensile strength, aging resistance and wear resistance of rubber compounds.
Modified graphene oxide masterbatch was used in combination with silica. The graphene oxide masterbatch was grafted with polysulfide compounds, and its combination with silica was controlled during the mixing heat treatment. The amino functional groups grafted on the surface of modified graphene oxide catalyzed the silanization reaction of silane coupling agent, thereby improving the interfacial interaction.
It effectively promotes the dispersion of fillers in the rubber matrix, enhances the interfacial bonding between graphene oxide and the rubber matrix, improves the reinforcing effect, reduces tire rolling resistance, and achieves high-efficiency tire rubber material performance.
Smart Images

Figure CN118909326A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of tire rubber, and in particular relates to a filler composition capable of reducing tire rolling resistance, a low rolling resistance tire rubber material, a preparation method thereof and a tire. Background Art
[0002] The rolling resistance, wet skid resistance and wear resistance of tread rubber affect the fuel efficiency, safety and service life of tires respectively. The improvement of one performance often reduces the other one or two performances. The relationship between them and the constraints is called the "magic triangle". Studies have shown that the addition of fillers will improve the tensile strength, aging resistance and wear resistance of rubber to varying degrees, and significantly affect the performance of the "magic triangle", making the performance of filler-modified tire rubber a research hotspot.
[0003] Limited by the cost and high binding energy of graphene, it is difficult to realize the real application of graphene as a single filler in the preparation of tire rubber. The use of white carbon black and graphene oxide as fillers can reduce the amount of graphene used, save costs, and utilize the hybrid synergistic effect of fillers to improve the dispersibility of graphene in the rubber matrix, which is an effective measure to prepare high-performance graphene tire rubber materials. However, due to the poor compatibility of graphene oxide with the rubber matrix, the interface bonding between graphene oxide and the rubber matrix is poor, which limits the actual reinforcement effect. In order to improve the problem of poor compatibility between graphene oxide and the rubber matrix, the relevant field provides many methods for modifying graphene oxide. For example, J.Phys.D et al. non-covalently modified graphene oxide with sodium 12α-dihydroxy-5β-cholanate to improve the compatibility of graphene oxide with the rubber matrix; Small et al. grafted 2-acrylamide on the surface of graphene oxide to enhance the interface bonding between rubber and graphene oxide. In addition, how to improve the synergistic reinforcement effect of graphene and silica in tire rubber has always been a major challenge faced by this field.
[0004] As mentioned above, common graphene modification methods usually involve complex chemical modification processes, there are problems such as the use of organic solvents, poor controllability, high difficulty in scale, etc., it is difficult to be actually applied to industrial products such as tires, and the dispersion effect is poor, the interface effect is weak, and the performance of the prepared rubber composite material is difficult to simultaneously improve the dynamic service performance (low rolling resistance, high wet-slip resistance), tensile strength, aging resistance and wear resistance of the rubber material, and it is impossible to apply it to tire formulations. In addition, while modifying graphene oxide, it is also necessary to consider the interaction between graphene and white carbon black, in order to use graphene oxide / white carbon black combination to fill tire rubber materials to achieve synergistic enhancement, and obtain tire rubber materials with low rolling resistance and high wet-slip resistance. Therefore, it is necessary to develop a modification method and filler composition based on graphene oxide to provide a new solution for preparing high-performance tire rubber materials with low rolling resistance. Summary of the invention
[0005] The present application discloses a filler composition capable of reducing the rolling resistance of a tire, a low rolling resistance tire rubber material, a preparation method thereof and a tire, aiming to solve the technical problems that the actual reinforcement effect of the existing filler using white carbon black and graphene oxide is poor, and the modification strategy for improving the compatibility of graphene oxide with the rubber matrix has poor controllability, causes great environmental pollution and cannot simultaneously improve the tensile strength, aging resistance and wear resistance of the rubber material.
[0006] In order to achieve the above objectives, the technical solution adopted in this application is:
[0007] The first aspect of the present application provides a filler composition capable of reducing tire rolling resistance, wherein the raw material composition of the filler composition comprises:
[0008] White carbon black; and a modified graphene oxide masterbatch, wherein the modified graphene oxide masterbatch is generated by mixing and heat treating the graphene oxide masterbatch and a polysulfide compound;
[0009] The chemical formula of the polysulfide compound is:
[0010]
[0011] Among them, 2≤n≤5.
[0012] In a preferred embodiment, the mass ratio of the white carbon black to the modified graphene oxide masterbatch is 100:(5-50).
[0013] In a preferred embodiment, when the graphene oxide masterbatch and the polysulfide compound are mixed and heat-treated, the mass ratio of the graphene oxide masterbatch to the polysulfide compound is 100:(0.05-1).
