Coating composition

By designing the structure with adhesive layer and hard coating in the laminate, using adhesive emulsion particles, inorganic oxides and sunscreens, combined with polymer nanoparticles, the wear resistance of water-based coatings and hard coating films is solved by using adhesive emulsion particles, inorganic oxides and sunscreens. The deficiencies in dissipation and optical characteristics have achieved a laminate with high wear resistance and optical characteristics.

CN118909504APending Publication Date: 2024-11-08ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411172149.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2020-03-04
Filing Date
2021-03-04
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the prior art, water-based coatings are difficult to show high levels of wear resistance and optical properties, and hard coated coatings are difficult to maintain weather resistance and durability when exposed to ultraviolet rays for a long time.

Method used

A laminated structure with an adhesive layer, wherein the adhesive layer contains adhesive emulsion particles, inorganic oxides and sunscreens, and a hard coat layer contains matrix components containing inorganic oxides and polymer nanoparticles, by optimizing the layer The haze, surface roughness and distribution of polymer nanoparticles improve their wear resistance and optical properties.

Benefits of technology

Laminated bodies with high wear resistance, adhesion and optical properties are achieved, suitable for a variety of dura film applications, especially in automotive parts and electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005009607060001201
    Figure BDA0005009607060001201
  • Figure BDA0005009607060001211
    Figure BDA0005009607060001211
  • Figure BDA0005009607060001221
    Figure BDA0005009607060001221
Patent Text Reader

Abstract

The invention relates to a coating composition. The coating composition comprises: a mixture of adhesive emulsion particles (F) and an inorganic oxide (G) and / or a composite of the inorganic oxide (G) and the adhesive emulsion particles (F); an opacifier (S1); and an isocyanate compound, in which the average particle diameter of the mixture and / or composite is 2-2000 nm, the mass ratio of the inorganic oxide (G) to the adhesive emulsion particles (F) is 1: 0.1-1: 10, and the inorganic oxide (G) is silicon oxide having a spherical and / or linked structure.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application. The international application number of the original application is PCT / JP2021 / 008553, the international application date is March 4, 2021, the Chinese national application number is 202180016893.7, the date of entry into China is August 25, 2022, and the name of the invention is "Laminate, hard coating film and coating composition". Technical Field

[0002] The present invention relates to a laminate, a hard coating film and a coating composition. Background Art

[0003] (First Background Art)

[0004] The film formed by drying the aqueous dispersion obtained by polymerization at room temperature or under heating has a tendency to show barrier properties, pollution resistance, chemical resistance, flame retardancy, heat resistance, weather resistance, scratch resistance, and abrasion resistance, so the aqueous dispersion is used as a water-based paint. When such a water-based paint is used for purposes requiring transparency, due to long-term exposure to outdoor or ultraviolet rays, the optical properties such as transparency or blur, discoloration, whitening, and the generation of cracks may become a problem. In addition, when the paint is used as a topcoat, abrasion resistance is required for the topcoat. From the aspect of abrasion resistance, solvent-based paint is sometimes used. For this solvent-based paint, it is relatively easy to contain an organic sunscreen while maintaining the properties of the paint or the obtained film. However, out of consideration for the hygienic state of the work site and the load on the earth's environment, it is desired to use a water-based paint.

[0005] As a technology for improving the optical properties of water-based coatings, Patent Document 1 describes a method of including an ultraviolet absorber in polymerization for the purpose of imparting weather resistance. In addition, Patent Document 2 describes a method of dissolving an ultraviolet absorber and including it in a film-forming aid component. In addition, as a technology for imparting hard coating properties to a resin material, a method of adding an inorganic oxide to a resin material is described (for example, see Patent Documents 3 and 4).

[0006] (Second Background Art)

[0007] Resin materials are excellent in formability and lightness, but in most cases, they are inferior to inorganic materials such as metals and glass in hardness, barrier properties, stain resistance, chemical resistance, flame retardancy, heat resistance, and weather resistance. Among them, the hardness of resin materials is significantly lower than that of inorganic glass, and the surface is easily damaged, so they are often used with a hard coat. However, hard coats have difficulty maintaining stain resistance against coal dust and the like and performance under high temperature and high humidity, and have difficulty maintaining appearance when exposed to ultraviolet rays for a long time. Resin materials with a hard coat cannot be used for applications that require high wear resistance, durability, and weather resistance.

[0008] In order to impart wear resistance to resin materials, a method of using an active energy ray-curable resin composition (see, for example, Patent Document 5), a method of adding an inorganic oxide to a resin material (see, for example, Patent Document 3 and Patent Document 6), and a method of adding polymer particles to a resin material (see, for example, Patent Document 7) have been proposed. In addition, in order to impart weather resistance to a resin material, a scheme of using an acrylic polymer and cerium oxide in combination has been proposed (see, for example, Patent Document 8).

[0009] Prior art literature

[0010] Patent Literature

[0011] Patent Document 1: Japanese Patent Application Laid-Open No. 11-12505

[0012] Patent Document 2: Japanese Patent Application Laid-Open No. 7-173404

[0013] Patent Document 3: Japanese Patent Application Publication No. 2006-63244

[0014] Patent Document 4: Japanese Patent Application Laid-Open No. 8-238683

[0015] Patent Document 5: Japanese Patent Application Publication No. 2014-109712

[0016] Patent Document 6: Japanese Patent Application Laid-Open No. 8-238683

[0017] Patent Document 7: Japanese Patent Application Publication No. 2017-114949

[0018] Patent Document 8: Japanese Patent Application Laid-Open No. 5-339400 Summary of the invention

[0019] Problems to be solved by the invention

[0020] (Topic 1)

[0021] The methods of Patent Documents 1 and 2 are common methods for imparting weather resistance to water-based coatings, but the amount of ultraviolet absorber that can be contained in the coating film is small, making it difficult to impart high weather resistance. In addition, the coating film disposed on the substrate has insufficient adhesion.

[0022] The methods of Patent Documents 3 and 4 are common methods for imparting abrasion resistance to resin materials, but they use solvent-based paints and are not easily applicable to water-based paints.

[0023] As described above, substrates with coating films obtained from water-based coating materials in the prior art still have room for improvement in terms of high abrasion resistance and optical properties.

[0024] The present invention has been made in view of the above-mentioned problems, and a first object of the present invention is to provide a laminate having high abrasion resistance, adhesion, and optical properties.

[0025] (Topic 2)

[0026] The methods of Patent Documents 5 and 3 are common methods for imparting wear resistance to resin materials, but it is difficult to impart high wear resistance.

[0027] The method of Patent Document 6 is a common method of using a soft silicone polymer and hard inorganic oxide fine particles as a hard coating film. However, the silicone polymer corresponding to the matrix component does not have sufficient hardness, so the wear resistance is insufficient.

[0028] The method of Patent Document 7 is a method using polymer particles, silicone polymers, and inorganic oxide microparticles as a hard coating film. Although the physical properties of the coating film are described, the physical properties of each component are not described, the wear resistance is insufficient, and the contamination resistance is not described.

[0029] According to Patent Document 8, although a certain degree of improvement is observed in weather resistance, it cannot be said to be a sufficient level from the perspective of the balance of physical properties in terms of wear resistance and durability.

[0030] As described above, conventional hard coating films still have room for improvement in terms of high abrasion resistance, durability, and weather resistance.

[0031] The present invention has been made in view of the above problems, and a second object of the present invention is to provide a hard coating film having high abrasion resistance, durability and weather resistance, a substrate with a hard coating film, a coating composition and a window material.

[0032] Means for solving problems

[0033] The present inventors have conducted intensive studies and have found that the above-mentioned problems can be solved by forming a laminate having a substrate with a specific adhesive layer and a hard coat layer, thereby completing the present invention.

[0034] That is, the present invention includes the following aspects. [1]

[0036] A laminate comprising:

[0037] A substrate with an adhesive layer, comprising a substrate and an adhesive layer, wherein the adhesive layer is disposed on the substrate and comprises adhesive emulsion particles (F), an inorganic oxide (G) and a light shielding agent (S1); and

[0038] a hard coating layer (C) disposed on the substrate with the adhesive layer and comprising a matrix component (B) containing an inorganic oxide (D),

[0039] The haze value H1 of the adhesive layer-attached substrate is greater than the haze value H2 of the laminate. [2]

[0041] The laminate as described in [1], wherein the H2 is 5% or less. [3]

[0043] A laminate comprising:

[0044] A substrate with an adhesive layer, comprising a substrate and an adhesive layer, wherein the adhesive layer is disposed on the substrate and comprises adhesive emulsion particles (F), an inorganic oxide (G) and a light shielding agent (S1); and

[0045] a hard coating layer (C) disposed on the substrate with the adhesive layer and comprising a matrix component (B) containing an inorganic oxide (D),

[0046] The surface roughness Ra1 of the adhesive layer-attached substrate is greater than the surface roughness Ra2 of the laminate. [4]

[0048] The laminate as described in [3], wherein the Ra1 is 10 to 500 nm. [5]

[0050] The laminate as described in [3] or [4], wherein the above-mentioned Ra2 is less than 100 nm. [6]

[0052] The laminate according to any one of [1] to [5], wherein the light-shielding agent (S1) contains an ultraviolet absorber. [7]

[0054] The laminate according to any one of [1] to [6], wherein the adhesive layer further contains a hindered amine light stabilizer. [8]

[0056] The laminate according to any one of [1] to [7], wherein

[0057] The hard coating layer (C) further comprises polymer nanoparticles (A) dispersed in the matrix component (B),

[0058] The Martens hardness HM of the polymer nanoparticles (A) is A The Martens hardness HM of the matrix component (B) B Meet HM B / HM A >1 relationship,

[0059] The Martens hardness HM of the hard coating is 100N / mm 2 above. [9]

[0061] The laminate as described in [8], wherein the average particle size of the polymer nanoparticles (A) is from 10 nm to 400 nm.

[10]

[0063] The laminate as described in [8] or [9], wherein the volume fraction of the polymer nanoparticles (A) in the hard coat layer (C) is 2% to 80%.

[11]

[0065] The laminate according to any one of [8] to

[10] , wherein

[0066] The polymer nanoparticles (A) contain a hydrolyzable silicon compound (a),

[0067] The content of the hydrolyzable silicon compound (a) in the polymer nanoparticles (A) is 50% by mass or more.

[12]

[0069] A laminate as described in

[11] , wherein the hydrolyzable silicon compound (a) comprises one or more selected from compounds containing an atomic group represented by the following formula (a-1), their hydrolysis products and condensation products, and compounds represented by the following formula (a-2), their hydrolysis products and condensation products.

[0070] -R 1 n1 SiX 1 3-n1 (a-1)

[0071] (In formula (a-1), R 1 represents a hydrogen atom, an alkyl group, an alkenyl group, an alkynyl group or an aryl group having 1 to 10 carbon atoms, and R 1 It may have a substituent containing a halogen, hydroxyl, mercapto, amino, (meth)acryloyl or epoxy group, X 1 represents a hydrolyzable group, and n1 represents an integer of 0 to 2. )

[0072] SiX 2 4(a-2)

[0073] (In formula (a-2), X 2 represents a hydrolyzable group. )

[13]

[0075] The laminate as described in any one of [1] to

[12] , wherein the inorganic oxide (D) contains at least one inorganic component selected from the group consisting of Ce, Nb, Al, Zn, Ti, Zr, Sb, Mg, Sn, Bi, Co and Cu.

[14]

[0077] The laminate according to any one of [1] to

[13] , wherein the hard coat layer (C) further contains a light shielding agent (S2).

[15]

[0079] The laminate according to any one of [1] to

[14] , wherein the inorganic oxide (G) is silicon oxide having a spherical structure and / or a linked structure.

[16]

[0081] The laminate according to any one of [1] to

[15] , wherein the adhesive layer comprises a composite of the inorganic oxide (G) and the adhesive emulsion particles (F).

[17]

[0083] A laminate as described in any one of [1] to

[16] , wherein the average particle size of at least one selected from the group consisting of the above-mentioned inorganic oxide (G), the above-mentioned adhesive emulsion particles (F), and a composite of the above-mentioned inorganic oxide (G) and the above-mentioned adhesive emulsion particles (F) is greater than 2 nm and less than 400 nm.

[18]

[0085] The laminate according to any one of [1] to

[17] , wherein the mass ratio of the inorganic oxide (G) to the adhesive emulsion particles (F) is 1:0.1 to 1:10.

[19]

[0087] The laminate according to any one of [1] to

[18] , wherein the adhesive layer further contains an isocyanate compound and / or a urethane compound.

[20]

[0089] A laminate as described in any one of [1] to

[19] , wherein when the hard coating layer is subjected to a Taber abrasion test under the conditions of a wear wheel CS-10F and a load of 500 g according to ASTM D1044, the difference between the haze at a rotation speed of 500 times and the haze before the Taber abrasion test is 10 or less. [twenty one]

[0091] A laminate as described in any one of [1] to

[20] , wherein when the hard coating layer is subjected to a Taber abrasion test under the conditions of a wear wheel CS-10F and a load of 500 g according to ASTM D1044, the difference between the haze at a rotation speed of 1000 times and the haze before the Taber abrasion test is 10 or less. [twenty two]

[0093] The laminate according to any one of [1] to

[21] , wherein the elastic recovery rate η of the hard coating layer measured by an indentation test in accordance with ISO14577-1 is IT It is above 0.50. [twenty three]

[0095] The laminate according to any one of [1] to

[22] , wherein the hard coat layer has a thickness of 1 μm to 100 μm. [twenty four]

[0097] The laminate according to any one of [1] to

[23] , wherein the matrix component (B) contains a hydrolyzable silicon compound (b).

[25]

[0099] A laminate as described in

[24] , wherein the hydrolyzable silicon compound (b) comprises one or more selected from compounds containing an atomic group represented by the following formula (b-1), their hydrolysis products and condensation products, and compounds represented by the following formula (b-2), their hydrolysis products and condensation products.

[0100] -R 2 n2 SiX 3 3-n2 (b-1)

[0101] (In formula (b-1), R 2 represents a hydrogen atom, an alkyl group, an alkenyl group, an alkynyl group or an aryl group having 1 to 10 carbon atoms, and R 2 It may have a substituent containing a halogen, hydroxyl, mercapto, amino, (meth)acryloyl or epoxy group, X 3 represents a hydrolyzable group, and n2 represents an integer of 0 to 2. )

[0102] SiX 4 4(b-2)

[0103] (In formula (b-2), X 4 represents a hydrolyzable group. )

[26]

[0105] The laminate according to any one of [1] to

[25] , wherein the average particle size of the inorganic oxide (D) is 2 nm or more and 150 nm or less.

[27]

[0107] The laminate according to any one of [1] to

[26] , wherein the inorganic oxide (D) is silicon oxide particles.

[28]

[0109] The laminate according to any one of [1] to

[27] , which is a laminate for automobile parts.

[29]

[0111] A coating composition comprising:

[0112] A mixture of adhesive latex particles (F) and an inorganic oxide (G) and / or a complex of the inorganic oxide (G) and the adhesive latex particles (F); and

[0113] Sunscreen (S1),

[0114] in,

[0115] The average particle size of the mixture and / or composite is 2 nm or more and 2000 nm or less.

[0116] The mass ratio of the inorganic oxide (G) to the adhesive latex particles (F) is 1:0.1 to 1:10.

[30]

[0118] The coating composition as described in

[29] , wherein the sunscreen (S1) contains an ultraviolet absorber.

[31]

[0120] The coating composition according to any one of

[29] or

[30] , further comprising a hindered amine light stabilizer.

[32]

[0122] The coating composition according to any one of

[29] to

[31] , wherein the inorganic oxide (G) is spherical and / or interconnected silicon oxide.

[33]

[0124] The coating composition according to any one of

[29] to

[32] , wherein the aspect ratio (major axis / minor axis) of the inorganic oxide (G) is 3 to 25.

[34]

[0126] The coating composition according to any one of

[29] to

[33] , further comprising an isocyanate compound and / or a urethane compound.

[35]

[0128] The coating composition as described in

[34] , wherein the isocyanate compound is a water-dispersible isocyanate compound.

[36]

[0130] The coating composition as described in

[35] , wherein the water-dispersible isocyanate compound is a blocked isocyanate.

[37]

[0132] A coating composition comprising polymer nanoparticles (A) and a matrix raw material component (B'), wherein:

[0133] The elastic recovery rate η of the polymer nanoparticles (A) measured by the indentation test according to ISO14577-1 is ITA 0.30 or more and 0.90 or less,

[0134] The Martens hardness HM of the polymer nanoparticles (A) is A The Martens hardness HM of the matrix raw material component (B') B’ Meet HM B’ / HM A >1 relationship,

[0135] The matrix raw material component (B') comprises an inorganic oxide (D),

[0136] The inorganic oxide (D) contains at least one inorganic component selected from the group consisting of Ce, Nb, Al, Zn, Ti, Zr, Sb, Mg, Sn, Bi, Co and Cu.

[38]

[0138] The coating composition as described in

[37] , further comprising a sunscreen agent (S2).

[39]

[0140] The coating composition as described in any one of

[29] to

[38] , wherein the polymer nanoparticles (A) and / or the adhesive latex particles (F) have a functional group (e) containing a secondary amide group and / or a tertiary amide group.

[40]

[0142] The coating composition according to any one of

[29] to

[39] , wherein the polymer nanoparticles (A) and / or the adhesive latex particles (F) have a functional group containing a hydroxyl group.

[41]

[0144] A hard coating film comprising polymer nanoparticles (A) and a matrix component (B), wherein:

[0145] The Martens hardness HM of the polymer nanoparticles (A) is A The Martens hardness HM of the matrix component (B) B Meet HM B / HM A >1 relationship,

[0146] The Martens hardness HM of the hard coating film is 100 N / mm 2 above,

[0147] The matrix component (B) comprises an inorganic oxide (D),

[0148] The inorganic oxide (D) contains at least one inorganic component selected from the group consisting of Ce, Nb, Al, Zn, Ti, Zr, Sb, Mg, Sn, Bi, Co and Cu.

[0149] Effects of the Invention

[0150] (1st effect)

[0151] According to the present invention, a laminate having high abrasion resistance, adhesion, and optical characteristics can be provided.

[0152] (Second effect)

[0153] According to the present invention, a hard coating film having high abrasion resistance, durability and weather resistance, a substrate with the hard coating film, a coating composition and a window material can be provided. DETAILED DESCRIPTION

[0154] A specific embodiment of the present invention (hereinafter referred to as "this embodiment") will be described in detail below. It should be noted that the present invention is not limited to the following this embodiment, and can be implemented with various modifications within the scope of the gist thereof.

[0155] <<First Embodiment>>

[0156] Here, a first mode of the present embodiment (also referred to as “first embodiment” in this specification) will be described in detail.

[0157] <Laminated body>

[0158] The laminate of the present embodiment (hereinafter, unless otherwise specified, the "present embodiment" in the <<First embodiment>> item refers to the first embodiment) is a laminate having a substrate with an adhesive layer and an adhesive layer disposed on the substrate and containing adhesive latex particles (F), an inorganic oxide (G) and a light-shielding agent; and a hard coating layer disposed on the substrate with an adhesive layer and containing a matrix component (B) containing an inorganic oxide (D), wherein the haze value H1 of the substrate with an adhesive layer is greater than the haze value H2 of the laminate. Since the laminate of the present embodiment is constructed as described above, it has high wear resistance, adhesion and optical properties.

[0159] In the present embodiment, from the viewpoint of adhesion, the ratio of H1 to H2 (H1 / H2) is preferably 2 or more, more preferably 5 or more, further preferably 10 or more, and particularly preferably 20 or more.

[0160] In addition, in the present embodiment, even when it is difficult to confirm the magnitude relationship between H1 and H2, the magnitude relationship can be estimated by evaluating the surface roughness. That is, the laminate of the present embodiment can be defined as follows: it is a laminate having a substrate with an adhesive layer and a hard coating layer (C), the substrate with an adhesive layer having a substrate and an adhesive layer disposed on the substrate and containing adhesive latex particles (F), an inorganic oxide (G) and a light shielding agent (S1); the hard coating layer (C) is disposed on the substrate with the adhesive layer and contains a matrix component (B) containing an inorganic oxide (D), wherein the surface roughness Ra1 of the substrate with the adhesive layer is greater than the surface roughness Ra2 of the laminate.

[0161] In the present embodiment, from the viewpoint of adhesion, the ratio of Ra1 to Ra2 (Ra1 / Ra2) is preferably 1.5 or more, more preferably 2 or more, further preferably 3 or more, and particularly preferably 5 or more.

[0162] Since the laminate of the present embodiment is constructed as described above, it has high wear resistance, adhesion and optical properties. The laminate of the present embodiment exhibits high levels of wear resistance, adhesion and optical properties, and is therefore useful as a hard film for, for example, building materials, automobile parts, electronic equipment, motor products, etc., but is not limited thereto, and is particularly preferably used as an automobile part.

[0163] [Base material with adhesive layer]

[0164] The adhesive layer-attached substrate in this embodiment comprises a substrate and an adhesive layer disposed on the substrate and containing adhesive emulsion particles (F), an inorganic oxide (G) and a light shielding agent. In this embodiment, the adhesive layer is disposed on at least one surface and / or both surfaces of the substrate.

[0165] [Base material]

[0166] The substrate in the present embodiment is not particularly limited, and resin, metal, glass, etc. can be cited. As the shape of the substrate, for example, a plate-like shape, a shape including concave and convex shapes, a shape including a curved surface, a hollow shape, a shape of a porous body, a combination thereof, etc. can be cited, but not limited to. In addition, regardless of the type of substrate, for example, sheets, films, fibers, etc. can be cited. Among them, from the aspect of imparting hard coating properties and formability, resin is preferably used. The resin used as the substrate can be cited, but not limited to, for example, thermoplastic resins and thermosetting resins. The thermoplastic resin used as the substrate can be cited, but not limited to, for example, polyethylene, polypropylene, polystyrene, ABS resin, vinyl chloride resin, methyl methacrylate resin, nylon, fluororesin, polycarbonate, polyester resin, etc. In addition, the thermosetting resin used as the substrate can be cited, but not limited to, for example, phenol resin, urea resin, melamine resin, unsaturated polyester resin, epoxy resin, silicone resin, silicone rubber, SB rubber, natural rubber, thermosetting elastomer, etc.

[0167] [Adhesive layer]

[0168] In this embodiment, the adhesive layer contains adhesive emulsion particles (F), an inorganic oxide (G), and a light shielding agent.

[0169] [Adhesive emulsion particles (F)]

[0170] The adhesive latex particles (F) in the present embodiment play a role in imparting flexibility and improving adhesion to the substrate. The adhesive latex particles (F) are not particularly limited, and are, for example, particles composed of polycarbonyl compounds such as polyurethane, polyester, poly(meth)acrylate, polyvinyl acetate, polybutadiene, polyvinyl chloride, chlorinated polypropylene, polyethylene, polystyrene, polystyrene-(meth)acrylate copolymers, rosin derivatives, alcohol adducts of styrene-maleic anhydride copolymers, cellulose resins, silicone compounds, etc. In the present embodiment, the adhesive latex particles (F) are preferably poly(meth)acrylate.

[0171] The preparation method of the adhesive latex particles (F) in the present embodiment is not particularly limited, and preferably a structure obtained by polymerizing a vinyl monomer in the presence of water and an emulsifier. When the adhesive latex particles (F) obtained in this way are included in the adhesive layer, there is a tendency to maintain better adhesion to the substrate.

[0172] The vinyl monomer is not particularly limited, and examples thereof include (meth)acrylates, aromatic vinyl compounds, cyanide vinyl compounds, and monomers containing functional groups such as carboxyl group-containing vinyl monomers, hydroxyl group-containing vinyl monomers, epoxy group-containing vinyl monomers, carbonyl group-containing vinyl monomers, and vinyl monomers having secondary amide groups and / or tertiary amide groups.

[0173] The (meth)acrylate is not particularly limited, and examples thereof include alkyl (meth)acrylates having 1 to 50 carbon atoms in the alkyl portion and (poly)oxyethylene di(meth)acrylates having 1 to 100 oxyethylene groups.

[0174] The alkyl (meth)acrylate is not particularly limited, and examples thereof include methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, methylcyclohexyl (meth)acrylate, cyclohexyl (meth)acrylate, lauryl (meth)acrylate, and dodecyl (meth)acrylate.

[0175] The (poly)oxyethylene di(meth)acrylate is not particularly limited, and examples thereof include ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, diethylene glycol methoxy(meth)acrylate, and tetraethylene glycol di(meth)acrylate.

[0176] The aromatic vinyl compound is not particularly limited, and examples thereof include styrene and 4-vinyltoluene.

[0177] The vinyl cyanide compound is not particularly limited, and examples thereof include acrylonitrile and methacrylonitrile.

[0178] There is no particular limitation on the carboxyl-containing vinyl monomer, and for example, (methyl) acrylic acid, crotonic acid, itaconic acid, maleic acid, fumaric acid, maleic anhydride, or half fats of dibasic acids such as itaconic acid, maleic acid, and fumaric acid can be cited. When using a carboxyl-containing vinyl monomer, a carboxyl group can be introduced into the adhesive emulsion particles (F) in the present embodiment, and the stability of the emulsion can be improved by providing electrostatic repulsion between the particles, and there is a tendency to improve resistance to external dispersion destruction such as agglomeration during stirring. At this time, from the perspective of further improving the electrostatic repulsion, a part or all of the above-mentioned imported carboxyl groups can also be neutralized with amines such as ammonia or triethylamine, dimethylethanolamine, or alkalis such as NaOH and KOH.

[0179] The hydroxyl group-containing vinyl monomer is not particularly limited, and examples thereof include hydroxyalkyl (meth)acrylic acid esters such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate; hydroxyalkyl fumaric acid esters such as di-2-hydroxyethyl fumarate and mono-2-hydroxyethyl monobutyl fumarate; allyl alcohol, (poly)oxyethylene mono(meth)acrylates having 1 to 100 oxyethylene groups; (poly)oxypropylene mono(meth)acrylates having 1 to 100 oxypropylene groups; and "PRAXCELL FM, FA Monomer" (trade name of caprolactone addition monomer manufactured by Daicel Chemical Co., Ltd.), and other hydroxyalkyl esters of α,β-ethylenically unsaturated carboxylic acids.

[0180] The (poly)oxyethylene (meth)acrylate is not particularly limited, and examples thereof include ethylene glycol (meth)acrylate, ethylene glycol methoxy (meth)acrylate, diethylene glycol (meth)acrylate, diethylene glycol methoxy (meth)acrylate, tetraethylene glycol (meth)acrylate, and tetraethylene glycol methoxy (meth)acrylate.

[0181] The (poly)oxypropylene (meth)acrylate is not particularly limited, and examples thereof include propylene glycol (meth)acrylate, propylene glycol methoxy (meth)acrylate, dipropylene glycol (meth)acrylate, dipropylene glycol methoxy (meth)acrylate, tetrapropylene glycol (meth)acrylate, and tetrapropylene glycol methoxy (meth)acrylate.

[0182] The epoxy group-containing vinyl monomer is not particularly limited, and examples thereof include glycidyl group-containing vinyl monomers, etc. The glycidyl group-containing vinyl monomer is not particularly limited, and examples thereof include glycidyl (meth)acrylate, allyl glycidyl ether, and allyl dimethyl glycidyl ether.

[0183] The carbonyl group-containing vinyl monomer is not particularly limited, and examples thereof include acetylacetone acrylamide and the like.

[0184] Specific examples of vinyl monomers other than the above are not particularly limited, and examples thereof include olefins such as ethylene, propylene, and isobutylene, dienes such as butadiene, halogenated olefins such as vinyl chloride, vinylidene chloride, vinyl fluoride, tetrafluoroethylene, and chlorotrifluoroethylene, vinyl acetate, vinyl propionate, vinyl n-butyrate, vinyl benzoate, vinyl p-tert-butylbenzoate, vinyl pivalate, vinyl 2-ethylhexanoate, vinyl versatate, and vinyl laurate, carboxylic acid vinyl esters such as isopropenyl acetate and isopropenyl propionate, ethyl vinyl ether, isobutylene, and the like. Vinyl ethers such as allyl vinyl ether, cyclohexyl vinyl ether, allyl esters such as allyl acetate and allyl benzoate, allyl ethers such as allyl ethyl ether and allyl phenyl ether, and 4-(meth)acryloyloxy-2,2,6,6-tetramethylpiperidine, 4-(meth)acryloyloxy-1,2,2,6,6-pentamethylpiperidine, perfluoromethyl (meth)acrylate, perfluoropropyl (meth)acrylate, perfluoropropyl methyl (meth)acrylate, vinyl pyrrolidone, trimethylolpropane tri(meth)acrylate, allyl (meth)acrylate, etc., or a combination thereof.

[0185] The vinyl monomer having a secondary amide group and / or a tertiary amide group is not particularly limited, and examples thereof include N-alkyl or N-alkylene-substituted (meth)acrylamide, etc. Specifically, examples thereof include N-methylacrylamide, N-methylmethacrylamide, N-ethylacrylamide, N,N-dimethylacrylamide, N,N-dimethylmethacrylamide, N,N-diethylacrylamide, N-ethylmethacrylamide, N-methyl-N-ethylacrylamide, N-methyl-N-ethylmethacrylamide, N-isopropylacrylamide, N-n-propylacrylamide, N-isopropylmethacrylamide, N-n-propylmethacrylamide, N-methyl-N-n-propylacrylamide, N-methyl N-acryloyl-N-isopropylacrylamide, N-acryloylpyrrolidine, N-methacryloylpyrrolidine, N-acryloylpiperidine, N-methacryloylpiperidine, N-acryloylhexahydroazepine, N-acryloylmorpholine, N-methacryloylmorpholine, N-vinylpyrrolidone, N-vinylcaprolactam, N,N'-methylenebisacrylamide, N,N'-methylenebismethacrylamide, N-vinylacetamide, acetylacetoneacrylamide, acetylacetonemethacrylamide, N-methylolacrylamide, N-methylolmethacrylamide, etc.

[0186] The silicone compound is not particularly limited, and examples thereof include trimethoxysilane, triethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, cyclohexyltrimethoxysilane, cyclohexyltriethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, dimethoxysilane, diethoxysilane, methyldimethoxysilane, methyldiethoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane, dimethoxydiphenylsilane, diethoxydiphenylsilane, 3-propylene Hydrolysis condensates of acyloxypropyltrimethoxysilane, 3-acryloxypropyltriethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, p-phenylvinyltrimethoxysilane, p-phenylvinyltriethoxysilane, tetramethoxysilane, tetraethoxysilane, and the like.

[0187] The adhesive latex particles (F) may contain an emulsifier. The emulsifier is not particularly limited, and examples thereof include acidic emulsifiers such as alkylbenzenesulfonic acid, alkylsulfonic acid, alkylsulfonated succinic acid, polyoxyethylene alkylsulfuric acid, polyoxyethylene alkylarylsulfuric acid, polyoxyethylene distyrylphenyl ether sulfonic acid, etc.; anionic surfactants such as alkali metal (Li, Na, K, etc.) salts of acidic emulsifiers, ammonium salts of acidic emulsifiers, fatty acid soaps, etc.; cationic surfactants in the form of quaternary ammonium salts, pyridinium salts, and imidazolinium salts such as alkyltrimethylammonium bromide, alkylpyridinium bromide, and imidazolinium laurate; nonionic surfactants such as polyoxyethylene alkylaryl ether, polyoxyethylene sorbitan fatty acid ester, polyoxyethylene oxypropylene block copolymer, polyoxyethylene distyrylphenyl ether, and reactive emulsifiers having free radical polymerizable double bonds, etc.

[0188] Examples of the reactive emulsifier having a radical polymerizable double bond include, but are not limited to, Eleminol JS-2 (trade name, manufactured by Sanyo Chemical Industry Co., Ltd.), Latemul S-120, S-180A or S-180 (trade name, manufactured by Kao Corporation), Aquaron HS-10, KH-1025, RN-10, RN-20, RN30, RN50 (trade name, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), Adeka Reasoap SE1025, SR-1025, NE-20, NE-30, NE-40 (trade names, manufactured by Asahi Denka Kogyo Co., Ltd.), ammonium salts of p-styrenesulfonic acid, sodium salts of p-styrenesulfonic acid, potassium salts of p-styrenesulfonic acid, alkylsulfonic acid (meth)acrylates such as 2-sulfoethyl acrylate, methylpropanesulfonic acid (meth)acrylamide, ammonium salts of allylsulfonic acid, sodium salts of allylsulfonic acid, potassium salts of allylsulfonic acid, etc.

[0189] [Average particle size of adhesive emulsion particles (F)]

[0190] The average particle size of the adhesive emulsion particles (F) in the present embodiment is obtained by the particle size observed by cross-sectional SEM or dynamic light scattering. The average particle size of the adhesive emulsion particles (F) is not particularly limited, and is preferably less than 300nm. By adjusting the average particle size of the adhesive emulsion particles (F) to the above range, there is a tendency to form an adhesive layer with better adhesion by increasing the contact area with the substrate. In addition, from the aspect of improving the transparency of the obtained adhesive layer, the average particle size is more preferably less than 200nm, and from the aspect of good storage stability of the raw material composition of the adhesive layer, it is preferably more than 10nm, more preferably more than 50nm. Regarding the determination method of the average particle size of the adhesive emulsion particles (F), it can be measured by the method described in the embodiments described later.

[0191] [Inorganic oxide (G)]

[0192] From the aspect of improving the adhesion brought by the interaction with the hard coat, the adhesive layer in the present embodiment includes an inorganic oxide (G). It is believed that the adhesive layer in the present embodiment increases the surface roughness of the adhesive layer by including adhesive latex particles (F) and inorganic oxide (G), thereby improving the adhesion. Regarding the surface roughness of the adhesive layer, for example, by using a thermal gradient tester, the minimum film forming temperature measured according to JIS K6828-2 between the adhesive latex particles (F) and the inorganic oxide (G) is compared, thereby evaluating. That is, the minimum film forming temperature T1 of the adhesive latex particles (F) can be less than the minimum film forming temperature T2 of the inorganic oxide (G) to indirectly confirm that the adhesive layer has sufficient surface roughness. As a specific determination method of the minimum film forming temperature T1 and T2, based on the method described in the embodiment described later.

[0193] As specific examples of the inorganic oxide (G) in the present embodiment, oxides such as silicon, aluminum, titanium, zirconium, zinc, cerium, tin, indium, gallium, germanium, antimony, molybdenum, niobium, magnesium, bismuth, cobalt, and copper can be cited but are not limited thereto. They can be a single substance or a mixture. Among the above substances, the inorganic oxide (G) is preferably silicon oxide particles. On the other hand, from the aspect of improving optical properties, the inorganic oxide (G) preferably includes at least one selected from the group consisting of cerium oxide, zinc oxide, aluminum oxide, zirconium oxide, niobium oxide, bismuth oxide, cobalt oxide, copper oxide, tin oxide, and titanium oxide.

[0194] Regarding the primary average particle size of the inorganic oxide (G) in the present embodiment, from the aspect of good storage stability of the raw material composition of the adhesive layer, it is preferably 2 nm or more. From the aspect of good transparency as the whole laminate, it is preferably 150 nm or less, more preferably 100 nm or less, and further preferably 50 nm or less. Therefore, the primary average particle size is preferably 2 nm or more and 100 nm or less, more preferably 2 nm or more and 50 nm or less, and further preferably 4 nm or more and 50 nm or less. The primary average particle size can be measured by the method described in the embodiments described later.

[0195] The inorganic oxide (G) is not particularly limited, but is preferably silicon oxide particles represented by dry silicon oxide and colloidal silicon oxide from the perspective of interaction with the hydrolyzable silicon compound (b) described below and adhesion to the hard coat layer. Colloidal silicon oxide is preferred because it can be used in the form of an aqueous dispersion.

[0196] [Colloidal Silica Suitable for Use as Inorganic Oxide (G)]

[0197] The acidic colloidal silica using water as a dispersion solvent suitable for use in the present embodiment is not particularly limited, and can be prepared by a sol-gel method or a commercially available product. When prepared by a sol-gel method, reference can be made to Werner Stober et al; J. Colloid and Interface Sci., 26, 62-69 (1968), Rickey D. Badley et al; Lang muir 6, 792-801 (1990), Journal of the Color Society, 61 [9] 488-493 (1988), etc.

[0198] When commercially available products are used, for example, Snowtex-O, Snowtex-OS, Snowtex-OXS, Snowtex-O-40, Snowtex-OL, Snowtex OYL, Snowtex-OUP, Snowtex-PS-SO, Snowtex-PS-MO, Snowtex-AK-XS, Snowtex-AK, Snowtex-AK-L, Snowtex-AK-YL, Snowtex-AK-PS-S (trade names, manufactured by Nissan Chemical Industries, Ltd.), Adelite AT-20Q (trade name, manufactured by Asahi Denka Industries, Ltd.), Klebosol 20H12, Klebosol 30CAL25 (trade names, manufactured by Clariant (Japan) Ltd.), etc. may be mentioned.