[0014] In a preferred embodiment, the graphene oxide masterbatch comprises natural latex and graphene oxide compounded in the natural latex;
[0015] The mass percentage concentration of the graphene oxide is 5-20wt%.
[0016] In a preferred embodiment, the heat treatment temperature is 80-170° C., and the heat treatment time is 1-8 min.
[0017] The second aspect of the present application provides a low rolling resistance tire rubber material, the raw material composition of the low rolling resistance tire rubber material comprises:
[0018] Tire rubber base;
[0019] Silane coupling agent;
[0020] The filler composition according to any one of claims 1 to 3; and
[0021] Additives available for tire compounds.
[0022] In a preferred embodiment, the mass ratio of the tire rubber base material to the filler composition is 100:(40-70).
[0023] In a preferred embodiment, the additives available for the tire rubber compound include: an antioxidant, a resin, a dispersant and a vulcanization package.
[0024] The third aspect of the present application provides a method for preparing the low rolling resistance tire rubber material of the present application, the preparation method comprising the steps of:
[0025] According to the raw material composition of the tire rubber compound, the raw materials are mixed, kneaded and hot-pressed and vulcanized to obtain the low rolling resistance tire rubber compound.
[0026] A fourth aspect of the present application provides a tire containing the low rolling resistance tire rubber compound of the present application.
[0027] Compared with the prior art, the advantages or beneficial effects of the embodiments of the present application include at least:
[0028] The filler composition provided in the present application is a graphene oxide masterbatch grafted with a polysulfide compound as shown in the chemical formula, and is used in combination with white carbon black. Thanks to the modification of the graphene masterbatch, white carbon black and the graphene oxide masterbatch can be combined through adsorption to block the graphene oxide flakes, thereby inhibiting each other's self-agglomeration and effectively promoting the dispersion of the combined filler in the rubber matrix; on the other hand, the compatibility of graphene oxide with the rubber matrix can be improved, and the polysulfide compound grafted on the graphene oxide can participate in the cross-linking reaction of the rubber, so that the interface bonding between the graphene oxide and the rubber matrix is significantly enhanced; on the third aspect, the amino functional group grafted on the surface of the modified graphene oxide catalyzes the silanization reaction of white carbon black and the silane coupling agent, which can effectively improve the interface between white carbon black and the rubber matrix, thereby effectively improving the reinforcement effect of the combined filler and reducing the rolling resistance of the tread rubber through the synergistic effect of the modified graphene oxide, white carbon black and the silane coupling agent. In addition, the modified graphene oxide masterbatch of the present application does not use organic solvents and the process is controllable, which is easy to mass produce. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments recorded in the present application, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0030] Figure 1 The polysulfide compound S provided in the embodiment of the present application nInfrared spectrum of (n=2). DETAILED DESCRIPTION
[0031] The technical solutions in the embodiments of the present application will be described clearly and completely below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0032] In the following description of this embodiment, the term "and / or" is used to describe the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can represent: A exists alone, B exists alone, and A and B exist at the same time. Among them, A and B can be singular or plural; the single symbol " / " means "or".
[0033] In the following description of this embodiment, the term "at least one" refers to one or more, and "plurality" refers to two or more. "At least one of the following" or similar expressions refer to any combination of these items, including any combination of single items or plural items. For example, "at least one of A, B or C", or "at least one of A, B and C" can represent any one of A, B, C, or A+B, or A+C, or B+C, or A+B+C, where A, B, C can be single or multiple, respectively.
[0034] In the following description of this embodiment, the order of serial numbers does not mean the order of execution. Some or all of the steps can be executed in parallel or sequentially. The execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of this embodiment.
[0035] In the following description of the present embodiment, the numerical range should be understood to also specifically disclose each intermediate value between the upper and lower limits of the range. Any stated value or intermediate value in the stated range and any other stated value or each smaller range between the intermediate values in the stated range are also included in the present embodiment, and the upper and lower limits of the smaller range can be independently included or excluded in the range.
[0036] Unless otherwise stated, the technical / scientific terms used in the present embodiment have the same meanings as those generally understood by those skilled in the art to which the present application belongs. Although the present application only describes preferred methods and materials, any similar or equivalent methods and materials may also be used in the implementation or testing of the present application. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials related to the documents. In the event of any conflict with any incorporated document, the content of this specification shall prevail.
[0037] In a first aspect, the present invention provides a filler composition that can reduce tire rolling resistance. The raw material composition of the filler composition of the present invention comprises:
[0038] White carbon black; and a modified graphene oxide masterbatch, wherein the modified graphene oxide masterbatch is generated by mixing and heat treating the graphene oxide masterbatch and a polysulfide compound;
[0039] The chemical formula of the polysulfide compound is:
[0040]
[0041] Among them, 2≤n≤5.