[0199] In addition, the alkaline colloidal silica includes silica stabilized by the addition of alkali metal ions, ammonium ions, or amines, and examples thereof include, but are not particularly limited to, Snowtex-20, Snowtex-30, Snowtex-XS, Snowtex-50, Snowtex-30L, Snowtex-XL, Snowtex-YL, Snowtex ZL, Snowtex-UP, Snowtex-ST-PS-S, Snowtex ST-PS-M, Snowtex-C, Snowtex-CXS, Snowtex-CM, Snowtex-N, Snowtex-NXS, Snowtex-NS, and Snowtex-N-40 (trade names, manufactured by Nissan Chemical Industries, Ltd.), Adelite AT-20, Adelite AT-30, Adelite AT-20N, Adelite AT-30N, Adelite AT-20A, Adelite AT-30A, Adelite AT-40, and Adelite AT-50 (trade name, manufactured by Asahi Electric Industries, Ltd.), Klebosol 30R9, Klebosol 30R50, Klebosol 50R50 (trade name, manufactured by Clariant Japan Ltd.), Ludox HS-40, Ludox HS-30, Ludox LS, Ludox AS-30, Ludox SM-AS, Ludox AM, Ludox HSA and Ludox SM (trade name, manufactured by DuPont), etc.

[0200] In addition, there is no particular limitation on the colloidal silica using a water-soluble solvent as a dispersion medium, and examples thereof include MA-ST-M (methanol dispersion type with a particle size of 20 to 25 nm), IPA-ST (isopropanol dispersion type with a particle size of 10 to 15 nm), EG-ST (ethylene glycol dispersion type with a particle size of 10 to 15 nm), EGST-ZL (ethylene glycol dispersion type with a particle size of 70 to 100 nm), NPC-ST (ethylene glycol monopropyl ether dispersion type with a particle size of 10 to 15 nm), and TOL-ST (toluene dispersion type with a particle size of 10 to 15 nm) manufactured by Nissan Chemical Industries, Ltd.

[0201] The dry silica particles are not particularly limited, and examples thereof include AEROSIL manufactured by NIPPON AEROSIL CO., LTD. and REOLOSIL manufactured by TOKUYAMA CO., LTD.

[0202] The silicon oxide particles may contain an inorganic base (sodium hydroxide, potassium hydroxide, lithium hydroxide, ammonia, etc.) or an organic base (tetramethylammonium, triethylamine, etc.) as a stabilizer.

[0203] [Shape of Inorganic Oxide (G)]

[0204] In addition, the shape of the inorganic oxide (G) in the present embodiment can include but is not limited to one or more mixtures of spherical, tetragonal, polyhedral, elliptical, flat, linear, beaded, chained, etc. In the present embodiment, from the aspect of the hardness and transparency of the laminate, the inorganic oxide (G) preferably has a spherical and / or beaded, chained and other linked structures. In addition, from the aspect of the adhesion of the laminate, the inorganic oxide (G) more preferably has a beaded, chained and other linked structures. Here, the beaded is a spherical primary particle linked to a beaded structure, and the chain is a spherical primary particle linked to a chain structure. In the present embodiment, it is particularly preferred that the inorganic oxide (G) is silicon oxide with a spherical and / or linked structure.

[0205] The aspect ratio (long diameter / short diameter) of the beaded or chain-shaped inorganic oxide (G) is preferably 3 to 25. From the aspect of adhesion, the aspect ratio (long diameter / short diameter) is preferably 3 or more. In addition, from the aspect of transparency, the aspect ratio (long diameter / short diameter) is preferably 25 or less. The aspect ratio can be measured by the method described in the examples described later.

[0206] [Complex of adhesive emulsion particles (F) and inorganic oxide (G)]

[0207] Inorganic oxide (G) can be pre-compounded with adhesive latex particles (F). The composite of adhesive latex particles (F) and inorganic oxide (G) is obtained, for example, by polymerizing the vinyl monomer constituting the above-mentioned adhesive latex particles (F) in the presence of inorganic oxide (G). From the aspect of interaction with inorganic oxide (G), the vinyl monomer preferably includes the above-mentioned vinyl monomer with secondary amide group and / or tertiary amide group. By hydrogen bonding of the hydroxyl group of inorganic oxide (G) and secondary amide group and / or tertiary amide group, a composite can be formed ideally.

[0208] In the present embodiment, from the aspect of transparency and adhesion, it is preferred that the average particle diameter of at least one of the group consisting of the composite of the inorganic oxide (G), the adhesive emulsion particles (F) and the inorganic oxide (G) and the adhesive emulsion particles (F) is more than 2nm and less than 400nm. The above-mentioned average particle diameter can be measured by the method described in the embodiment described later. Here, the bonding layer in the present embodiment can be obtained by applying the coating composition (J) described later to the substrate and making a coating film by heat treatment, ultraviolet irradiation, infrared irradiation, etc., therefore, as long as the inorganic oxide (G) in the coating composition (J), the adhesive emulsion particles (F) and the composite of the inorganic oxide (G) and the adhesive emulsion particles (F) are known, then it is possible to determine each average particle diameter in the bonding layer in the form of the average particle diameter of the composite of the inorganic oxide (G), the adhesive emulsion particles (F) and the inorganic oxide (G) and the adhesive emulsion particles (F) in the corresponding bonding layer in a good consistent manner.

[0209] From the aspect of adhesion, the mass ratio of the adhesive emulsion particles (F) to the inorganic oxide (G) is preferably 1:0.1 to 1:10, more preferably 1:0.3 to 1:5, and further preferably 1:0.5 to 1:2. Here, the adhesive layer in the present embodiment can be obtained by applying the coating composition (J) described later to a substrate and forming a coating film by heat treatment, ultraviolet irradiation, infrared irradiation, etc. Therefore, as long as the mass ratio of the adhesive emulsion particles (F) to the inorganic oxide (G) in the coating composition (J) is known, the mass ratio in the adhesive layer can be determined in a form that the mass ratio is well consistent with the mass ratio of the adhesive emulsion particles (F) to the inorganic oxide (G) in the corresponding adhesive layer.

[0210] From the viewpoint of adhesion, the thickness of the adhesive layer is preferably 0.1 μm or more, more preferably 0.3 μm or more, and from the viewpoint of transparency, the thickness of the adhesive layer is preferably 100.0 μm or less, more preferably 50.0 μm or less.

[0211] [Sunscreen]

[0212] In the adhesive layer of the present embodiment, from the aspect of ensuring optical properties, in addition to adhesive emulsion particles (F) and inorganic oxides (G), a sunscreen is further included. The sunscreen is not particularly limited, but from the aspect of improving optical properties, it is preferred to include a UV absorber. Specific examples of UV absorbers include, but are not limited to, 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-methoxybenzophenone-5-sulfonic acid, 2-hydroxy-4-n-octyloxybenzophenone, 2-hydroxy-4-n-dodecyloxybenzophenone, 2-hydroxy-4-benzyloxybenzophenone, bis(5-benzoyl-4-hydroxy-2-methoxyphenyl)methane, 2,2'-dihydroxy-4-methoxybenzophenone, 2,2'-dihydroxy-4,4'-dimethyl Benzophenone-based ultraviolet absorbers such as oxybenzophenone (trade name "UVINUL3049" manufactured by BASF), 2,2',4,4'-tetrahydroxybenzophenone (trade name "UVINUL3050" manufactured by BASF), 4-dodecyloxy-2-hydroxybenzophenone, 5-benzoyl-2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxy-2'-carboxybenzophenone, 2-hydroxy-4-stearyloxybenzophenone, and 4,6-dibenzoylresorcinol;2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-(2'-hydroxy-5'-tert-butylphenyl)benzotriazole, 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)benzotriazole, 2-(2-hydroxy-5-tert-octylphenyl)benzotriazole, 2-(2-hydroxy-3,5-di-tert-octylphenyl)benzotriazole, 2-[2'-hydroxy-3',5'-bis(α,α'-dimethylbenzyl)phenyl]benzotriazole), methyl-3-[3-tert-butyl-5-(2H-phenyl)benzotriazole] 3-[(2H-benzotriazol-2-yl)-4-hydroxyphenyl]propionate and polyethylene glycol (molecular weight 300) condensate (trade name "TINUVIN1130" manufactured by BASF), isooctyl-3-[3-(2H-benzotriazol-2-yl)-5-tert-butyl-4-hydroxyphenyl]propionate (trade name "TINUVIN384" manufactured by BASF), 2-(3-dodecyl-5-methyl-2-hydroxyphenyl)benzotriazole (trade name "TINUVIN IN571”), 2-(2'-hydroxy-3'-tert-butyl-5'-methylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3',5'-di-tert-amylphenyl)benzotriazole, 2-(2'-hydroxy-4'-octyloxyphenyl)benzotriazole, 2-[2'-hydroxy-3'-(3",4",5",6"-tetrahydrophthalimidomethyl)-5'-methylphenyl]benzotriazole, 2,2-methylenebis[4-(1,1,3,3-tetramethylbutyl)-6-(2H -benzotriazole-2-yl)phenol], 2-(2H-benzotriazole-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol (trade name "TINUVIN900" manufactured by BASF), TINUVIN384-2, TINUVIN326, TINUVIN327, TINUVIN109, TINUVIN970, TINUVIN328, TINUVIN171, TINUVIN970, TINUVIN PS, TINUVIN P, TINUVIN99-2, TINUVIN928 (trade name, manufactured by BASF) and other benzotriazole-based ultraviolet absorbers;2-[4-[(2-hydroxy-3-dodecyloxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2-[4-[(2-hydroxy-3-tridecyloxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2,4-bis(2-hydroxy-4-butylhydroxyphenyl)-6-(2,4-bisbutylhydroxyphenyl)-1,3,5-triazine (manufactured by BASF Corporation) triazine-based ultraviolet absorbers such as TINUVIN 460 (trade name, manufactured by BASF), 2-(2-hydroxy-4-[1-octyloxycarbonylethoxy]phenyl)-4,6-bis(4-phenylphenyl)-1,3,5-triazine (trade name, manufactured by BASF), TINUVIN 400, TINUVIN 405, TINUVIN 477, and TINUVIN 1600 (trade name, manufactured by BASF); malonate-based ultraviolet absorbers such as HOSTAVIN PR25, HOSTAVIN B-CAP, and HOSTAVIN VSU (trade name, manufactured by Clariant); and HOSTAVIN 3206 LIQ, HOSTAVIN VSU P, and HOSTAVIN 3212 Anilide-based ultraviolet absorbers such as LIQ (trade name, manufactured by Clariant); salicylate-based ultraviolet absorbers such as amyl salicylate, menthyl salicylate, homomenthyl salicylate, octyl salicylate, phenyl salicylate, benzyl salicylate, and p-isopropylphenyl salicylate; cyanoacrylate-based ultraviolet absorbers such as ethyl 2-cyano-3,3-diphenylacrylate (trade name "UVINUL3035" manufactured by BASF), (2-ethylhexyl)-2-cyano-3,3-diphenylacrylate (trade name "UVINUL3039" manufactured by BASF), and 1,3-bis((2'-cyano-3',3'-diphenylacryloyl)oxy)-2,2-bis-(((2'-cyano-3',3'-diphenylacryloyl)oxy)methyl)propane (trade name "UVINUL3030" manufactured by BASF);2-Hydroxy-4-acryloxybenzophenone, 2-hydroxy-4-methacryloxybenzophenone, 2-hydroxy-5-acryloxybenzophenone, 2-hydroxy-5-methacryloxybenzophenone, 2-hydroxy-4-(acryloxy-ethoxy)benzophenone, 2-hydroxy-4-(methacryloxy-ethoxy)benzophenone, 2-hydroxy-4-(methacryloxy-diethoxy)benzophenone, 2-hydroxy-4-(acryloxy-triethoxy)benzophenone, 2-(2'-hydroxy-5'-methacryloxy)benzophenone 2-(2'-hydroxy-5'-methacryloyloxyethylphenyl)-2H-benzotriazole (trade name "RUVA-93" manufactured by Otsuka Chemical Co., Ltd.), 2-(2'-hydroxy-5'-methacryloyloxyethyl-3-tert-butylphenyl)-2H-benzotriazole, 2-(2'-hydroxy-5'-methacryloyloxypropyl-3-tert-butylphenyl)-5-chloro-2H-benzotriazole, 3-methacryloyl-2-hydroxypropyl-3-[3'-(2"-benzotriazolyl)-4-hydroxy-5-tert-butyl]phenyl propionate (Japan Ciba-G Radical polymerizable UV absorbers having a radical polymerizable double bond in the molecule, such as CGL-104 (trade name manufactured by Nippon Shokubai Co., Ltd.); UV-absorbing polymers such as UV-G101, UV-G301, UV-G137, UV-G12, and UV-G13 (trade names manufactured by Nippon Shokubai Co., Ltd.); UV absorbers reactive with silanol groups, isocyanate groups, epoxy groups, semicarbazide groups, and hydrazide groups, etc., and one of them or two or more of them can be used in combination. From the aspect of the ultraviolet absorption capacity, the ultraviolet absorber preferably includes at least one selected from the group consisting of benzotriazole ultraviolet absorbers, benzophenone ultraviolet absorbers, triazine ultraviolet absorbers, malonate ultraviolet absorbers, anilide ultraviolet absorbers, salicylate ultraviolet absorbers, and cyanoacrylate ultraviolet absorbers, and more preferably includes at least one selected from the group consisting of benzotriazole ultraviolet absorbers, benzophenone ultraviolet absorbers, triazine ultraviolet absorbers, and cyanoacrylate ultraviolet absorbers. ;

[0213] [Components that may be contained in the adhesive layer]

[0214] The adhesive layer in the present embodiment is not particularly limited as long as it comprises adhesive latex particles (F), inorganic oxides (G) and sunscreens, and may also comprise other components. As other components, it is not particularly limited, for example, thermoplastic resins, thermosetting resins, rubber-elastomers, etc. can be cited, wherein preferred acrylic resins, acrylic urethane resins, carbamate resins, silicone resins, etc. are preferably acrylic resins, acrylic urethane resins, carbamate resins, silicone resins, etc. In addition, the adhesive layer can arbitrarily comprise appropriate additives as required. As additives, it is possible to cite but is not limited to, for example, crosslinking agents, tackifiers, plasticizers, pigments, dyes, fillers, anti-aging agents, conductive materials, light stabilizers, stripping regulators, softeners, surfactants, flame retardants, antioxidants, catalysts, etc., and from the aspect of optical properties, it is preferred to include light stabilizers and / or antioxidants. From the same aspect, it is not particularly limited as light stabilizers, for example, hindered amine compounds, benzotriazole compounds, triazine compounds, benzophenone compounds, benzoate compounds, etc. can be cited. The antioxidant is not particularly limited, and examples thereof include phenolic compounds, amine compounds, phosphorus compounds, and sulfur compounds.

[0215] Examples of crosslinking agents include, but are not limited to, isocyanate crosslinking agents, epoxy crosslinking agents, carbodiimide crosslinking agents, oxazoline crosslinking agents, aziridine crosslinking agents, amine crosslinking agents, peroxide crosslinking agents, melamine crosslinking agents, urea crosslinking agents, metal alkoxide crosslinking agents, metal chelate crosslinking agents, and metal salt crosslinking agents.

[0216] Examples of the light stabilizer include, but are not limited to, bis(2,2,6,6-tetramethyl-4-piperidinyl)succinate, bis(2,2,6,6-tetramethylpiperidinyl)sebacate, bis(1,2,2,6,6-pentamethyl-4-piperidinyl)2-(3,5-di-tert-butyl-4-hydroxybenzyl)-2-butylmalonate, 1-[2-[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propynyloxy]ethyl]-4-[3-(3,5 -di-tert-butyl-4-hydroxyphenyl)propynyloxy]-2,2,6,6-tetramethylpiperidine, a mixture of bis(1,2,2,6,6-pentamethyl-4-piperidyl) sebacate and methyl-1,2,2,6,6-pentamethyl-4-piperidyl-sebacate (trade name "TINUVIN 292" manufactured by BASF), bis(1-octyloxy-2,2,6,6-tetramethyl-4-piperidyl) sebacate, TINUVIN 12 3. Hindered amine light stabilizers such as TINUVIN144, TINUVIN152, TINUVIN249, TINUVIN292, and TINUVIN5100 (trade names, manufactured by BASF); 1,2,2,6,6-pentamethyl-4-piperidinyl methacrylate, 1,2,2,6,6-pentamethyl-4-piperidinyl acrylate, 2,2,6,6-tetramethyl-4-piperidinyl methacrylate, 2, Free radical polymerizable hindered amine light stabilizers such as 2,6,6-tetramethyl-4-piperidinyl acrylate, 1,2,2,6,6-pentamethyl-4-iminopiperidinyl methacrylate, 2,2,6,6-tetramethyl-4-iminopiperidinyl methacrylate, 4-cyano-2,2,6,6-tetramethyl-4-piperidinyl methacrylate, and 4-cyano-1,2,2,6,6-pentamethyl-4-piperidinyl methacrylate; and light-stable polymers such as Udouble E-133, Udouble E-135, Udouble S-2000, Udouble S-2834, Udouble S-2840, Udouble S-2818, and Udouble S-2860 (trade names, manufactured by Nippon Shokubai Co., Ltd.).

[0217] The above components may be used alone or in combination of two or more.

[0218] The content of the ultraviolet absorber is preferably 1 part by mass or more, more preferably 5 parts by mass or more, further preferably 12 parts by mass or more, and further preferably 20 parts by mass or more, based on 100 parts by mass of the solid content of the adhesive emulsion particles (F) from the viewpoint of optical properties. In addition, from the viewpoint of solubility, it is preferably 300 parts by mass or less, more preferably 150 parts by mass or less, and further preferably 50 parts by mass or less, based on 100 parts by mass of the solid content of the adhesive emulsion particles (F).

[0219] The content of the light stabilizer is preferably 0.01 parts by mass or more, more preferably 0.05 parts by mass or more, further preferably 0.1 parts by mass or more, and further preferably 0.5 parts by mass or more, based on 100 parts by mass of the solid content of the adhesive latex particles (F) from the perspective of optical properties. In addition, from the perspective of coating stability, it is preferably 100 parts by mass or less, more preferably 50 parts by mass or less, and further preferably 10 parts by mass or less, based on 100 parts by mass of the solid content of the adhesive latex particles (F).