[0042] It should be noted that the examples of the present application have no restrictions on the specific sources and models of materials such as white carbon black and graphene oxide masterbatch, which can be obtained through commercial channels or synthesized in the laboratory. However, in order to facilitate the implementation of the technical solutions described above in the art, the examples of the present application also provide a method for preparing a polysulfide compound, preferably comprising:
[0043] After the molten sulfur and the vinyl monomer are stirred and reacted for 2 to 8 hours, monosubstituted aniline is added and stirred and reacted for 1 to 4 hours under the protection of an inert gas, and then the reactants are dissolved with tetrahydrofuran, the unreacted sulfur is filtered out, and the filtrate is poured into ethanol for precipitation to obtain a polysulfide compound.
[0044] It should be noted that the embodiments of the present application do not limit the materials, material ratios and related parameters involved in the preparation method. For example, the mass percentages of sulfur, vinyl monomer and mono-substituted aniline may preferably be (50-70%):(10-30%):(20-50%); the vinyl monomer may preferably be one or more of styrene and divinylbenzene; the mono-substituted aniline may preferably be one or more of hydroxyaniline, methylaniline, 4-chloroaniline and m-phenylenediamine.
[0045] As a specific example: 5 g of sulfur was added to a three-necked flask equipped with a mechanical stirrer, heated to 119°C to melt it, and 5 g of hydroxyaniline was added under argon protection, and stirred for 2 hours; after the reaction was completed, the reactant was dissolved in tetrahydrofuran and filtered to remove the unreacted sulfur, and the filtered solution was poured into ethanol to obtain a polysulfide compound S n Its chemical formula is: Among them, n=2.
[0046] In order to test the successful synthesis of polysulfide compound S2, the present application example provides a spectrum of polysulfide compound S2, specifically: Figure 1 shown.
[0047] according to Figure 1 It can be seen that 3357~3459cm -1 The signal peak at 1607cm comes from the NH of the amino group in the polysulfide compound; -1 The signal peak at 1463cm -1 is the vibration peak of the aromatic ring; at 1015cm -1 The absorption peak of the CS bond is at 550cm -1 The absorption peak of SS bond is at , and the results show that the polysulfide compound was successfully prepared.
[0048] The filler composition provided in the present application is a graphene oxide masterbatch grafted with a polysulfide compound as shown in the chemical formula, and is used in combination with white carbon black. Thanks to the modification of the graphene masterbatch, white carbon black and the graphene oxide masterbatch can be combined through adsorption to block the graphene oxide flakes, thereby inhibiting each other's self-agglomeration and effectively promoting the dispersion of the combined filler in the rubber matrix; on the other hand, the compatibility of graphene oxide with the rubber matrix can be improved, and the polysulfide compound grafted on the graphene oxide can participate in the cross-linking reaction of the rubber, so that the interface bonding between the graphene oxide and the rubber matrix is significantly enhanced; on the third aspect, the amino functional group grafted on the surface of the modified graphene oxide catalyzes the silanization reaction of white carbon black and the silane coupling agent, which can effectively improve the interface between white carbon black and the rubber matrix, thereby effectively improving the reinforcement effect of the combined filler and reducing the rolling resistance of the tread rubber through the synergistic effect of the modified graphene oxide, white carbon black and the silane coupling agent. In addition, the modified graphene oxide masterbatch of the present application does not use organic solvents and the process is controllable, which is easy to mass produce.
[0049] In the embodiment of the present application, the mass ratio of the white carbon black to the modified graphene oxide masterbatch can be preferably 100:(5-50), for example, (100:5), (100:10), (100:15), (100:20), (100:25), (100:30), (100:35), (100:40), (100:45), (100:50) or any ratio within the mass ratio range. Among them, the embodiment of the present application can adjust the composition of the filler in the tire rubber composition through the mass ratio, and utilize the synergistic effect of modified graphene and white carbon black to achieve efficient reinforcement, low rolling resistance and high wet skid resistance of the tire rubber. In particular, hybridization of modified graphene and silica can inhibit mutual agglomeration and improve their dispersion in the rubber matrix. At the same time, the polysulfide compound and silane coupling agent grafted onto graphene oxide provide covalent bonding for the interface between graphene, silica and rubber, respectively, and the amino group grafted onto graphene oxide can catalyze the silanization reaction, thereby significantly improving the dynamic properties of the tire rubber composition.
[0050] In the embodiment of the present application, when the graphene oxide masterbatch and the polysulfide compound are mixed and heat treated, the mass ratio of the graphene oxide masterbatch to the polysulfide compound may preferably be 100:(0.05-1), such as (100:0.05), (100:0.1), (100:0.2), (100:0.3), (100:0.5), (100:0.8), (100:1) or any ratio within the mass ratio range. Among them, the embodiment of the present application can achieve efficient reinforcement, low rolling resistance and high wet skid resistance of tire rubber by the mass ratio. In particular, the polysulfide compound and the silane coupling agent grafted onto the graphene oxide provide covalent bonding for the interface between graphene, white carbon black and rubber, respectively, and the amino group grafted onto the graphene oxide can catalyze the silanization reaction, thereby significantly improving the dynamic performance of the tire rubber composition.