[0220] The content of the antioxidant is preferably 0.01 parts by mass or more, more preferably 0.05 parts by mass or more, further preferably 0.1 parts by mass or more, and further preferably 0.5 parts by mass or more, based on 100 parts by mass of the solid content of the adhesive latex particles (F) from the perspective of optical properties. In addition, from the perspective of coating stability, it is preferably 100 parts by mass or less, more preferably 50 parts by mass or less, and further preferably 10 parts by mass or less, based on 100 parts by mass of the solid content of the adhesive latex particles (F).

[0221] [Isocyanate compound]

[0222] In the adhesive layer in the present embodiment, from the aspect of improving the adhesion of the adhesive layer and the substrate, it is preferred to further contain isocyanate compounds and / or carbamate compounds as isocyanate-based crosslinking agents. In the case of further comprising isocyanate compounds and / or carbamate compounds, it is preferred to use adhesive latex particles (F) formed by the polymerization of monomers comprising the above-mentioned hydroxyl-containing vinyl monomer. In this case, the hydroxyl group of the adhesive latex particles (F) and the isocyanate compounds form carbamate bonds when the coating is formed, which has a tendency to improve the adhesion of the coating, the coating strength.

[0223] The isocyanate compound is a compound having at least one isocyanate group in one molecule. The isocyanate compound may be a compound having two or more isocyanate groups in one molecule.

[0224] Examples of the isocyanate compound include, but are not limited to, aliphatic diisocyanates such as 1,4-tetramethylene diisocyanate, ethyl (2,6-diisocyanato) hexanoate, 1,6-hexamethylene diisocyanate, 1,12-dodecamethylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate or 2,4,4-trimethylhexamethylene diisocyanate; aliphatic triisocyanates such as 1,3,6-hexamethylene triisocyanate, 1,8-diisocyanato-4-isocyanatomethyloctane, 2-isocyanatoethyl (2,6-diisocyanato) hexanoate; 1,3-bis(isocyanatomethylcyclohexane) or 1,4-bis(isocyanatomethylcyclohexane); alicyclic diisocyanates such as 2,5-diisocyanatomethyl-2-isocyanatepropyl-norbornane or 2,6-diisocyanatomethyl-2-isocyanatepropyl-norbornane; arylalkyl diisocyanates such as m-phenylenediisocyanate, α,α,α'α'-tetramethyl-m-phenylenediisocyanate; m-phenylenediisocyanate or Aromatic diisocyanates such as p-phenylene diisocyanate, tolyl-2,4-diisocyanate or tolyl-2,6-diisocyanate, diphenylmethane-4,4'-diisocyanate, naphthalene-1,5-diisocyanate, diphenyl-4,4'-diisocyanate, 4,4'-diisocyanato-3,3'-dimethylbiphenyl, 3-methyl-diphenylmethane-4,4'-diisocyanate, and diphenyl ether-4,4'-diisocyanate; aromatic triisocyanates such as triphenylmethane triisocyanate and tris(isocyanatophenyl)thiophosphate; and diisocyanates or triisocyanates having a uretdione structure obtained by cyclodimerizing the isocyanate groups of the above diisocyanates or triisocyanates. Polyisocyanates; polyisocyanates having an isocyanurate structure obtained by cyclotrimerizing the isocyanate groups of the above-mentioned diisocyanates or triisocyanates; polyisocyanates having a biuret structure obtained by reacting the above-mentioned diisocyanates or triisocyanates with water; polyisocyanates having an oxadiazinetrione structure obtained by reacting the above-mentioned diisocyanates or triisocyanates with carbon dioxide; polyisocyanates having an allophanate structure obtained by reacting the above-mentioned diisocyanates or triisocyanates with various alcohols; polyisocyanates obtained by reacting the above-mentioned diisocyanates or triisocyanates with a compound containing active hydrogen such as a polyhydroxy compound, a polycarboxyl compound, or a polyamine compound, etc.In addition, as the isocyanate compound having an alkoxysilane part and / or a siloxane part in the molecule, 3-isocyanate propyl triethoxy silane and / or the hydrolysis condensation product of 3-isocyanate propyl triethoxy silane etc. can be enumerated. They can be used as one or two or more are mixed and used. The isocyanate compound can also be a blocked polyisocyanate formed by reacting an isocyanate group with a blocking agent.

[0225] There is no particular limitation on the above-mentioned end-capping agent, and examples thereof include oxime compounds, alcohol compounds, amide compounds, imide compounds, phenol compounds, amine compounds, active methylene compounds, imidazole compounds, and pyrazole compounds. There is no particular limitation on the oxime compound, and examples thereof include formaldehyde oxime, acetaldehyde oxime, acetone oxime, methyl ethyl ketone oxime, and cyclohexanone oxime. There is no particular limitation on the alcohol compound, and examples thereof include methanol, ethanol, 2-propanol, n-butanol, sec-butanol, 2-ethyl-1-hexanol, 2-methoxyethanol, 2-ethoxyethanol, and 2-butoxyethanol. There is no particular limitation on the amide compound, and examples thereof include acetanilide, acetamide, ε-caprolactam, δ-valerolactam, and γ-butyrolactam. There is no particular limitation on the imide compound, and examples thereof include succinimide and maleimide. There is no particular limitation on the phenolic compound, and examples thereof include phenol, cresol, ethylphenol, butylphenol, nonylphenol, dinonylphenol, styrenated phenol, and hydroxybenzoic acid esters. There is no particular limitation on the amine compound, and examples thereof include diphenylamine, aniline, carbazole, di-n-propylamine, diisopropylamine, and isopropylethylamine. There is no particular limitation on the active methylene compound, and examples thereof include dimethyl malonate, diethyl malonate, methyl acetoacetate, ethyl acetoacetate, and acetylacetone. There is no particular limitation on the imidazole compound, and examples thereof include imidazole and 2-methylimidazole. There is no particular limitation on the pyrazole compound, and examples thereof include pyrazole, 3-methylpyrazole, and 3,5-dimethylpyrazole.

[0226] In addition, among the above-mentioned polyisocyanate compounds, from the aspect of weather resistance and pot life, diisocyanates or triisocyanates of aliphatic or alicyclic systems, aralkylene diisocyanates or polyisocyanates derived therefrom are particularly preferred. In addition, as the polyisocyanate, it is preferred to have structures such as biuret, isocyanurate, carbamate, uretdione, allophanate in the molecule. Polyisocyanates with biuret structure are excellent in adhesion in most cases. Polyisocyanates with isocyanurate structure are excellent in weather resistance in most cases. Polyisocyanates with carbamate structure using alcohol compounds with long side chains are excellent in elasticity and stretchability in most cases. Polyisocyanates with uretdione structure or allophanate structure are low viscosity in most cases.

[0227] As an isocyanate compound, from the aspect of water dispersibility, it is preferred that the polyisocyanate compound having two or more isocyanate groups in one molecule is reacted with a hydroxyl-containing hydrophilic compound having a nonionic and / or ionic hydrophilic group with an isocyanate group / hydroxyl equivalent ratio in the range of 1.05 to 1000. More preferably, the equivalent ratio is in the range of 2 to 200, and further preferably in the range of 4 to 100. By making the equivalent ratio above 1.05, the isocyanate group content in the hydrophilic polyisocyanate can be above a specific level, so that the crosslinking points in the crosslinkable water-based coating composition increase, so that the curing speed increases, or the strength of the coating such as the coating film is improved, which is preferred. By making the equivalent ratio below 1000, hydrophilicity can be exhibited, which is preferred. The water-dispersible isocyanate compound is not particularly limited, and a commercial product may be used. For example, WT30-100 manufactured by Asahi Kasei Corporation and WM44-L70G manufactured by Asahi Kasei Corporation are preferably used as commercial products having the above characteristics.

[0228] As the water-dispersible isocyanate compound, any one having a hydrophilic group introduced therein by a conventionally known method can be used without particular limitation. 1 O(R 2 O) n -H (here, R 1 represents an alkyl group having 1 to 30 carbon atoms or a group containing two or more aromatic rings, R 2 represents an alkylene group having 1 to 5 carbon atoms. n is an integer of 2 to 250) and a reaction product of a compound (m) represented by and a polyisocyanate compound; a reaction product of a vinyl polymer having a hydrophilic group and a hydroxyl group and a polyisocyanate compound; a reaction product of an emulsifier obtained by reacting an alkoxypolyalkylene glycol with a dialkanolamine and a polyisocyanate compound, etc. Among these, the reaction product of the compound (m) and a polyisocyanate compound, and the reaction product of a vinyl polymer having a hydrophilic group and a hydroxyl group and a polyisocyanate compound are excellent in water dispersibility and are therefore particularly preferred.

[0229] Examples of the compound (m) include alkoxypolyalkylene glycols such as polymethylene glycol monomethyl ether, polyethylene glycol monomethyl ether, polyethylene glycol monoethyl ether, polyethylene glycol monopropyl ether, polyethylene glycol monolauryl ether, polyoxyethylene-oxypropylene (random and / or block) glycol monomethyl ether, polyoxyethylene-oxytetramethylene (random and / or block) glycol polybutylene glycol monomethyl ether, and nonionic surfactants having a group containing two or more aromatic rings such as (mono to penta) styrenated phenyl groups, mono (or di or tri) styrenated-methyl-phenyl groups, tribenzylphenyl groups, and β-naphthyl groups. Among these, polyethylene glycol monomethyl ether and nonionic surfactants having (mono to penta) styrenated phenyl groups are preferred from the aspects of self-emulsification ability and pot life.

[0230] As these compounds (m), compounds having a molecular weight in the range of preferably 100 to 10,000, more preferably 300 to 5,000 can be suitably used.

[0231] As the hydrophilic group of the vinyl polymer having a hydrophilic group and a hydroxyl group, various known anionic groups, cationic groups, and nonionic groups can be enumerated, preferably nonionic groups. By being a nonionic group, the pot life of the coating composition can be significantly extended, and the particle size of the polyisocyanate oil droplets can be reduced in addition, so there is a tendency to further improve the water resistance of the formed coating film.

[0232] Specific examples of the vinyl polymer having a hydrophilic group and a hydroxyl group include acrylic polymers, fluoroolefin polymers, vinyl ester polymers, aromatic vinyl polymers, polyolefin polymers, etc. Among these, acrylic polymers are preferred from the perspective of weather resistance of the coating film formed.

[0233] The polymerization method for obtaining an acrylic polymer suitable as a vinyl polymer having a hydrophilic group and a hydroxyl group is not particularly limited, and examples thereof include suspension polymerization, emulsion polymerization, or solution polymerization. Preferably, the acrylic polymer is obtained by solution polymerization of an ethylenically unsaturated monomer (i) having a hydrophilic group and an ethylenically unsaturated monomer (ii) having a hydroxyl group, and other ethylenically unsaturated monomers (iii) copolymerizable with these monomers may be used as required.

[0234] As the ethylenically unsaturated monomer (i) having a hydrophilic group, for example, alkoxypolyalkylene glycol (meth)acrylates such as methoxypolyethylene glycol (meth)acrylate, ethoxypolyethylene glycol (meth)acrylate, butoxypolyethylene glycol (meth)acrylate, polyalkylene glycol di(meth)acrylates such as polyethylene glycol di(meth)acrylate, (meth)acrylamide monomers, anionic vinyl monomers, etc. can be cited. In addition, ethylenically unsaturated monomers having both a hydrophilic group and a hydroxyl group in the molecule such as polyalkylene glycol (meth)acrylates can also be used. These can be used alone or in combination of two or more.

[0235] In addition, other ethylenically unsaturated monomers (iii) copolymerizable with these monomers include, for example, (meth)acrylates, aromatic vinyl compounds, vinyl cyanides, carbonyl group-containing vinyl monomers, olefins, dienes, halogenated olefins, vinyl ethers, allyl esters, etc. These monomers may be used alone or in combination of two or more.

[0236] As the vinyl polymer containing a hydrophilic group and a hydroxyl group, a polymer having a weight average molecular weight (polystyrene conversion GPC method) in the range of preferably 2,000 to 100,000, more preferably 3,000 to 50,000 can be suitably used.

[0237] Regarding the content of the isocyanate compound (M) in the coating composition (J) relative to the adhesive emulsion particles (F) formed by polymerization of monomers including a hydroxyl-containing vinyl monomer, the ratio of the number of moles of hydroxyl groups contained in the adhesive emulsion particles (F) to the number of moles of isocyanate groups contained in the isocyanate compound (C) (X = number of moles of isocyanate groups / number of moles of hydroxyl groups) is preferably 0.02 or more. From the aspect of the close adhesion between the formed coating film and the substrate, X is more preferably 0.1 or more, and from the aspect of the scratch resistance of the coating film, X is more preferably 0.15 or more. In addition, from the aspect of the stability of the coating composition (resistance to gelation and high viscosity), X is preferably 10 or less, and from the aspect of the low water contact angle and high transparency (low HAZE) of the formed coating film, X is more preferably 5 or less. The ratio (X) may be 0.02 to 10, 0.02 to 5, 0.1 to 10, 0.1 to 5, 0.15 to 10, or 0.15 to 5.

[0238] As one embodiment, the mass ratio of the isocyanate compound to the adhesive latex particles (F) and the inorganic oxide (G) (mass of the isocyanate compound / total mass of the adhesive latex particles (F) and the inorganic oxide (G)) is preferably 0.001 or more, more preferably 0.01 or more, and further preferably 0.05 or more from the aspect of adhesion. In addition, from the aspect of transparency, the mass ratio is preferably 1.0 or less, more preferably 0.7 or less, and further preferably 0.5 or less.

[0239] In addition, the viscosity of the isocyanate compound (M) is preferably 1 to 50,000 mPa·s (20°C), more preferably 1 to 20,000 mPa·s (20°C), and further preferably 10 to 10,000 mPa·s (20°C). The viscosity of the isocyanate compound (C) may be 10 to 50,000 mPa·s (20°C), 10 to 20,000 mPa·s (20°C), or 10 to 10,000 mPa·s (20°C). When the viscosity of the polyisocyanate compound (M) is 50,000 mPa·s or less, it is easily dispersed in water, and thus is preferred. The viscosity here can be measured using a conventional E-type viscometer. In one embodiment, the viscosity is measured using an E-type viscometer (RE-80U manufactured by Toki Sangyo Co., Ltd.) at a rotation speed of 2.5 rpm and 25°C. The isocyanate compound is not particularly limited, and a commercially available product may be used. For example, WT30-100 manufactured by Asahi Kasei Corporation and WM44-L70G manufactured by Asahi Kasei Corporation are preferably used as commercially available products having the above characteristics.

[0240] Among the various isocyanate compounds described above, a part or the entire amount thereof may react with a polyol to form a urethane compound.

[0241] <Method for preparing adhesive layer>

[0242] The method for preparing the adhesive layer in the present embodiment is not particularly limited. For example, adhesive latex particles (F), inorganic oxides (G), sunscreens, and other suitable components can be dispersed and dissolved in a solvent, and the obtained coating composition (J) is applied to the above-mentioned substrate, and a coating film is made by heat treatment, ultraviolet irradiation, infrared irradiation, etc., thereby obtaining the adhesive layer. It should be noted that, with respect to adhesive latex particles (F) and inorganic oxides (G), they can also be made into a composite in advance for use. In addition, as the above-mentioned coating method, it is possible to cite, but not limited to, for example, spray coating, flow coating, brush coating, dip coating, spin coating, screen printing, casting, gravure printing, flexographic printing, etc. It should be noted that the coating composition (J) after the above-mentioned coating can be made into a coating film by heat treatment or ultraviolet irradiation, infrared irradiation, etc., preferably at room temperature to 250°C, more preferably at a temperature of 40°C to 150°C. Furthermore, the coating can be applied not only to an already formed substrate but also to a flat plate in advance before the forming process, such as pre-coated metal including rustproof steel sheet.

[0243] [Coating composition (J)]

[0244] The coating composition (J) in this embodiment is a coating composition comprising a mixture of adhesive emulsion particles (F) and an inorganic oxide (G) and / or a complex of the inorganic oxide (G) and the adhesive emulsion particles (F), and comprising a sunscreen (S1), wherein the average particle size of the mixture and / or the complex is preferably greater than 2 nm and less than 2000 nm, and the mass ratio of the inorganic oxide (G) to the adhesive emulsion particles (F) is 1:0.1 to 1:10.

[0245] The average particle size can be measured by the method described in Examples below.

[0246] It should be noted that when the coating composition (J) contains a mixture of adhesive emulsion particles (F) and an inorganic oxide (G), when the average particle size of the adhesive emulsion particles (F) and the primary average particle size of the inorganic oxide (G) are both greater than 2 nm and less than 2000 nm, the average particle size of the mixture is greater than 2 nm and less than 2000 nm.

[0247] The coating composition (J) may contain a solvent, and as the solvent, a solvent that can be used in the coating composition (I) described later can be appropriately used.

[0248] Among the components contained in the coating composition (J), the details of the aspects not mentioned below are the same as those described above for the components contained in the adhesive layer.

[0249] [Complex of adhesive emulsion particles (F) and inorganic oxide (G)]

[0250] The adhesive latex particles (F) and the inorganic oxide (G) contained in the coating composition (J) may be mixed separately, or a composite of the adhesive latex particles (F) and the inorganic oxide (G) may be formed in advance. The composite of the adhesive latex particles (F) and the inorganic oxide (G) is obtained, for example, by polymerizing the vinyl monomer of the adhesive latex particles (F) in the presence of the inorganic oxide (G).

[0251] Among the vinyl monomers, from the aspect of interaction with the inorganic oxide (G), it is preferred to include the above-mentioned vinyl monomers having secondary amide groups and / or tertiary amide groups. A complex can be formed ideally by hydrogen bonding of the hydroxyl group of the inorganic oxide (G) with the secondary amide groups and / or tertiary amide groups.

[0252] Regarding the average particle size of the mixture of adhesive emulsion particles (F) and inorganic oxide (G) and / or the complex of adhesive emulsion particles (F) and inorganic oxide (G) in this embodiment, from the perspective of good storage stability of the raw material composition of the adhesive layer, it is more preferably not less than 20 nm, and from the perspective of transparency, it is preferably not more than 2000 nm, more preferably not more than 1000 nm, and further preferably not more than 500 nm.

[0253] The average particle size can be measured by the method described in the examples below, and can be adjusted to the above range by, for example, adjusting the mass ratio or solid content concentration of the adhesive emulsion particles (F) and the inorganic oxide (G).

[0254] The mass ratio of the adhesive emulsion particles (F) to the inorganic oxide (G) in the coating composition (J) is preferably 1:0.1 to 1:10, more preferably 1:0.3 to 1:5, and even more preferably 1:0.5 to 1:2.

[0255] The inorganic oxide (G) in the coating composition (J) is preferably spherical and / or linked silicon oxide, and the above-mentioned substances as spherical and / or linked silicon oxide contained in the bonding layer can be suitably used. There is no particular limitation on spherical silicon oxide, and commercial products can also be used, for example, Snowtex C and Snowtex OS manufactured by Nissan Chemical Industries, Ltd. are preferably used. In addition, there is no particular limitation on linked silicon oxide, and commercial products can also be used, for example, Snowtex PSSO manufactured by Nissan Chemical Industries, Ltd. is preferably used.

[0256] The aspect ratio (long diameter / short diameter) of the inorganic oxide (G) in the coating composition (J) is preferably 3 to 25. The aspect ratio can be measured based on the method described in the examples described below. The inorganic oxide (G) having the aspect ratio is not particularly limited, and a commercially available product may be used, for example, Snowtex PSSO manufactured by Nissan Chemical Industries, Ltd. is preferably used.

[0257] The coating composition (J) contains a sunscreen (S1), and the sunscreen (S1) contained in the adhesive layer can be suitably used as the sunscreen. In the present embodiment, the sunscreen (S1) preferably contains a UV absorber, and the UV absorber contained in the adhesive layer can be suitably used as the UV absorber.

[0258] The coating composition (J) preferably further contains a hindered amine light stabilizer, and the hindered amine light stabilizer contained in the adhesive layer may be preferably the hindered amine light stabilizer described above.

[0259] In the coating composition (J), the adhesive latex particles (F) preferably contain a functional group (e) having a secondary amide group and / or a tertiary amide group. The functional group (e) having a secondary amide group and / or a tertiary amide group is not particularly limited, and for example, the functional group exemplified as the functional group (e) having a secondary amide group and / or a tertiary amide group in the coating composition (I) described later can be suitably used.

[0260] In the coating composition (J), the adhesive latex particles (F) preferably contain a functional group having a hydroxyl group. The functional group having a hydroxyl group is not particularly limited, and for example, the functional groups exemplified as the functional group having a hydroxyl group in the coating composition (I) described below can be appropriately used.

[0261] [Isocyanate compound]

[0262] In the coating composition (J), from the aspect of improving the adhesion between the adhesive layer and the substrate, it is preferred to contain an isocyanate compound and / or a carbamate compound, and it is more preferred that the isocyanate compound is a water-dispersible isocyanate compound, and it is further preferred that the water-dispersible isocyanate compound is a blocked isocyanate. There is no particular limitation on the isocyanate compound and / or carbamate compound, and for example, the substances described above as the isocyanate compound and / or carbamate compound in the adhesive layer can be suitably used. In addition, the water-dispersible isocyanate compound or the blocked isocyanate can also suitably use the substances described above as the water-dispersible isocyanate compound and the blocked isocyanate in the adhesive layer.

[0263] [Properties of coating composition (J)]

[0264] In the coating composition (J), from the viewpoint of coating properties, the solid content concentration is preferably 0.01 to 60% by mass, more preferably 1 to 40% by mass. In addition, from the viewpoint of coating properties, the viscosity of the coating composition (J) at 20° C. is preferably 0.1 to 100,000 mPa·s, more preferably 1 to 10,000 mPa·s.

[0265] [Hard coating]

[0266] The hard coating layer (hereinafter also referred to as "layer (C)") in this embodiment is disposed on the substrate with the adhesive layer and comprises a matrix component (B) containing an inorganic oxide (D), which contributes to the durability of the laminate. It should be noted that in this specification, the Martens hardness HM is 100 N / mm 2 The above layer is particularly referred to as a "hard coat layer".

[0267] In this embodiment, from the aspect of wear resistance, in the hard coating layer, it is preferred that the hard coating layer further comprises polymer nanoparticles (A) dispersed in the matrix component (B), and the Martens hardness HM of the polymer nanoparticles (A) is A The Martens hardness HM of the matrix component (B) B Meet HM B / HM A >1, the Martens hardness HM of the hard coating is 100N / mm 2 above.

[0268] It should be noted that it is difficult to confirm the above Martens hardness HM A and Martens hardness HM B In the case of the size relationship of the polymer nanoparticles (A) and the matrix component (B) described later, the size relationship of the Martens hardness can also be inferred by comparing the adhesion of the polymer nanoparticles (A) and the matrix component (B) described later. The lower the adhesion, the higher the elasticity, so the lower the adhesion, the less likely the coating is to deform, indicating that the hardness is higher. Specifically, the preferred layer (C) can also be defined as follows. That is, the preferred layer (C) comprises polymer nanoparticles (A) and the matrix component (B), and the adhesion F of the polymer nanoparticles (A) measured by the adhesion mode of the scanning probe microscope (SPM) is A Adhesion F to the above matrix component (B) B Satisfy F A / F B >1, the Martens hardness HM of the hard coating is 100N / mm 2 above.

[0269] In the layer (C) of the present embodiment, the polymer nanoparticles (A) are preferably dispersed in the matrix component (B). "Dispersion" in the present embodiment refers to using the polymer nanoparticles (A) as a dispersed phase and the matrix component (B) as a continuous phase, so that the polymer nanoparticles (A) are evenly distributed in the matrix component (B) or distributed in the matrix component (B) while forming a structure. The above dispersion can be confirmed by cross-sectional SEM observation of the hard coat. In the hard coat in the present embodiment, the polymer nanoparticles (A) are dispersed in the matrix component (B) and tend to have high wear resistance.

[0270] [Martens hardness]

[0271] The Martens hardness in the present embodiment is the hardness obtained according to ISO14577-1, and is the value calculated by the indentation depth of 2mN under the measuring conditions (Vickers tetrahedral pyramid diamond indenter, the increase condition of load 2mN / 20sec, the reduction condition of load 2mN / 20sec). The Martens hardness in the present embodiment can be measured using, for example, a micro-hardness meter Fischer scope (Fischer Instruments manufactures HM2000S), an ultra-micro indentation hardness tester (Elionix Co., Ltd. manufactures ENT-NEXUS), a nano-indenter (Toyo Technica manufactures iNano, G200), and a nano-indentation system (Bruker manufactures TI980), and the shallower the indentation depth, the higher the Martens hardness, and the deeper the indentation depth, the lower the Martens hardness.

[0272] [Adhesion]

[0273] The adhesion in this embodiment can be measured using a scanning probe microscope (SPM). Since the lower the adhesion, the higher the elasticity, the lower the adhesion, the less likely the coating is to deform and the higher the hardness. The adhesion measurement method can be measured using, but not limited to, SPM-970, SPM-9700HT manufactured by Shimadzu Corporation, Dimension ICON manufactured by Bruker AXS, AFM5000II manufactured by Hitachi High-Tech Science, etc.

[0274] [Other hardness]

[0275] By determining the magnitude relation of measured values ​​as indexes with other hardnesses, the magnitude relation of Martens hardness and adhesive force in the above-mentioned present embodiment can also be inferred.As other hardnesses, as long as the index that the deformation of material is not easy to be represented after the material is applied with force is not particularly limited, the index represented by the logarithmic decrement rate measured by the Vickers hardness, indentation hardness, and the pendulum type viscoelasticity instrument represented by the rigid pendulum type physical property testing machine can be enumerated, which is measured by a microhardness meter, a nanoindentation tester as a representative, and measured by a pendulum type viscoelasticity instrument.In addition, the index represented by the phase, friction, viscoelasticity, adsorption, hardness and elastic modulus measured by a scanning probe microscope (SPM) can also be enumerated.In these indexes, if it is confirmed that the hardness of the matrix component (B) is higher than the hardness of polymer nanoparticles (A), then with regard to Martens hardness and adhesive force, it can also be inferred that the matrix component (B) is harder than polymer nanoparticles (A).

[0276] [Martens hardness HM of polymer nanoparticles (A) A Martens hardness HM of matrix component (B) B ]

[0277] The Martens hardness HM of the polymer nanoparticles (A) in this embodiment is A Martens hardness HM of matrix component (B) B It is preferable to satisfy the relationship of the following formula (1).

[0278] HM B / HM A >1 Formula (1)

[0279] Formula (1) indicates that soft polymer nanoparticles (A) exist in a hard matrix component (B). By making the hardness three-dimensionally inclined, layer (C) tends to be able to impart wear resistance that is not exhibited in conventional coatings. The reason for this is not intended to be limiting, but it is presumed that the soft nanoparticles absorb impacts and the hard matrix component suppresses deformation. As HM A In terms of impact absorption, 50 N / mm is preferred. 2 More preferably 100 N / mm 2 From the viewpoint of film forming properties, 2000 N / mm is preferred. 2 Below, more preferably 800N / mm 2 Below, more preferably 350N / mm 2 Below. As HM B The range is preferably 100 N / mm from the perspective of impact absorption. 2 More preferably 150N / mm 2 The above, preferably 4000 N / mm from the viewpoint of film forming properties 2Below, more preferably 2000N / mm 2 the following.

[0280] It should be noted that the layer (C) can be obtained in the form of a cured product, which is obtained by curing the coating composition (I) described later by hydrolysis condensation or the like. For the polymer nanoparticles (A), the composition thereof usually does not change during the curing process. Therefore, the Martens hardness HM of the polymer nanoparticles (A) in the coating composition (I) measured by the method described in the examples described later is A The value of is related to the Martens hardness HM of the polymer nanoparticles (A) in the layer (C) A In good agreement, the Martens hardness HM in layer (C) can be determined in this form A The value of .

[0281] In addition, the matrix component (B) corresponds to a cured product obtained by curing the matrix raw material component (B') described later by hydrolysis condensation or the like. Therefore, the Martens hardness HM of the matrix raw material component (B') measured by the method described in the examples described later is B’ The value of the corresponding matrix component (B) is the Martens hardness HM B In good agreement, the Martens hardness HM can be determined in this form B The value of .

[0282] The above HM A and H.M. B The values ​​of can be adjusted to the above-mentioned magnitude relationship by the structures and composition ratios of the constituent components of the polymer nanoparticles (A) and the matrix raw material component (B') described later, and the method is not particularly limited.

[0283] [Adhesion force F of polymer nanoparticles (A) A Adhesion F to matrix component (B) B ]

[0284] The adhesion force F of the polymer nanoparticles (A) in this embodiment is A Adhesion F to the matrix component (B) B It is preferable to satisfy the relationship of the following formula (2).

[0285] F A / F B >1 Formula (2)

[0286] Similar to the above formula (1), formula (2) also indicates that there are soft polymer nanoparticles (A) in the hard matrix component (B), and by making the hardness have a three-dimensional inclination like this, the layer (C) has a tendency to be able to impart wear resistance that is not shown in the existing coating film. The reason for this is not intended to be limited, but it is presumed that the soft nanoparticles absorb impact and the hard matrix component suppresses deformation.

[0287] As mentioned above, the adhesion force F of the polymer nanoparticles (A) A Adhesion F to matrix component (B) B The hardness of each component can be adjusted to the above-mentioned size relationship by adjusting the structure and composition ratio of the constituent components of the polymer nanoparticles (A) and the matrix raw material component (B') described later, and the method is not particularly limited.

[0288] [Martens hardness HM of layer (C)]

[0289] The Martens hardness HM of the layer (C) is 100 N / mm from the viewpoint of wear resistance. 2 As described above, the higher the Martens hardness HM, the less deformation due to impact and the less damage associated with destruction, which is advantageous from this point of view. The Martens hardness HM of the layer (C) is preferably 100 N / mm 2 More preferably 150N / mm 2 More preferably, 200 N / mm 2 From the perspective of flexural resistance, 4000 N / mm is preferred. 2 Below, more preferably 2000N / mm 2 Below, more preferably 1500N / mm 2 As follows. As a method for adjusting the Martens hardness HM of the layer (C) to the above range, there can be cited, but not limited to, for example, mixing the polymer nanoparticles (A) satisfying the specific relationship represented by the formula (3) described later with the matrix raw material component (B') described later and dispersing and dissolving the obtained composition in a solvent, applying the obtained coating composition to a substrate, and forming a coating film by heat treatment, ultraviolet irradiation, infrared irradiation, etc. In particular, if the content of the matrix component (B) increases relative to the total amount of the polymer nanoparticles (A) and the matrix component (B), the Martens hardness HM of the layer (C) tends to increase, and if the content of the matrix component (B) decreases, the Martens hardness HM of the layer (C) tends to decrease.

[0290] [Haze change in Taber abrasion test]

[0291] The Taber abrasion test in this embodiment is carried out according to the method described in ASTM D1044, and is measured under the conditions of abrasion wheel CS-10F and a load of 500 g. The smaller the change in haze, the better the wear resistance of the material. When the change in haze at 500 rotations relative to the haze before the test, that is, the difference between the haze at 500 rotations and the haze before the Taber abrasion test is 10 or less, it is suitable for the standard of ECE R43 rear side glass, and when it is 4 or less, it is suitable for the standard of ANSI / SAE Z.26.1 and can be suitably used as a window material for automobiles. In addition, when the haze change at 1000 rotations, that is, the difference between the haze at 1000 rotations and the haze before the Taber abrasion test is 10 or less, it is suitable for the standard of automobile windows and can be suitably used as automobile window materials. When it is 2 or less, it is suitable for the standards of ANSI / SAE Z.26.1, ECE R43, and JISR3211 / R3212 and can be suitably used for all automobile window materials. It is preferred that the haze change at 1000 rotations is 10 or less, more preferably 6 or less, and further preferably 2 or less. As a method for adjusting the haze change within the above range, for example, polymer nanoparticles (A) satisfying the specific relationship represented by formula (3) described later and matrix raw material component (B') described later are mixed and the obtained composition is dispersed and dissolved in a solvent, the obtained coating composition is applied on a substrate, and a coating film is formed by heat treatment, ultraviolet irradiation, infrared irradiation, etc.

[0292] [Elastic recovery factor η of layer (C) IT ]

[0293] Elastic recovery rate η of layer (C) IT is the total mechanical work done by the depression W total The amount of work done by the elastic recovery deformation of the concave elast The ratio is defined as “W elast / W total The ratio η IT "Parameters recorded. Elastic recovery rate η IT The higher the value, the more the coating can recover to its original state after deformation, and the higher the self-repair ability of the deformation. IT Under the measurement conditions (Vickers tetrahedral diamond indenter, load increase condition 2mN / 20sec, load decrease condition 2mN / 20sec), it is preferably 0.50 or more. If it is within this range, the larger the value, the more preferred. More specifically, the elastic recovery rate η ITMore preferably, it is 0.55 or more, further preferably 0.60 or more, and further preferably 0.65 or more. The elastic recovery rate of the coating film in the present embodiment can be measured by, but not limited to, for example, using a micro hardness meter Fischer scope (HM2000S manufactured by Fischer Instruments), an ultra-micro indentation hardness tester (ENT-NEXUS manufactured by Elionix Co., Ltd.), a nanoindenter (iNano, G200 manufactured by Toyo Technica), a nanoindentation system (TI980 manufactured by Bruker), etc. to perform an indentation test to measure the surface of the hard coating. As a method for measuring the elastic recovery rate η IT The method for adjusting to the above range may include, but is not limited to, mixing polymer nanoparticles (A) satisfying the specific relationship represented by formula (3) described later with the matrix raw material component (B') described later, dispersing and dissolving the obtained composition in a solvent, applying the obtained coating composition on a substrate, and forming a coating film by heat treatment, ultraviolet irradiation, infrared irradiation, etc.

[0294] [Thickness of layer (C)]

[0295] In the present embodiment, from the aspect of further demonstrating the wear resistance of the hard coating layer and from the aspect of fully ensuring the followability to the deformation of the substrate, it is preferred to appropriately adjust the film thickness. Specifically, from the aspect of wear resistance, the film thickness of the layer (C) is preferably 1.0 μm or more, more preferably 3.0 μm or more. In addition, from the aspect of substrate followability, the film thickness of the layer (C) is preferably 100.0 μm or less, more preferably 50.0 μm or less, and further preferably 20.0 μm or less.

[0296] [Polymer nanoparticles (A)]

[0297] By using the polymer nanoparticles (A) in this embodiment, it is possible to impart impact absorption to the hard coating layer, and it is possible to reduce the tendency of the change in the haze of the hard coating layer in the Taber abrasion test. Regarding the polymer nanoparticles (A), as long as the particle size is of the order of nm (less than 1 μm), there is no particular limitation on the shape. It should be noted that the Martens hardness HM of the polymer nanoparticles (A) is A The above range can be controlled by the structure and composition ratio of the constituent components of the polymer nanoparticles (A), and the method is not particularly limited.

[0298] [Average particle size of polymer nanoparticles (A)]

[0299] The average particle size of the polymer nanoparticles (A) in this embodiment is not particularly limited as long as it is of the order of nm (less than 1 μm), and is obtained by observing the particle size by cross-sectional SEM or dynamic light scattering. From the perspective of optical properties, the average particle size of the polymer nanoparticles (A) is preferably greater than 10 nm, more preferably greater than 15 nm, and more preferably greater than 20 nm. From the perspective of transparency, it is preferably less than 400 nm, more preferably less than 200 nm, and further preferably less than 100 nm. The method for determining the average particle size of the polymer nanoparticles (A) can be, for example, but not limited to, by measuring the cumulative particle size using a dynamic light scattering particle size distribution measuring device (model: ELSZ-1000) manufactured by Otsuka Electronics Co., Ltd. using an aqueous dispersion of the polymer nanoparticles (A).

[0300] [Volume fraction of polymer nanoparticles (A) in layer (C)]

[0301] In this embodiment, the volume fraction of the polymer nanoparticles (A) in the layer (C) is preferably 2% or more, more preferably 3% or more, and further preferably 5% or more from the perspective of film-forming properties, and is preferably 80% or less, more preferably 70% or less, and further preferably 45% or less from the perspective of transparency. The volume fraction of the polymer nanoparticles (A) in the layer (C) can be calculated, for example, based on the proportion of the polymer nanoparticles (A) in the entire coating film in the cross-sectional SEM image of the layer (C) and the component ratio of the polymer nanoparticles (A) in the components constituting the layer (C).