[0051] In an embodiment of the present application, the graphene oxide masterbatch comprises natural latex and graphene oxide compounded in the natural latex, and the mass percentage concentration of the graphene oxide may preferably be 5-20wt%, such as 5wt%, 10wt%, 15wt%, 20wt% or any ratio within the mass percentage concentration range. Among them, the embodiment of the present application can improve the dispersion of graphene oxide in the rubber matrix by preparing a masterbatch from graphene oxide through the mass percentage concentration, and at the same time provide a simple and easily scalable processing platform for the thermal reduction treatment of graphene oxide and the modification of polysulfide compounds. In short, by controlling the percentage concentration, a graphene oxide masterbatch with good dispersibility and easy modification can be prepared.
[0052] It should be noted that the present application embodiment does not limit the preparation method of the graphene oxide masterbatch, and the synthesis can be carried out according to the steps disclosed in the art. To facilitate the implementation of the technical solution of the present application in the art, the present application provides an example preparation of a graphene oxide masterbatch, which specifically includes:
[0053] The graphene oxide aqueous dispersion is added to the natural rubber latex and stirred to mix evenly, the stirring rate is 100-500r / min, and a 2-8wt% calcium chloride aqueous solution is sprayed at a spraying flow rate of 0.5-3L / min. After the spraying is completed, the mixed solution is flocculated and dried to obtain a graphene oxide masterbatch. The amount of the graphene oxide aqueous dispersion added is calculated based on the mass percentage concentration of the graphene oxide equivalent to 5-20wt% of the natural rubber latex.
[0054] As a specific example: the graphene oxide dispersion is ultrasonically treated (power is 70kw, time is 20min), and then the natural latex NR is pumped into the ultrasonically treated graphene oxide dispersion at a stirring rate of 100r / min and stirred and mixed, and then an 8wt% calcium chloride aqueous solution is sprayed at a flow rate of 2L / min. The mixed solution of natural latex NR and graphene oxide is flocculated to obtain a brown slurry, and the brown slurry is pumped into a centrifugal speed of 1900r / min for 20min to obtain a blocky brown solid; the brown solid is dried at a temperature of 40°C for 36h to obtain a graphene oxide masterbatch GO / NR. Wherein, the mass percentage concentration of the graphene oxide relative to the natural latex NR is 10wt%.
[0055] The preparation process of modified graphene oxide masterbatch includes:
[0056] Polysulfide S n Add the graphene oxide masterbatch GO / NR into an internal mixer and mix them for heat treatment to obtain the modified graphene masterbatch S n -GO / NR. The mixed heat treatment temperature is 80-170°C, and the heat treatment time is 1-8 min. In the exemplary description, the heat treatment temperature is 80°C, and the time is 1 min, 3 min, 8 min; or, the heat treatment temperature is 150°C, and the time is 1 min, 3 min, 8 min; or, the heat treatment temperature is 170°C, and the time is 1 min, 3 min, 8 min.
[0057] In a second aspect, the embodiment of the present application provides a low rolling resistance tire rubber material. The raw material composition of the low rolling resistance tire rubber material of the embodiment of the present application comprises:
[0058] Tire rubber base;
[0059] Silane coupling agent;
[0060] The filler composition described hereinabove; and
[0061] Additives available for tire compounds.
[0062] It should be noted that the tire rubber base material can be various general tire rubbers in the art, and the example is described as a mixture of natural rubber and solution polymerized styrene butadiene rubber. Wherein, the mass ratio of natural rubber to solution polymerized styrene butadiene rubber can be preferably (10-40): (60-90), such as (10:90), (20:80), (30:70), (40:60), etc. In order to obtain a tire rubber with excellent comprehensive performance, preferably solution polymerized styrene butadiene rubber / natural rubber = 70 / 30. Of course, other general tire rubbers can also be used, and the embodiments of the present application are not described in detail one by one.
[0063] In the embodiment of the present application, the mass ratio of the tire rubber base material to the filler composition may preferably be 100:(40-70), for example, (100:40), (100:45), (100:50), (100:55), (100:60), (100:65), (100:70). Wherein, the embodiment of the present application can prepare a tire rubber composition with practical performance by controlling the mass ratio above. By adjusting the amount and composition of the filler in the tire rubber composition, the modified graphene oxide and white carbon black can produce a synergistic effect to achieve efficient reinforcement, low rolling resistance and high wet skid resistance of the tire rubber. In particular, hybridization of modified graphene and silica can inhibit mutual agglomeration and improve their dispersion in the rubber matrix. At the same time, the polysulfide compound and silane coupling agent grafted onto graphene oxide provide covalent bonding for the interface between graphene, silica and rubber, respectively, and the amino group grafted onto graphene oxide can catalyze the silanization reaction, thereby significantly improving the dynamic properties of the tire rubber composition.