[0302] [Constitutional components of polymer nanoparticles (A)]

[0303] [Hydrolyzable silicon compound (a)]

[0304] The polymer nanoparticles (A) in the present embodiment preferably contain a hydrolyzable silicon compound (a). The hydrolyzable silicon compound (a) is not particularly limited as long as it is a hydrolyzable silicon compound, a hydrolyzate thereof, or a condensate thereof.

[0305] From the viewpoint of improving abrasion resistance and weather resistance, the hydrolyzable silicon compound (a) is preferably a compound containing an atomic group represented by the following formula (a-1), or a hydrolyzate or condensate thereof.

[0306] -R 1 n1 SiX 1 3-n1 (a-1)

[0307] In formula (a-1), R 1 represents a hydrogen atom, an alkyl group, an alkenyl group, an alkynyl group or an aryl group having 1 to 10 carbon atoms, and R 1It may have a substituent containing a halogen, hydroxyl, mercapto, amino, (meth)acryloyl or epoxy group, X 1 represents a hydrolyzable group, and n1 represents an integer of 0 to 2. The hydrolyzable group is not particularly limited as long as it is a group that generates a hydroxyl group by hydrolysis, and examples of such a group include halogen, alkoxy, acyloxy, amino, phenoxy, and oxime groups.

[0308] Specific examples of compounds containing the atomic group represented by formula (a-1) include, but are not limited to, trimethoxysilane, triethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, propyltrimethoxysilane, propyltriethoxysilane, isobutyltriethoxysilane, hexyltrimethoxysilane, hexyltriethoxysilane, octyltrimethoxysilane, octyltriethoxysilane, decyltrimethoxysilane, decyltriethoxysilane, cyclohexyltrimethoxysilane, cyclohexyltriethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, dimethoxysilane, diethoxysilane, methyldimethoxysilane, methyldiethoxysilane, Dimethyldimethoxysilane, dimethyldiethoxysilane, dimethoxydiphenylsilane, diethoxydiphenylsilane, bis(trimethoxysilyl)methane, bis(triethoxysilyl)methane, bis(triphenoxysilyl)ethane, 1,1-bis(triethoxysilyl)ethane, 1,2-bis(triethoxysilyl)ethane, 1,1-bis(triethoxysilyl)propane, 1,2-bis(triethoxysilyl)propane, 1,3-bis(triethoxysilyl)propane, 1,4-bis(triethoxysilyl)butane, 1,5-bis(triethoxysilyl)pentane, 1,1-bis(trimethoxysilyl)ethane, 1,2-bis(trimethoxysilyl) 1,1-bis(trimethoxysilyl)propane, 1,2-bis(trimethoxysilyl)propane, 1,3-bis(trimethoxysilyl)propane, 1,4-bis(trimethoxysilyl)butane, 1,5-bis(trimethoxysilyl)pentane, 1,3-bis(triphenoxysilyl)propane, 1,4-bis(trimethoxysilyl)benzene, 1,4-bis(triethoxysilyl)benzene, 1,6-bis(trimethoxysilyl)hexane, 1,6-bis(triethoxysilyl)hexane, 1,7-bis(trimethoxysilyl)heptane, 1,7-bis(triethoxysilyl)heptane, 1,8-bis(trimethoxysilyl)octane, 1, 8-Bis(triethoxysilyl)octane, 3-chloropropyltrimethoxysilane, 3-chloropropyltriethoxysilane, trifluoropropyltrimethoxysilane, trifluoropropyltriethoxysilane, 3-hydroxypropyltrimethoxysilane, 3-hydroxypropyltriethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropylmethyldiethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane,4-epoxycyclohexyl)ethyl triethoxysilane, 3-acryloxypropyl trimethoxysilane, 3-acryloxypropyl triethoxysilane, 3-methacryloxypropyl trimethoxysilane, 3-methacryloxypropyl triethoxysilane, 3-methacryloxypropyl methyl dimethoxysilane, 3-methacryloxypropyl methyl dimethoxysilane, vinyl trimethoxysilane, vinyl triethoxysilane, p-phenylene trimethoxysilane, p-phenylene triethoxysilane, N-2-(aminoethyl)-3-aminopropyl methyl dimethoxysilane, N-2 -(Aminoethyl)-3-aminopropylmethyldiethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane, N-phenyl-3-aminopropyltriethoxysilane, 3-trimethoxysilyl-N-(1,3-dimethyl-butylene)propylamine, 3-triethoxysilyl-N-(1,3-dimethyl-butylene)propylamine, triacetoxysilane, Tris(trichloroacetoxy)silane, tris(trifluoroacetoxy)silane, tris(trimethoxysilylpropyl)isocyanurate, tris(triethoxysilylpropyl)isocyanurate, methyltriacetoxysilane, methyltris(trichloroacetoxy)silane, trichlorosilane, tribromosilane, methyltrifluorosilane, tris(methylethylketoxime)silane, phenyltris(methylethylketoxime)silane, bis(methylethylketoxime)silane, methylbis(methylethylketoxime)silane, hexamethyldisilane, hexamethylcyclotrisilazane, bis(dimethylamino)dimethylsilane, bis(diethylamino)dimethylsilane, (Dimethylamino) methylsilane, bis(diethylamino) methylsilane, 2-[(triethoxysilyl) propyl] dibenzylresorcinol, 2-[(trimethoxysilyl) propyl] dibenzylresorcinol, 2,2,6,6-tetramethyl-4-[3-(triethoxysilyl) propoxy] piperidine, 2,2,6,6-tetramethyl-4-[3-(trimethoxysilyl) propoxy] piperidine, 2-hydroxy-4-[3-(triethoxysilyl) propoxy] benzophenone, 2-hydroxy-4-[3-(trimethoxysilyl) propoxy] benzophenone, etc.

[0309] The hydrolyzable silicon compound (a) preferably includes a compound represented by the following formula (a-2), a hydrolyzate thereof, and a condensate thereof, from the viewpoint of being able to impart high hardness to the hard coat layer and further improving the wear resistance.

[0310] SiX 2 4(a-2)

[0311] In formula (a-2), X 2The hydrolyzable group is not particularly limited as long as it is a group that generates a hydroxyl group by hydrolysis, and examples thereof include halogen, alkoxy, acyloxy, amino, phenoxy, and oxime groups.

[0312] Specific examples of the compound represented by formula (a-2) include, but are not limited to, tetramethoxysilane, tetraethoxysilane, tetra(n-propoxy)silane, tetra(isopropoxy)silane, tetra(n-butoxy)silane, tetra(isobutoxy)silane, tetra-sec-butoxysilane, tetra-tert-butoxysilane, tetraacetoxysilane, tetra(trichloroacetoxy)silane, tetra(trifluoroacetoxy)silane, tetrachlorosilane, tetrabromosilane, tetrafluorosilane, tetra(methyl ethyl ketoxime)silane, and partially hydrolyzed condensates of tetramethoxysilane or tetraethoxysilane (e.g., trade names "M-Silicate 51", "Silicate 35", "Silicate 45", "Silicate 40", and "FR-3" manufactured by Tama Chemical Industries, Ltd.; trade names "MS51", "MS56", "MS57", and "MS56S" manufactured by Mitsubishi Chemical Corporation; trade names "Methyl Silicate 51", "Methyl Silicate 35", "Si ... 53A", "Ethyl Silicate40", "Ethyl Silicate 48", "EMS-485", "N-103X", "PX", "PS-169", "PS-162R", "PC-291", "PC-301", "PC-302R", "PC-309", "EMSi48"), etc.

[0313] As described above, in this embodiment, the hydrolyzable silicon compound (a) preferably includes one or more selected from the group consisting of compounds containing the atomic group represented by the above formula (a-1), their hydrolysis products and condensation products, and compounds represented by the above formula (a-2), their hydrolysis products and condensation products.

[0314] [Content of the hydrolyzable silicon compound (a) in the polymer nanoparticles (A)]

[0315] The content of the hydrolyzable silicon compound (a) in the present embodiment represents the solid content weight ratio of the hydrolyzable silicon compound (a) contained in the polymer nanoparticles (A). The higher the content, the better the wear resistance, weather resistance and heat resistance. The content is preferably 50% by mass or more, more preferably 60% by mass or more. The content of the hydrolyzable silicon compound (a) in the polymer nanoparticles (A) can be measured by, but not limited to, IR analysis, NMR analysis, elemental analysis, etc. of the polymer nanoparticles (A).

[0316] [Matrix component (B)]

[0317] By using the matrix component (B) in this embodiment, impact absorption can be imparted to the hard coat layer, and the amount of change in haze of the hard coat layer in the Taber abrasion test can be reduced. B The above range can be controlled by the structure and composition ratio of the constituent components of the matrix raw material component (B') described later, and the method is not particularly limited.

[0318] [Constituents of the matrix component (B)]

[0319] [Hydrolyzable silicon compound (b)]

[0320] The matrix component (B) in the present embodiment is not particularly limited as long as it is a component that can disperse the polymer nanoparticles (A). In the present embodiment, from the aspect of high toughness, the matrix component (B) preferably contains a hydrolyzable silicon compound (b). In this specification, "the matrix component (B) contains a hydrolyzable silicon compound (b)" means that the matrix component (B) contains a polymer having a structural unit derived from the hydrolyzable silicon compound (b). The hydrolyzable silicon compound (b) is not particularly limited as long as it is a hydrolyzable silicon compound, its hydrolyzate and condensate.

[0321] As the matrix component (B), in addition to the above-mentioned polymers, various components other than the polymer nanoparticles (A) may be included. Among them, as other polymers that may be included in addition to the above-mentioned polymers, water-soluble resins such as polyvinyl alcohol, polyethylene glycol, polyvinyl pyrrolidone, and polyacrylic acid; acrylic resins such as PMMA, PAN, and polyacrylamide; polymers such as polystyrene, polyurethane, polyamide, polyimide, polyvinylidene chloride, polyester, polycarbonate, polyether, polyethylene, polysulfone, polypropylene, polybutadiene, PTFE, PVDF, and EVA; and copolymers thereof, etc.

[0322] From the perspective of further improving wear resistance and weather resistance, the hydrolyzable silicon compound (b) preferably contains one or more selected from the group consisting of a compound containing an atomic group represented by the following formula (b-1), its hydrolysis products and condensation products, and a compound represented by the following formula (b-2), its hydrolysis products and condensation products.

[0323] -R 2 n2 SiX 3 3-n2 (b-1)

[0324] In formula (b-1), R 2 represents a hydrogen atom, an alkyl group, an alkenyl group, an alkynyl group or an aryl group having 1 to 10 carbon atoms, and R 2It may have a substituent containing a halogen, hydroxyl, mercapto, amino, (meth)acryloyl or epoxy group, X 3 represents a hydrolyzable group, and n2 represents an integer of 0 to 2. The hydrolyzable group is not particularly limited as long as it is a group that generates a hydroxyl group by hydrolysis, and examples of such a group include a halogen atom, an alkoxy group, an acyloxy group, an amino group, a phenoxy group, and an oxime group.

[0325] SiX 4 4(b-2)

[0326] In formula (b-2), X 4 The hydrolyzable group is not particularly limited as long as it is a group that generates a hydroxyl group by hydrolysis, and examples of such a group include halogen, alkoxy, acyloxy, amino, phenoxy, and oxime groups.

[0327] Specific examples of the compound containing the atomic group represented by the general formula (b-1) include, but are not limited to, trimethoxysilane, triethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, propyltrimethoxysilane, propyltriethoxysilane, isobutyltriethoxysilane, hexyltrimethoxysilane, hexyltriethoxysilane, octyltrimethoxysilane, octyltriethoxysilane, decyltrimethoxysilane, decyltriethoxysilane, cyclohexyltrimethoxysilane, cyclohexyltriethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, dimethoxysilane, diethoxysilane, methyldimethoxysilane, methyldiethoxysilane, dimethoxysilane Methyldimethoxysilane, dimethyldiethoxysilane, dimethoxydiphenylsilane, diethoxydiphenylsilane, bis(trimethoxysilyl)methane, bis(triethoxysilyl)methane, bis(triphenoxysilyl)ethane, 1,1-bis(triethoxysilyl)ethane, 1,2-bis(triethoxysilyl)ethane, 1,1-bis(triethoxysilyl)propane, 1,2-bis(triethoxysilyl)propane, 1,3-bis(triethoxysilyl)propane, 1,4-bis(triethoxysilyl)butane, 1,5-bis(triethoxysilyl)pentane, 1,1-bis(trimethoxysilyl)ethane, 1,2-bis(trimethoxysilyl) )ethane, 1,1-bis(trimethoxysilyl)propane, 1,2-bis(trimethoxysilyl)propane, 1,3-bis(trimethoxysilyl)propane, 1,4-bis(trimethoxysilyl)butane, 1,5-bis(trimethoxysilyl)pentane, 1,3-bis(triphenoxysilyl)propane, 1,4-bis(trimethoxysilyl)benzene, 1,4-bis(triethoxysilyl)benzene, 1,6-bis(trimethoxysilyl)hexane, 1,6-bis(triethoxysilyl)hexane, 1,7-bis(trimethoxysilyl)heptane, 1,7-bis(triethoxysilyl)heptane, 1,8-bis(trimethoxysilyl)octane, 1, 8-Bis(triethoxysilyl)octane, 3-chloropropyltrimethoxysilane, 3-chloropropyltriethoxysilane, trifluoropropyltrimethoxysilane, trifluoropropyltriethoxysilane, 3-hydroxypropyltrimethoxysilane, 3-hydroxypropyltriethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropylmethyldiethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane,4-epoxycyclohexyl)ethyl triethoxysilane, 3-acryloxypropyl trimethoxysilane, 3-acryloxypropyl triethoxysilane, 3-methacryloxypropyl trimethoxysilane, 3-methacryloxypropyl triethoxysilane, 3-methacryloxypropyl methyl dimethoxysilane, 3-methacryloxypropyl methyl dimethoxysilane, vinyl trimethoxysilane, vinyl triethoxysilane, p-phenylene trimethoxysilane, p-phenylene triethoxysilane, N-2-(aminoethyl)-3-aminopropyl methyl dimethoxysilane, N-2 -(Aminoethyl)-3-aminopropylmethyldiethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane, N-phenyl-3-aminopropyltriethoxysilane, 3-trimethoxysilyl-N-(1,3-dimethyl-butylene)propylamine, 3-triethoxysilyl-N-(1,3-dimethyl-butylene)propylamine, triacetoxysilane, Tris(trichloroacetoxy)silane, tris(trifluoroacetoxy)silane, tris(trimethoxysilylpropyl)isocyanurate, tris(triethoxysilylpropyl)isocyanurate, methyltriacetoxysilane, methyltris(trichloroacetoxy)silane, trichlorosilane, tribromosilane, methyltrifluorosilane, tris(methylethylketoxime)silane, phenyltris(methylethylketoxime)silane, bis(methylethylketoxime)silane, methylbis(methylethylketoxime)silane, hexamethyldisilane, hexamethylcyclotrisilazane, bis(dimethylamino)dimethylsilane, bis(diethylamino)dimethylsilane, (Dimethylamino) methylsilane, bis(diethylamino) methylsilane, 2-[(triethoxysilyl) propyl] dibenzylresorcinol, 2-[(trimethoxysilyl) propyl] dibenzylresorcinol, 2,2,6,6-tetramethyl-4-[3-(triethoxysilyl) propoxy] piperidine, 2,2,6,6-tetramethyl-4-[3-(trimethoxysilyl) propoxy] piperidine, 2-hydroxy-4-[3-(triethoxysilyl) propoxy] benzophenone, 2-hydroxy-4-[3-(trimethoxysilyl) propoxy] benzophenone, etc.

[0328] Specific examples of the compound represented by formula (b-2) include, but are not limited to, tetramethoxysilane, tetraethoxysilane, tetra(n-propoxy)silane, tetra(isopropoxy)silane, tetra(n-butoxy)silane, tetra(isobutoxy)silane, tetra-sec-butoxysilane, tetra-tert-butoxysilane, tetraacetoxysilane, tetra(trichloroacetoxy)silane, tetra(trifluoroacetoxy)silane, tetrachlorosilane, tetrabromosilane, tetrafluorosilane, tetra(methyl ethyl ketoxime)silane, and partially hydrolyzed condensates of tetramethoxysilane or tetraethoxysilane (e.g., trade names "M-Silicate 51", "Silicate 35", "Silicate 45", "Silicate 40", and "FR-3" manufactured by Tama Chemical Industries, Ltd.; trade names "MS51", "MS56", "MS57", and "MS56S" manufactured by Mitsubishi Chemical Corporation; trade names "Methyl Silicate 51", "Methyl Silicate 35", "Si ... 53A", "Ethyl Silicate 40", "Ethyl Silicate 48", "EMS-485", "N-103X", "PX", "PS-169", "PS-162R", "PC-291", "PC-301", "PC-302R", "PC-309", "EMSi48"), etc.

[0329] As described above, in this embodiment, the hydrolyzable silicon compound (b) preferably includes one or more selected from the group consisting of compounds containing the atomic group represented by the above formula (b-1), their hydrolysis products and condensation products, and compounds represented by the above formula (b-2), their hydrolysis products and condensation products.

[0330] In the present embodiment, the "hydrolyzable silicon compound (a) contained in the polymer nanoparticles (A)" and the "hydrolyzable silicon compound (b) contained in the matrix component (B)" may be of the same kind or of different kinds. Even when the two are of the same kind, they can be distinguished by making the hydrolyzable silicon compound (a) contained in the polymer nanoparticles (A) and the hydrolyzable silicon compound (b) contained in the matrix component (B).

[0331] [Inorganic oxide (D)]

[0332] The matrix component (B) in the present embodiment includes an inorganic oxide (D). By including the inorganic oxide (D), the hardness of the matrix component (B) can be increased and the wear resistance can be improved. In addition, the hydrophilicity of the hydroxyl groups on the particle surface of the inorganic oxide (D) also has a tendency to improve the anti-fouling property of the coating film.

[0333] As specific examples of the inorganic oxide (D) in the present embodiment, oxides of silicon, aluminum, titanium, zirconium, zinc, cerium, tin, indium, gallium, germanium, antimony, molybdenum, niobium, magnesium, bismuth, cobalt, copper, etc. can be cited but are not limited to. Regardless of their shape, they can be used alone or as a mixture. As an inorganic oxide (D), from the aspect of interaction with the above-mentioned hydrolyzable silicon compound (b), it is preferred to further include silicon oxide particles represented by dry silicon oxide and colloidal silicon oxide, and from the aspect of dispersibility, as the form of silicon oxide particles, it is preferred to further include colloidal silicon oxide. When the inorganic oxide (D) contains colloidal silicon oxide, it is preferably in the form of an aqueous dispersion, and any of acidic and alkaline can be used.