[0064] In the embodiment of the present application, the auxiliary agent available for the tire rubber material refers to various auxiliary agents commonly used in tire rubber materials, and may include antioxidants, resins, dispersants, and vulcanization packages. Wherein, the specific sources, compositions, and dosages of antioxidants, resins, dispersants, and vulcanization packages are not limited in the embodiment of the present application. As an example description, the antioxidant may be one or both of antioxidants RD and 6PPD, and the mass ratio of the antioxidant to the tire rubber base material is (1-3): 100; the dispersant may be dispersant TDAE (environmentally friendly aromatic oil / rubber filler oil), and the mass ratio of the dispersant to the tire rubber base material is (2-5): 100; the resin may be a common additive for tire rubber materials, and may be one or more of phenolic resins, C5 resins, coumarone-indene resins, styrene resins, and terpene resins, and the mass ratio of the resin to the tire rubber base material is (4-18): 100. Of course, the embodiment of the present application does not limit the specific auxiliary agent type, auxiliary agent composition, and dosage, and is subject to the general use in the art.
[0065] In the embodiment of the present application, the material composition of the vulcanization package includes stearic acid, zinc oxide, accelerator and sulfur. Wherein, the accelerator can be preferably one or two of accelerator NS and accelerator DPG. The amount of the vulcanization package added is (0.6-2.4) according to the mass ratio of accelerator, stearic acid, zinc oxide and tire rubber base material: (1-4): (3.5-5.5): 100. In addition, in order to improve the performance improvement effect of the filler composition of the present application on the tire rubber base material, the mass ratio of silane coupling agent to tire rubber base material is (3-8): 100. Of course, the specific source and model of the silane coupling agent are not limited in the embodiment of the present application, and various silane coupling agents known in the art can be used.
[0066] In a third aspect, the present application also provides a method for preparing the low rolling resistance tire rubber material of the present application, and the method preferably comprises:
[0067] According to the raw material composition of the tire rubber compound, the raw materials are mixed, kneaded and hot-pressed and vulcanized to obtain the low rolling resistance tire rubber compound.
[0068] In a preferred implementation process, the filler composition, tire rubber base material and silane coupling agent can be first mixed in an internal mixer to form a rubber mix, and then the rubber mix is transferred to an open mixer to add additives including but not limited to zinc oxide, stearic acid, accelerators and sulfur, and after standing for 24 hours, a low rolling resistance tire rubber is prepared by hot pressing vulcanization. Among them, the mixing temperature can be preferably 80-170°C and the time is 1-8 minutes.
[0069] In a fourth aspect, the embodiment of the present application provides a tire containing the low rolling resistance tire rubber material of the embodiment of the present application. In particular, since the filler composition of the embodiment of the present application can effectively improve the reinforcement effect and reduce the rolling resistance of the tread rubber, the tire of the embodiment of the present application has excellent dynamic service performance such as low rolling resistance, low heat generation, and anti-slip.
[0070] The technical solution of the present application will be further described below in conjunction with specific embodiments.
[0071] Example 1
[0072] This embodiment provides a filler composition S2-GO / NR-white carbon black, the raw material composition of which includes:
[0073] 100 g of white carbon black; and,
[0074] 30 g of modified graphene oxide masterbatch S2-GO / NR;
[0075] The preparation process of the filler composition S2-GO / NR-white carbon black includes:
[0076] The graphene oxide masterbatch GO / NR prepared above and the polysulfide compound S2 were added into an internal mixer at a mass ratio of 100:0.5, mixed and heat treated at a temperature of 150°C for 3 minutes to obtain a modified graphene oxide masterbatch S2-GO / NR;
[0077] The modified graphene oxide masterbatch S2-GO / NR and white carbon black are stirred and mixed to obtain a filler composition S2-GO / NR-white carbon black.
[0078] Example 2
[0079] This embodiment provides a tire rubber material TYRE, the raw material composition of which is:
[0080] Natural rubber NR 30g, styrene-butadiene rubber SSBR 70g, antioxidant 6PPD 2g, RD 2g, silane coupling agent KH5505g, styrene resin 12g, dispersant TDAE 3g, stearic acid 4.5g, zinc oxide 2g, accelerator NS 1.8g, accelerator DPG 1.5g, sulfur 1.8g and S2-GO / NR-white carbon black 40g;
[0081] The specific preparation process includes:
[0082] The natural rubber NR, styrene-butadiene rubber SSBR, S2-GO / NR-white carbon black, silane coupling agent, resin, dispersant and antioxidant in the stated mass parts are added into an internal mixer, and are internally mixed at a temperature of 150° C. for 3 minutes to obtain a rubber mixture; the rubber mixture is added into an open mixer, and stearic acid, zinc oxide, an accelerator and sulfur are added at room temperature, and hot-press vulcanization is performed to obtain a tire rubber compound TYRE-1.
[0083] Example 3
[0084] This embodiment provides a tire rubber material TYRE-2, the raw material composition of which is:
[0085] Natural rubber NR 30g, styrene-butadiene rubber SSBR 70g, antioxidant 6PPD 2g, RD 2g, silane coupling agent KH5505g, styrene resin 12g, dispersant TDAE 3g, stearic acid 4.5g, zinc oxide 2g, accelerator NS 1.8g, accelerator DPG 1.5g, sulfur 1.8g and S2-GO / NR-white carbon black 50g;
[0086] The specific preparation process includes:
[0087] The natural rubber NR, styrene-butadiene rubber SSBR, S2-GO / NR-white carbon black, silane coupling agent, resin, dispersant and antioxidant in the stated mass parts are added into an internal mixer, and are internally mixed at a temperature of 150° C. for 3 minutes to obtain a rubber mixture; the rubber mixture is added into an open mixer, and stearic acid, zinc oxide, an accelerator and sulfur are added at room temperature and hot-press vulcanization is performed to obtain a tire rubber compound TYRE-2.
[0088] Example 4
[0089] This embodiment provides a tire rubber material TYRE-3, the raw material composition of which is:
[0090] Natural rubber NR 30g, styrene-butadiene rubber SSBR 70g, antioxidant 6PPD 2g, RD 2g, silane coupling agent KH5505g, styrene resin 12g, dispersant TDAE 3g, stearic acid 4.5g, zinc oxide 2g, accelerator NS 1.8g, accelerator DPG 1.5g, sulfur 1.8g and S2-GO / NR-white carbon black 60g;
[0091] The specific preparation process includes:
[0092] The natural rubber NR, styrene-butadiene rubber SSBR, S2-GO / NR-white carbon black, silane coupling agent, resin, dispersant and antioxidant in the stated mass parts are added into an internal mixer, and are internally mixed at a temperature of 150° C. for 3 minutes to obtain a rubber mixture; the rubber mixture is added into an open mixer, and stearic acid, zinc oxide, an accelerator and sulfur are added at room temperature, and hot-press vulcanization is performed to obtain a tire rubber compound TYRE-3.
[0093] Example 5
[0094] This embodiment provides a tire rubber material TYRE-4, the raw material composition of which is:
[0095] Natural rubber NR 30g, styrene-butadiene rubber SSBR 70g, antioxidant 6PPD 2g, RD 2g, silane coupling agent KH5505g, styrene resin 12g, dispersant TDAE 3g, stearic acid 4.5g, zinc oxide 2g, accelerator NS 1.8g, accelerator DPG 1.5g, sulfur 1.8g and S2-GO / NR-white carbon black 70g;
[0096] The specific preparation process includes:
[0097] The natural rubber NR, styrene-butadiene rubber SSBR, S2-GO / NR-white carbon black, silane coupling agent, resin, dispersant and antioxidant in the stated mass parts are added into an internal mixer, and are internally mixed at a temperature of 150° C. for 3 minutes to obtain a rubber mixture; the rubber mixture is added into an open mixer, and stearic acid, zinc oxide, an accelerator and sulfur are added at room temperature and hot-press vulcanization is performed to obtain a tire rubber compound TYRE-4.
[0098] The present application conducts static and dynamic performance tests on the tire rubber prepared in Examples 2-5. Among them, the tensile strength, elongation at break and 300% tensile stress are based on the measurement standard of IS037-2005, the test temperature is room temperature, and the tensile rate is 500mm / min. The dynamic performance test conditions are: in the tensile mode, the temperature is -100℃~100℃, the heating rate is 3℃ / min, the frequency is 1Hz, the dynamic strain is 0.5%, and the tanδ at 0℃ is measured; the temperature is -10℃~100℃, the heating rate is 3℃ / min, the frequency is 10Hz, the dynamic strain is 5%, and the tanδ at 60℃ is measured. The compression heat generation test conditions are: temperature 50℃, frequency 10Hz, prestress 1MPa. The measurement results are shown in Table 1.
[0099] Table 1: Performance test results of tire rubber materials in the examples
[0100] TYRE-1 TYRE-2 TYRE-3 TYRE-4 Tensile strength(MPa) 17.4 20.1 23.8 22.8 300% modulus (MPa) 8.4 10.2 13.4 12.6 Elongation at break (%) 451 467 478 470 0℃tanδ(loss factor) 0.88 0.87 0.96 0.95 60℃tanδ(loss factor) 0.147 0.133 0.084 0.102 Compression fatigue heat generation (℃) 22.1 20.5 15.6 18.5
[0101] According to Table 1, adding filler composition can effectively improve wet skid resistance (tanδ at 0℃ increased) and rolling resistance (tanδ at 60℃ decreased), reduce compression heat generation, and improve dynamic service performance. In addition, the filler content of TYPE1-2 is too low to meet the mechanical performance requirements of the tread rubber. The filler content of TYPE4 is too high, and the interaction between the fillers exceeds the dispersing effect of the polysulfide compound, resulting in agglomeration, so all performances are inferior to TYPE3. Overall, the performance of TYPE3 (Example 4) is the best.