[0334] In addition, in the present embodiment, the inorganic oxide (D) preferably contains at least one inorganic component selected from the group consisting of Ce, Nb, Al, Zn, Ti, Zr, Sb, Mg, Sn, Bi, Co and Cu (hereinafter also referred to as "inorganic component"). The inorganic oxide (D) has a tendency to improve weather resistance without sacrificing wear resistance and durability by containing the inorganic component. In the case of using commercial products, for example, ultrafine particle material products of cerium oxide, zinc oxide, aluminum oxide, bismuth oxide, cobalt oxide, copper oxide, tin oxide, and titanium oxide manufactured by CIK Nano Tek Co., Ltd. can be cited but are not limited to; titanium oxide "Tainoc" (trade name), cerium oxide "Needral" (trade name), tin oxide "Ceramace" (trade name), niobium oxide sol, and zirconium oxide sol manufactured by Duomu Chemical Co., Ltd. From the aspect of improving weather resistance performance, the inorganic oxide (D) preferably contains at least one inorganic component selected from the group consisting of Ce, Nb, Zn, Ti and Zr, and more preferably contains Ce.

[0335] In the inorganic oxide (D) in the present embodiment, from the perspective of the balance of wear resistance, durability and weather resistance, it is preferred to contain at least one inorganic oxide (D') selected from the group consisting of Ce, Nb, Zn, Ti and Zr. The content of the inorganic oxide (D') in the hard coating film is not particularly limited. From the perspective of the balance of wear resistance, durability and weather resistance, it is preferably 1% by mass or more, and more preferably 2% by mass or more. In addition, from the perspective of transparency, the above content is preferably 50% by mass or less, and more preferably 30% by mass or less. Here, the above content can be determined as the total amount of Ce, Nb, Zn, Ti and Zr when the hard coating film is 100% by mass.

[0336] [Average particle size of inorganic oxide (D)]

[0337] Regarding the average particle size of the inorganic oxide (D) in the present embodiment, it is preferably 2 nm or more from the aspect of good storage stability of the composition of the hard coating. From the aspect of good transparency as a whole laminate, it is preferably 150 nm or less, more preferably 100 nm or less, and further preferably 50 nm or less. Therefore, the average particle size is preferably 2 nm or more and 100 nm or less, more preferably 2 nm or more and 50 nm or less. The method for determining the average particle size (D) of the inorganic oxide can be, for example, but not limited to, the following method: observe the water-dispersed colloidal silica using a transmission microscope photograph magnified 50,000 to 100,000 times, and photograph 100 to 200 inorganic oxides as particles, and measure the average value of the major and minor diameters of the inorganic oxide particles.

[0338] [Colloidal Silica Which May Be Contained in the Inorganic Oxide (D)]

[0339] The acidic colloidal silica using water as a dispersion solvent suitable for use in the present embodiment is not particularly limited, and can be prepared by a sol-gel method or a commercially available product. When prepared by a sol-gel method, reference can be made to Werner Stober et al; J. Colloid and Interface Sci., 26, 62-69 (1968), Rickey D. Badley et al; Lang muir 6, 792-801 (1990), Journal of the Color Society, 61 [9] 488-493 (1988), etc. When commercially available products are used, for example, Snowtex-O, Snowtex-OS, Snowtex-OXS, Snowtex-O-40, Snowtex-OL, Snowtex OYL, Snowtex-OUP, Snowtex-PS-SO, Snowtex-PS-MO, Snowtex-AK-XS, Snowtex-AK, Snowtex-AK-L, Snowtex-AK-YL, Snowtex-AK-PS-S (trade names, manufactured by Nissan Chemical Industries, Ltd.), Adelite AT-20Q (trade name, manufactured by Asahi Denka Industries, Ltd.), Klebosol 20H12, Klebosol 30CAL25 (trade names, manufactured by Clariant (Japan) Ltd.), etc. may be mentioned.

[0340] In addition, as the basic colloidal silica, there are silicas stabilized by the addition of alkali metal ions, ammonium ions, or amines, and examples thereof include, but are not limited to, Snowtex-20, Snowtex-30, Snowtex-XS, Snowtex-50, Snowtex-30L, Snowtex-XL, Snowtex-YL, Snowtex ZL, Snowtex-UP, Snowtex-ST-PS-S, Snowtex ST-PS-M, Snowtex-C, Snowtex-CXS, Snowtex-CM, Snowtex-N, Snowtex-NXS, Snowtex-NS, and Snowtex-N-40 (trade names, manufactured by Nissan Chemical Industries, Ltd.), Adelite AT-20, Adelite AT-30, Adelite AT-20N, Adelite AT-30N, Adelite AT-20A, Adelite AT-30A, Adelite AT-40, and Adelite AT-50 (trade name, manufactured by Asahi Electric Industries, Ltd.), Klebosol 30R9, Klebosol 30R50, Klebosol 50R50 (trade name, manufactured by Clariant Japan Ltd.), Ludox HS-40, Ludox HS-30, Ludox LS, Ludox AS-30, Ludox SM-AS, Ludox AM, Ludox HSA and Ludox SM (trade name, manufactured by DuPont), etc.

[0341] In addition, there is no particular limitation on the colloidal silica using a water-soluble solvent as a dispersion medium, and examples thereof include MA-ST-M (methanol dispersion type with a particle size of 20 to 25 nm), IPA-ST (isopropanol dispersion type with a particle size of 10 to 15 nm), EG-ST (ethylene glycol dispersion type with a particle size of 10 to 15 nm), EGST-ZL (ethylene glycol dispersion type with a particle size of 70 to 100 nm), NPC-ST (ethylene glycol monopropyl ether dispersion type with a particle size of 10 to 15 nm), and TOL-ST (toluene dispersion type with a particle size of 10 to 15 nm) manufactured by Nissan Chemical Industries, Ltd.

[0342] The dry silica particles are not particularly limited, and examples thereof include AEROSIL manufactured by NIPPON AEROSIL CO., LTD. and REOLOSIL manufactured by TOKUYAMA CO., LTD.

[0343] Furthermore, these silicon oxide particles may contain an inorganic base (sodium hydroxide, potassium hydroxide, lithium hydroxide, ammonia, etc.) or an organic base (tetramethylammonium, triethylamine, etc.) as a stabilizer.

[0344] [Shape of Inorganic Oxide (D)]

[0345] In addition, the shape of the inorganic oxide (D) in this embodiment can be, but is not limited to, spherical, square, polyhedral, elliptical, flat, linear, beaded, chain, etc., and from the perspective of the hardness and transparency of the hard coating, spherical is particularly preferred.

[0346] [Functional group (e)]

[0347] In the polymer nanoparticles (A) in the present embodiment, it is preferred to have a functional group (e) that interacts with the matrix component (B) from the aspect of being able to improve the dispersibility of the polymer nanoparticles (A) in the matrix component (B) and improving the wear resistance. The situation that the polymer nanoparticles (A) have the functional group (e) can be confirmed by, for example, composition analysis based on IR, GC-MS, thermal decomposition GC-MS, LC-MS, GPC, MALDI-MS, TOF-SIMS, TG-DTA, NMR and analysis based on their combination.

[0348] Specific examples of the functional group (e) in the present embodiment include, but are not limited to, hydroxyl, carboxyl, amino, amide, and functional groups containing ether bonds. From the perspective of interaction, functional groups having hydrogen bonds are preferred, and from the perspective of high hydrogen bonding properties, amide groups are more preferred, and secondary amide groups and / or tertiary amide groups are further preferred.

[0349] Examples of the compound containing the functional group (e) and its reactant include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 2-hydroxyethyl vinyl ether or 4-hydroxybutyl vinyl ether, 2-hydroxyethyl allyl ether, (meth)acrylic acid, 2-carboxyethyl (meth)acrylate, 2-dimethylaminoethyl (meth)acrylate, 2-diethylaminoethyl (meth)acrylate, 2-di-n-propylaminoethyl (meth)acrylate, 3-dimethylaminopropyl (meth)acrylate, 4-dimethylaminobutyl (meth)acrylate, N-[2-(meth)acryloyloxy]ethylmorpholine, vinylpyridine, N-vinylcarbazole, N-vinylquinoline, N-methylacrylamide, N-methylmethacrylamide, N-ethylacrylamide, N,N-dimethylacrylamide, N,N-dimethylmethacrylamide 、N,N-diethylacrylamide, N-ethylmethacrylamide, N-methyl-N-ethylacrylamide, N-methyl-N-ethylmethacrylamide, N-isopropylacrylamide, N-n-propylacrylamide, N-isopropylmethacrylamide, N-n-propylmethacrylamide, N-methyl-N-n-propylacrylamide, N-methyl-N-isopropylacrylamide, N-acryloylpyrrolidine, N-methacryloylpyrrolidine, N-acryloylpiperidine, N-methacryloylpiperidine, N-acryloylhexahydroazepine, N-acryloylmorpholine, N-methacryloylmorpholine, N-vinylpyrrolidone, N-vinylcaprolactam, N,N'-methylenebisacrylamide, N,N'-methylenebismethacrylamide, N-vinylacetamide, acetylacetoneacrylamide, acetylacetonemethacrylamide, N-methylolacrylamide, N-methylolmethacrylamide, Blemmer PE-90, PE-200, PE-350, PME-100, PME-200, PME-400, AE-350 (trade names, manufactured by Nippon Oil & Fats Co., Ltd.), MA-30, MA-50, MA-100, MA-150, RA-1120, RA-2614, RMA-564, RMA-568, RMA-1114, MPG130-MA (trade names, manufactured by Nippon Emulsifier Co., Ltd.), etc. It should be noted that in this specification, (meth)acrylate is a simple description of acrylate or methacrylate, and (meth)acrylic acid is a simple description of acrylic acid or methacrylic acid.

[0350] [Core / Shell Structure of Polymer Nanoparticles (A)]

[0351] The polymer nanoparticles (A) in this embodiment preferably have a core / shell structure having a core layer and one or more shell layers covering the core layer. From the perspective of interaction with the outermost matrix component (B) of the core / shell structure, the polymer nanoparticles (A) preferably have a functional group (e).

[0352] [Other compounds that may be contained in the polymer nanoparticles (A)]

[0353] From the aspect of improving the stability of particles by making the particles have electrostatic repulsion, the polymer nanoparticles (A) of the present embodiment can include the polymer shown below. For example, polyurethane, polyester, poly(meth)acrylate, poly(meth)acrylic acid, polyvinyl acetate, polybutadiene, polyvinyl chloride, chlorinated polypropylene, polyethylene, polystyrene polymers, or copolymers of poly(meth)acrylate-organic silicon, polystyrene-(meth)acrylate, styrene maleic anhydride can be cited.

[0354] Among the polymers that can be included in the polymer nanoparticles (A), as compounds that are particularly excellent in electrostatic repulsion, polymers or copolymers of (meth) acrylic acid and (meth) acrylic acid esters can be cited. As specific examples, polymers or copolymers of methyl acrylate, (meth) acrylic acid, methyl methacrylate, butyl methacrylate, cyclohexyl methacrylate, 2-ethylhexyl acrylate, n-butyl acrylate, 2-hydroxyethyl (meth) acrylic acid, 2-hydroxypropyl (meth) acrylic acid, 3-hydroxybutyl (meth) acrylic acid, 4-hydroxybutyl (meth) acrylic acid, 3-hydroxybutyl (meth) acrylic acid, and 4-hydroxybutyl (meth) acrylic acid can be cited but are not limited to. At this time, in order to further improve the electrostatic repulsion, part or all of the (meth) acrylic acid can be neutralized using amines such as ammonia or triethylamine, dimethylethanolamine, or salts such as NaOH and KOH.

[0355] In addition, the polymer nanoparticles (A) may contain an emulsifier. The emulsifier is not particularly limited, and examples thereof include acidic emulsifiers such as alkylbenzenesulfonic acid, alkylsulfonic acid, alkylsulfonated succinic acid, polyoxyethylene alkylsulfuric acid, polyoxyethylene alkylarylsulfuric acid, polyoxyethylene distyrylphenyl ether sulfonic acid, etc.; anionic surfactants such as alkali metal (Li, Na, K, etc.) salts of acidic emulsifiers, ammonium salts of acidic emulsifiers, and fatty acid soaps; cationic surfactants in the form of quaternary ammonium salts, pyridinium salts, and imidazolinium salts such as alkyltrimethylammonium bromide, alkylpyridinium bromide, and lauric acid imidazolinium; nonionic surfactants such as polyoxyethylene alkylaryl ether, polyoxyethylene sorbitan fatty acid ester, polyoxyethylene oxypropylene block copolymer, and polyoxyethylene distyrylphenyl ether; reactive emulsifiers having free radical polymerizable double bonds, etc.

[0356] Examples of the reactive emulsifier having a radical polymerizable double bond include, but are not limited to, Eleminol JS-2 (trade name, manufactured by Sanyo Chemical Industry Co., Ltd.), Latemul S-120, S-180A or S-180 (trade name, manufactured by Kao Corporation), Aquaron HS-10, KH-1025, RN-10, RN-20, RN30, RN50 (trade name, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), Adeka Reasoap SE1025, SR-1025, NE-20, NE-30, NE-40 (trade names, manufactured by Asahi Denka Kogyo Co., Ltd.), ammonium salts of p-styrenesulfonic acid, sodium salts of p-styrenesulfonic acid, potassium salts of p-styrenesulfonic acid, alkylsulfonic acid (meth)acrylates such as 2-sulfoethyl acrylate, methylpropanesulfonic acid (meth)acrylamide, ammonium salts of allylsulfonic acid, sodium salts of allylsulfonic acid, potassium salts of allylsulfonic acid, etc.

[0357] [Other ingredients that may be contained in layer (C)]

[0358] In the layer (C) of the present embodiment, depending on the application, as the matrix component (B), a solvent, an emulsifier, a plasticizer, a pigment, a dye, a filler, an anti-aging agent, a conductive material, a UV absorber, a light stabilizer, a peeling regulator, a softener, a surfactant, a flame retardant, an antioxidant, and a catalyst may be included. In particular, in outdoor applications, high weather resistance is required, so it is preferred to include a sunscreen (S2) and a light stabilizer. As the sunscreen (S2), it is preferred to include a UV absorber.

[0359] Specific examples of the ultraviolet absorber and the light stabilizer include, but are not limited to, 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-methoxybenzophenone-5-sulfonic acid, 2-hydroxy-4-n-octyloxybenzophenone, 2-hydroxy-4-n-dodecyloxybenzophenone, 2-hydroxy-4-benzyloxybenzophenone, bis(5-benzoyl-4-hydroxy-2-methoxyphenyl)methane, 2,2'-dihydroxy-4,4'-dihydroxy-4-methoxybenzophenone, 2 ... Benzophenone-based ultraviolet absorbers such as dimethoxybenzophenone (trade name "UVINUL3049" manufactured by BASF), 2,2',4,4'-tetrahydroxybenzophenone (trade name "UVINUL3050" manufactured by BASF), 4-dodecyloxy-2-hydroxybenzophenone, 5-benzoyl-2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxy-2'-carboxybenzophenone, 2-hydroxy-4-stearyloxybenzophenone, and 4,6-dibenzoylresorcinol;2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-(2'-hydroxy-5'-tert-butylphenyl)benzotriazole, 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)benzotriazole, 2-(2-hydroxy-5-tert-octylphenyl)benzotriazole, 2-(2-hydroxy-3,5-di-tert-octylphenyl)benzotriazole, 2-[2'-hydroxy-3',5'-bis(α,α'-dimethylbenzyl)phenyl]benzotriazole), methyl-3-[3-tert-butyl-5-(2H-phenyl)benzotriazole] 3-[(2H-benzotriazol-2-yl)-4-hydroxyphenyl]propionate and polyethylene glycol (molecular weight 300) condensate (trade name "TINUVIN1130" manufactured by BASF), isooctyl-3-[3-(2H-benzotriazol-2-yl)-5-tert-butyl-4-hydroxyphenyl]propionate (trade name "TINUVIN384" manufactured by BASF), 2-(3-dodecyl-5-methyl-2-hydroxyphenyl)benzotriazole (trade name "TINUVIN IN571”), 2-(2'-hydroxy-3'-tert-butyl-5'-methylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3',5'-di-tert-amylphenyl)benzotriazole, 2-(2'-hydroxy-4'-octyloxyphenyl)benzotriazole, 2-[2'-hydroxy-3'-(3",4",5",6"-tetrahydrophthalimidomethyl)-5'-methylphenyl]benzotriazole, 2,2-methylenebis[4-(1,1,3,3-tetramethylbutyl)-6-(2H -benzotriazole-2-yl)phenol], 2-(2H-benzotriazole-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol (trade name "TINUVIN900" manufactured by BASF), TINUVIN384-2, TINUVIN326, TINUVIN327, TINUVIN109, TINUVIN970, TINUVIN328, TINUVIN171, TINUVIN970, TINUVIN PS, TINUVIN P, TINUVIN99-2, TINUVIN928 (trade name, manufactured by BASF) and other benzotriazole-based ultraviolet absorbers;2-[4-[(2-hydroxy-3-dodecyloxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2-[4-[(2-hydroxy-3-tridecyloxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2,4-bis(2-hydroxy-4-butylhydroxyphenyl)-6-(2,4-bisbutylhydroxyphenyl)-1,3,5-triazine (manufactured by BASF Corporation) triazine-based ultraviolet absorbers such as TINUVIN 460 (trade name, manufactured by BASF), 2-(2-hydroxy-4-[1-octyloxycarbonylethoxy]phenyl)-4,6-bis(4-phenylphenyl)-1,3,5-triazine (trade name, manufactured by BASF), TINUVIN 400, TINUVIN 405, TINUVIN 477, and TINUVIN 1600 (trade name, manufactured by BASF); malonate-based ultraviolet absorbers such as HOSTAVIN PR25, HOSTAVIN B-CAP, and HOSTAVIN VSU (trade name, manufactured by Clariant); and HOSTAVIN 3206 LIQ, HOSTAVIN VSU P, and HOSTAVIN 3212 Anilide-based ultraviolet absorbers such as LIQ (trade name, manufactured by Clariant); salicylate-based ultraviolet absorbers such as amyl salicylate, menthyl salicylate, homomenthyl salicylate, octyl salicylate, phenyl salicylate, benzyl salicylate, and p-isopropylphenyl salicylate; cyanoacrylate-based ultraviolet absorbers such as ethyl 2-cyano-3,3-diphenylacrylate (trade name "UVINUL3035" manufactured by BASF), (2-ethylhexyl)-2-cyano-3,3-diphenylacrylate (trade name "UVINUL3039" manufactured by BASF), and 1,3-bis((2'-cyano-3',3'-diphenylacryloyl)oxy)-2,2-bis-(((2'-cyano-3',3'-diphenylacryloyl)oxy)methyl)propane (trade name "UVINUL3030" manufactured by BASF);2-Hydroxy-4-acryloxybenzophenone, 2-hydroxy-4-methacryloxybenzophenone, 2-hydroxy-5-acryloxybenzophenone, 2-hydroxy-5-methacryloxybenzophenone, 2-hydroxy-4-(acryloxy-ethoxy)benzophenone, 2-hydroxy-4-(methacryloxy-ethoxy)benzophenone, 2-hydroxy-4-(methacryloxy-diethoxy)benzophenone, 2-hydroxy-4-(acryloxy-triethoxy)benzophenone, 2-(2'-hydroxy-5'-methacryloxyethylphenyl)-2H-benzotriazole (products manufactured by Otsuka Chemical Co., Ltd.) Radically polymerizable ultraviolet absorbers having a radically polymerizable double bond in the molecule, such as 2-(2'-hydroxy-5'-methacryloxyethyl-3-tert-butylphenyl)-2H-benzotriazole, 2-(2'-hydroxy-5'-methacryloxypropyl-3-tert-butylphenyl)-5-chloro-2H-benzotriazole, and 3-methacryloyl-2-hydroxypropyl-3-[3'-(2"-benzotriazolyl)-4-hydroxy-5-tert-butyl]phenyl propionate (trade name "CGL-104" manufactured by Ciba-Geigy Co., Ltd. of Japan); UV-G101, UV-G 301, UV-G137, UV-G12, UV-G13 (trade names of Nippon Shokubai Co., Ltd.), and other ultraviolet-absorbing polymers; bis(2,2,6,6-tetramethyl-4-piperidinyl) succinate, bis(2,2,6,6-tetramethylpiperidinyl) sebacate, bis(1,2,2,6,6-pentamethyl-4-piperidinyl) 2-(3,5-di-tert-butyl-4-hydroxybenzyl)-2-butylmalonate, 1-[2-[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propynyloxy]ethyl]-4-[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propynyloxy]-2,2 , 6,6-tetramethylpiperidine, a mixture of bis(1,2,2,6,6-pentamethyl-4-piperidinyl) sebacate and methyl-1,2,2,6,6-pentamethyl-4-piperidinyl-sebacate (trade name "TINUVIN292" manufactured by BASF), bis(1-octyloxy-2,2,6,6-tetramethyl-4-piperidinyl) sebacate, TINUVIN123, TINUVIN144, TINUVIN152, TINUVIN249, TINUVIN292, TINUVIN5100 (trade name, manufactured by BASF) and other hindered amine light stabilizers;Free radical polymerizable hindered amine light stabilizers such as 1,2,2,6,6-pentamethyl-4-piperidinyl methacrylate, 1,2,2,6,6-pentamethyl-4-piperidinyl methacrylate, 2,2,6,6-tetramethyl-4-piperidinyl methacrylate, 2,2,6,6-tetramethyl-4-piperidinyl acrylate, 1,2,2,6,6-pentamethyl-4-iminopiperidinyl methacrylate, 2,2,6,6-tetramethyl-4-iminopiperidinyl methacrylate, 4-cyano-2,2,6,6-tetramethyl-4-piperidinyl methacrylate, 4-cyano-1,2,2,6,6-pentamethyl-4-piperidinyl methacrylate; Udouble E-133, Udouble E-135, Udouble S-2000, Udouble S-2834, Udouble S-2840, Udouble S-2818, Udouble S-2860 (trade name, manufactured by Nippon Shokubai Co., Ltd.) and other light-stable polymers; UV absorbers reactive with silanol groups, isocyanate groups, epoxy groups, semicarbazide groups, and hydrazide groups; inorganic UV absorbers such as cerium oxide, zinc oxide, aluminum oxide, zirconium oxide, niobium oxide, bismuth oxide, cobalt oxide, copper oxide, tin oxide, and titanium oxide; etc., any one of them or two or more of them can be used in combination. ;