[0102] In order to illustrate the actual effect of the filler composition of the present application, the present application uses Example 4 with the best filler addition amount screened as the experimental group, and provides Comparative Examples 1-3 for comparison. Among them:
[0103] The difference between Comparative Example 1 and Example 4 is that the added filler S2-GO / NR-white carbon black is replaced by GO / NR-white carbon black (graphene oxide and white carbon black are mixed and heat-treated in a mass ratio of 50:100), and the remaining components and preparation process are the same as those in Example 4.
[0104] The difference between Comparative Example 2 and Example 4 is that the silane coupling agent KH550 is omitted, and the remaining components and the preparation process are the same as those of Example 4.
[0105] The difference between Comparative Example 3 and Example 4 is that the added filler S2-GO / NR-white carbon black is replaced by S2-GO / NR (that is, the filler composition does not contain white carbon black), and the other components and preparation process are the same as Example 4.
[0106] The tire rubber materials prepared in Comparative Examples 1-3 were subjected to performance tests, and the results are shown in Table 2.
[0107] Table 2: Performance test results of tire rubber materials prepared in Example 4 and Comparative Examples 1-3
[0108] Example 4 Comparative Example 1 Comparative Example 2 Comparative Example 3 Tensile strength(MPa) 23.8 21.5 22.2 23.5 300% modulus (MPa) 13.4 11.4 15.2 6.3 Elongation at break (%) 478 453 404 895 0℃tanδ(loss factor) 0.95 0.084 0.081 0.069 60℃tanδ(loss factor) 0.084 0.107 0.105 0.021 Compression fatigue heat generation (℃) 15.6 18.8 19.7 10.4
[0109] According to Table 2, the present embodiment of the present invention has better anti-skid performance (higher 0°C tanδ), lower rolling resistance (lower 60°C tanδ), excellent dynamic service performance, and better mechanical properties by using a combination of polysulfide compounds and coupling agents compared to Comparative Examples 1 and 2. If the polysulfide compound (Comparative Example 1) is not added, the graphene cannot be well dispersed, resulting in an insignificant reinforcement effect, high compression heat generation and rolling resistance of the rubber, and poor mechanical properties.
[0110] If the silane coupling agent is not added (Comparative Example 2), the agglomeration of the white carbon black filler will be more serious, the compression heat generation and rolling resistance of the rubber compound will be too high, while the elongation at break will be too low, and the mechanical properties and dynamic service performance will be poor.
[0111] Without adding silica filler, although the compression fatigue heat generation and rolling resistance (60℃tanδ) are the lowest, the modulus of the rubber compound is too low to meet the requirements of the tread rubber compound, and the anti-skid performance (0℃tanδ) is low and the dynamic service performance is poor.
[0112] The examples of the present application also study the effects of mixing temperature and time on tire rubber properties. The specific mixing and time settings are shown in Table 3.
[0113] Table 3: Mixing temperature and time
[0114]
[0115] The present application tests the performance of tire rubber compounds prepared under different mixing conditions, and the results are shown in Table 4.
[0116] Table 4: Performance test results of tire rubber compounds prepared under different mixing conditions
[0117]
[0118] According to Table 4, the tensile strength, 300% modulus and elongation at break of the rubber at 180°C are lower than those at 80°C and 150°C. When the temperature is too high, the molecular chain of natural rubber will age and degrade, thus affecting the tensile strength, modulus and elongation at break of the sample. When the temperature is too low, the modification efficiency of polysulfide compounds is not high, and the dispersibility and interfacial effect of graphene oxide are not as good as at higher temperatures.
[0119] At 180°C, due to the long heat treatment time, the rubber molecular chains in the masterbatch are cracked, and the various properties after heat treatment for 8 minutes are significantly deteriorated. At 80°C, the rubber prepared by the modified graphene oxide masterbatch does not change much with the extension of the heat treatment time, indicating that the reaction rate of polysulfide compounds is low at this temperature, so extending the modification time has little effect. The "150°C heat treatment for 3 minutes" process used in Example 5 has the lowest compression fatigue heat generation, the lowest rolling resistance (tan@60°C) and the highest wet skid resistance (tan@0°C).
[0120] Therefore, in summary, the tread compound designed with modified graphene oxide masterbatch obtained by heat treatment at 150°C for 3 min has better mechanical properties and dynamic service performance as well as lower fatigue temperature rise.
[0121] The present application also studies the effect of the mass ratio of modified graphene oxide masterbatch and white carbon black in the filler composition on the performance of the tire rubber compound. Specifically, Example 4 is used as the experimental group, and the modified graphene oxide masterbatch S in the filler composition is adjusted. n -GO / NR and silica mass ratio, and the properties of the obtained tire rubber compound were tested. The results are shown in Table 5.
[0122] Table 5: Different silica and S n -Tire compound performance under GO / NR ratio
[0123] 100:5 100:10 100:20 100:30 100:40 100:50 100:55 Tensile strength(MPa) 15.2 15.6 23.2 22.8 15.9 15.4 14.4 300% modulus (MPa) 14.8 13.4 13.8 13.4 11.5 10.8 9.5 Elongation at break (%) 305 326 344 478 412 438 443 0℃tanδ(loss factor) 0.92 0.94 0.93 0.95 0.94 0.82 0.76 60℃tanδ(loss factor) 0.131 0.114 0.102 0.084 0.079 0.076 0.081 Compression fatigue heat generation (℃) 26.5 22.4 18.7 15.6 14.8 14.6 14.6
[0124] According to Table 5, as the proportion of white carbon black in the filler composition increases, although the anti-skid ability of the rubber is better, the rolling resistance and compression heat generation performance are both higher. At the same time, the elongation at break of the rubber becomes shorter and the mechanical properties become worse.
[0125] As the proportion of modified graphene oxide masterbatch increases, although the compression fatigue heat generation and rolling resistance of the rubber are reduced, as the natural rubber content increases, the anti-skid ability and mechanical properties of the rubber deteriorate.
[0126] In summary, the modified graphene oxide masterbatch S in the filler composition n -The performance of the rubber compound is best when the mass ratio of GO / NR and silica is 100:30.
[0127] The various embodiments in this specification are described in a progressive manner, and the same or similar parts between the various embodiments can be referenced to each other, and each embodiment focuses on the differences from other embodiments.
[0128] The above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit the present application. Although the present application has been described in detail with reference to the aforementioned embodiments, a person of ordinary skill in the art should understand that the technical solutions recorded in the aforementioned embodiments may still be modified, or some or all of the technical features therein may be replaced by equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the present application.
Claims
1. A filler composition capable of reducing tire rolling resistance, characterized in that: The raw material composition includes: Silica; and A modified graphene oxide masterbatch, wherein the modified graphene oxide masterbatch is produced by mixing and heat treating the graphene oxide masterbatch and a polysulfide compound; The chemical formula of the polysulfide compound is: Among them, 2≤n≤5.
2. The filler composition according to claim 1, characterized in that The mass ratio of the white carbon black to the modified graphene oxide masterbatch is 100:(5-50).
3. The filler composition according to claim 1, characterized in that When the graphene oxide masterbatch and the polysulfide compound are mixed and heat-treated, the mass ratio of the graphene oxide masterbatch to the polysulfide compound is 100:(0.05-1).
4. The filler composition according to claim 1, characterized in that The graphene oxide masterbatch comprises natural latex and graphene oxide compounded in the natural latex; The mass percentage concentration of the graphene oxide is 5-20wt%.
5. The filler composition according to claim 1, characterized in that The heat treatment temperature is 80-170° C., and the heat treatment time is 1-8 minutes.
6. A low rolling resistance tire rubber compound, characterized in that: The raw material composition includes: Tire rubber base; Silane coupling agent; The filler composition according to any one of claims 1 to 3; and Additives available for tire compounds.
7. The low rolling resistance tire rubber material according to claim 6, characterized in that: The mass ratio of the tire rubber base material to the filler composition is 100:(40-70).
8. The low rolling resistance tire rubber material according to claim 6, characterized in that: The additives available for the tire rubber compound include: antioxidant, resin, dispersant and vulcanization package.
9. A method for preparing a low rolling resistance tire rubber compound according to any one of claims 6 to 8, characterized in that the steps include: According to the raw material composition of the tire rubber compound, the raw materials are mixed, kneaded and hot-pressed and vulcanized in sequence to obtain the low rolling resistance tire rubber compound.
10. A tire, characterized in that: Contains the low rolling resistance tire rubber material according to any one of claims 6-8.
Citation Information
Patent Citations
Tire tread rubber composition and preparation method thereof
CN109081961A
Tire with component comprised of rubber composition containing silica and graphene platelet reinforcement
US20140155544A1
Preparation of rubber reinforced with at least one of graphene and carbon nanotubes with specialized coupling agent and tire with component
US20150018481A1
Cited By
Non-tread formula for improving rolling resistance performance of tire
CN119144059A
A non-tread formulation for improving tire rolling resistance performance
CN119144059B