[0360] [Transparency of hard coat]

[0361] In this embodiment, the transparency of the hard coat layer can be evaluated by the total light transmittance maintenance rate obtained by the following formula from the aspect of appearance change. In this embodiment, the total light transmittance maintenance rate of the hard coat layer is preferably 90% or more, more preferably 95% or more from the aspect of ensuring lighting, and particularly preferably 98% or more from the aspect of ensuring visibility across the material. For example, by adopting the above-mentioned preferred embodiment as the polymer nanoparticles (A) and the matrix component (B), the total light transmittance maintenance rate of the hard coat layer can be adjusted to the above-mentioned range.

[0362] Total light transmittance maintenance rate of hard coat layer (%) = (total light transmittance of laminate (%) / total light transmittance of substrate (%)) × 100

[0363] <Coating composition (I)>

[0364] In the present embodiment, the layer (C) is preferably obtained by using the following coating composition (I), for example. Preferably, the coating composition (I) is a coating composition comprising polymer nanoparticles (A) and a matrix raw material component (B'), and the elastic recovery rate η of the polymer nanoparticles (A) measured by an indentation test according to ISO14577-1 is ITAThe Martens hardness HM of the polymer nanoparticles (A) is 0.30 or more and 0.90 or less. A The Martens hardness HM of the matrix raw material component (B') B’ Meet HM B’ / HM A >1, the matrix raw material component (B') contains an inorganic oxide (D).

[0365] The inorganic oxide (D) in the coating composition (I) preferably contains at least one inorganic component selected from the group consisting of Ce, Nb, Al, Zn, Ti, Zr, Sb, Mg, Sn, Bi, Co and Cu.

[0366] The details of the components contained in the coating composition (I) not mentioned below are the same as those described above for the components contained in the layer (C).

[0367] [Hardness of polymer nanoparticles (A) HM A Hardness HM of the matrix raw material component (B') B ]

[0368] In the coating composition (I), the Martens hardness HM of the polymer nanoparticles (A) is A Martens hardness HM of the matrix raw material component (B') B’ It is preferable to satisfy the relationship of the following formula (3).

[0369] HM B’ / HM A >1 Formula (3)

[0370] As described above, in the coating composition (I), since the above relationship is satisfied, in the layer (C) obtained by using the coating composition (I), the Martens hardness HM of the polymer nanoparticles (A) is A Martens hardness HM of the matrix raw material component (B') B’ The Martens hardness of each component in the coating composition (I) can be separated into polymer nanoparticles (A) and matrix raw material component (B') by centrifugation, ultrafiltration or the like, and the separated components can be measured based on the method described in the examples described below.

[0371] The above HM A and H.M. B The values ​​of can be adjusted to the above-mentioned magnitude relationship by adjusting the structures and composition ratios of the constituent components of the polymer nanoparticles (A) and the matrix raw material component (B'), and the method is not particularly limited.

[0372] [Elastic recovery rate η of polymer nanoparticles (A) ITA]

[0373] The elastic recovery rate η of the polymer nanoparticles (A) in this embodiment is ITA The coating film of the polymer nanoparticles (A) after film formation is used as W in ISO14577-1. elast / W total The ratio η IT The parameters recorded are measured and obtained by measuring the total mechanical work W of the depression. total The amount of work done by the elastic recovery deformation of the concave elast Elastic recovery rate η ITA The higher the elastic recovery rate, the more the coating film can recover to its original state when it is impacted, and the higher the self-repair ability against impact. From the perspective of effectively exerting the self-repair ability, the elastic recovery rate η of the polymer nanoparticles (A) ITA Under the measurement conditions (Vickers quadrangular pyramid diamond indenter, load increase condition 2mN / 20sec, load decrease condition 2mN / 20sec), η is preferably 0.30 or more, from the perspective of being able to follow the deformation of the substrate or matrix raw material component (B') when the coating is formed, ITA It is preferably 0.90 or less. The elastic recovery rate η of the polymer nanoparticles (A) ITA More preferably, it is 0.50 or more, and even more preferably, it is 0.60 or more. The elastic recovery rate of the polymer nanoparticles (A) can be determined by, but not limited to, the following methods: separating the polymer nanoparticles (A) and the matrix raw material component (B') by centrifugal separation, ultrafiltration, etc., dispersing the separated polymer nanoparticles (A) in a solvent to obtain a composition, applying the composition and drying it, and measuring the film after film formation using a micro hardness meter Fischerscope (HM2000S manufactured by Fischer Instruments), an ultra-micro indentation hardness tester (ENT-NEXUS manufactured by Elionix Co., Ltd.), a nanoindenter (iNano, G200 manufactured by Toyo Technica), a nanoindentation system (TI980 manufactured by Bruker), etc. As a method for measuring the elastic recovery rate η ITA The method of adjusting the content within the above range includes, but is not limited to, adjusting the structure and composition ratio of the components of the polymer nanoparticles (A).

[0374] It should be noted that the layer (C) can be obtained in the form of a cured product obtained by curing the coating composition (I) by hydrolysis condensation or the like. The composition of the polymer nanoparticles (A) is usually unchanged during the curing process. Therefore, the elastic recovery rate η of the polymer nanoparticles (A) in the coating composition (I) measured by the method described in the examples described later is ITAThe value of is related to the elastic recovery rate η of the polymer nanoparticles (A) in the layer (C) ITA The elastic recovery factor η in layer (C) can be determined in this form. ITA The value of .

[0375] [Solvent (H)]

[0376] The coating composition (I) in this embodiment preferably contains a solvent (H). The solvent (H) that can be used is not particularly limited, and a common solvent can be used. Examples of the solvent include, but are not limited to, water; ethylene glycol, butyl cellosolve, isopropyl alcohol, n-butanol, 2-butanol, ethanol, methanol, modified ethanol, 2-methoxy-1-propanol, 1-methoxy-2-propanol, diacetone alcohol, glycerol, monoalkyl monoglycerol ether, propylene glycol monomethyl ether, diethylene glycol monobutyl ether, propylene glycol monoethyl ether, propylene glycol monobutyl ether, dipropylene glycol monoethyl ether, dipropylene glycol monobutyl ether, diethylene glycol monophenyl ether, tetraethylene glycol monophenyl ether, etc. Alcohols; aromatic hydrocarbons such as toluene and xylene; aliphatic hydrocarbons such as hexane, cyclohexane, and heptane; esters such as ethyl acetate and n-butyl acetate; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; ethers such as tetrahydrofuran and dioxane; amides such as dimethylacetamide and dimethylformamide; halides such as chloroform, dichloromethane, and carbon tetrachloride; dimethyl sulfoxide and nitrobenzene; etc., and one of them or two or more thereof can be used in combination. Among them, from the perspective of reducing the environmental load when removing the solvent, solvents containing water and alcohols are particularly preferred.

[0377] The constituent components, size, composition ratio, etc. of the polymer nanoparticles (A) contained in the coating composition (I) are described below. The details of aspects not mentioned below are the same as the above description of the polymer nanoparticles (A) contained in the layer (C).

[0378] In addition, the matrix raw material component (B') contained in the coating composition (I) is cured by hydrolysis condensation or the like in the process of obtaining the layer (C). That is, the matrix raw material component (B') contained in the coating composition (I) has a relationship of forming a corresponding matrix component (B) in the obtained layer (C). The constituent components, size, composition ratio, etc. of the matrix raw material component (B') are also described below, and the details of the aspects not mentioned below are the same as the above description of the matrix component (B) contained in the layer (C).

[0379] In the coating composition (I), the polymer nanoparticles (A) preferably contain the above-mentioned hydrolyzable silicon compound (a), and the matrix raw material component (B') contains the above-mentioned hydrolyzable silicon compound (b). In addition, as the hydrolyzable silicon compound (a) in the coating composition (I), it is also preferred to contain one or more selected from the compounds containing the atomic group represented by the above-mentioned formula (a-1), their hydrolyzates and condensates, and the compounds represented by the above-mentioned formula (a-2), their hydrolyzates and condensates. Similarly, as the hydrolyzable silicon compound (b) in the coating composition (I), it is also preferred to contain one or more selected from the compounds containing the atomic group represented by the above-mentioned formula (b-1), their hydrolyzates and condensates, and the compounds represented by the above-mentioned formula (b-2), their hydrolyzates and condensates.

[0380] The details of the hydrolyzable silicon compounds (a) and (b) in the coating composition (I) are the same as those described above with respect to the polymer nanoparticles (A) and the matrix component (B) contained in the layer (C).

[0381] [Content of the hydrolyzable silicon compound (a) in the polymer nanoparticles (A)]

[0382] In the coating composition (I), the content of the hydrolyzable silicon compound (a) represents the solid content weight ratio of the hydrolyzable silicon compound (a) contained in the polymer nanoparticles (A). The higher the content, the better the wear resistance, weather resistance and heat resistance. From this point of view, the higher the content, the more preferred. The above content is preferably 50% by mass or more, more preferably 60% by mass or more. The content of the hydrolyzable silicon compound (a) in the polymer nanoparticles (A) can be measured by, but not limited to, IR analysis, NMR analysis, elemental analysis, etc. of the polymer nanoparticles (A).

[0383] [Functional group (e)]

[0384] In the coating composition (I), the polymer nanoparticle (A) preferably has a functional group (e) that interacts with the matrix raw material component (B'). When the polymer nanoparticle (A) has the functional group (e), the matrix raw material component (B') is easily adsorbed on the surface of the polymer nanoparticle (A), forming a protective colloid and tending to stabilize, so the storage stability of the coating composition (I) tends to improve as a result. In addition, when the polymer nanoparticle (A) has the functional group (e), the interaction between the polymer nanoparticle (A) and the matrix raw material component (B') is enhanced, thereby the tackifying property relative to the solid content concentration of the coating composition (I) can be improved, and there is a tendency to suppress the occurrence of sagging when applied into a complex shape, and the film thickness of the layer (C) has a tendency to become uniform. The situation that the polymer nanoparticle (A) has the functional group (e) can be confirmed by, for example, composition analysis based on IR, GC-MS, thermal decomposition GC-MS, LC-MS, GPC, MALDI-MS, TOF-SIMS, TG-DTA, NMR, and analysis based on their combination, etc.

[0385] Specific examples of the functional group (e) in the present embodiment include, but are not limited to, hydroxyl, carboxyl, amino, amide, and functional groups containing ether bonds. From the perspective of interaction, functional groups having hydrogen bonds are preferred, and from the perspective of high hydrogen bonding properties, amide groups are more preferred, and secondary amide groups and / or tertiary amide groups are further preferred.

[0386] Examples of the compound containing the functional group (e) and its reactant include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 2-hydroxyethyl vinyl ether or 4-hydroxybutyl vinyl ether, 2-hydroxyethyl allyl ether, (meth)acrylic acid, 2-carboxyethyl (meth)acrylate, 2-dimethylaminoethyl (meth)acrylate, 2-diethylaminoethyl (meth)acrylate, 2-di-n-propylaminoethyl (meth)acrylate, 3-dimethylaminopropyl (meth)acrylate, 4-dimethylaminobutyl (meth)acrylate, N-[2-(meth)acryloyloxy]ethylmorpholine, vinylpyridine, N-vinylcarbazole, N-vinylquinoline, N-methylacrylamide, N-methylmethacrylamide, N-ethylacrylamide, N,N-dimethylacrylamide, N,N-dimethylmethacrylamide, Amine, N,N-diethylacrylamide, N-ethylmethacrylamide, N-methyl-N-ethylacrylamide, N-methyl-N-ethylmethacrylamide, N-isopropylacrylamide, N-n-propylacrylamide, N-isopropylmethacrylamide, N-n-propylmethacrylamide, N-methyl-N-n-propylacrylamide, N-methyl-N-isopropylacrylamide, N-acryloylpyrrolidine, N-methacryloylpyrrolidine, N-acryloylpiperidine, N-methacryloylpiperidine, N-acryloylhexahydroazepine, N-acryloylmorpholine, N-methacryloylmorpholine, N-vinylpyrrolidone, N-vinylcaprolactam, N,N'-methylenebisacrylamide, N,N'-methylenebismethacrylamide, N-vinylacetamide, acetylacetoneacrylamide, acetylacetonemethacrylamide, N-methylolacrylamide, N-methylolmethacrylamide, Blemmer PE-90, PE-200, PE-350, PME-100, PME-200, PME-400, AE-350 (trade names, manufactured by Nippon Oil & Fats Co., Ltd.), MA-30, MA-50, MA-100, MA-150, RA-1120, RA-2614, RMA-564, RMA-568, RMA-1114, MPG130-MA (trade names, manufactured by Nippon Emulsifier Co., Ltd.), etc. It should be noted that in this specification, (meth)acrylate is a simple description of acrylate or methacrylate, and (meth)acrylic acid is a simple description of acrylic acid or methacrylic acid.

[0387] [Elastic recovery rate η of the matrix raw material component (B') ITB’ and the elastic recovery rate η of the matrix component (B) ITB ]

[0388] Elastic recovery rate η of the matrix raw material component (B') in the coating composition (I) ITB’ It is the "Welast / W total The ratio η IT The parameter recorded in the form of " is obtained by measuring the coating film of the matrix raw material component (B') after film formation, and the total mechanical work W of the depression is used. total The amount of work done by the elastic recovery deformation of the concave elast Elastic recovery rate η ITB’ The higher the value, the more the coating can recover to its original state when it is impacted, and the higher the self-repair ability against impact. From the perspective of effectively exerting the self-repair ability, the elastic recovery rate η of the matrix raw material component (B') ITB’ Under the measurement conditions (Vickers tetrahedral diamond indenter, load increase condition 2mN / 20sec, load reduction condition 2mN / 20sec), it is preferably 0.60 or more, more preferably 0.65 or more. In addition, from the aspect of being able to follow the deformation of the substrate and component (A) when the coating is made, η ITB’ Preferably, it is less than 0.95. The elastic recovery rate of the matrix raw material component (B') can be measured by, but not limited to, the following methods: separating the polymer nanoparticles (A) and the matrix raw material component (B') by centrifugal separation or the like, dissolving the separated matrix raw material component (B') in a solvent to obtain a composition, applying the composition and drying it, and measuring the film after film formation using a micro hardness meter Fischerscope (HM2000S manufactured by Fischer Instruments), an ultra-micro indentation hardness tester (ENT-NEXUS manufactured by Elionix Co., Ltd.), a nano indenter (iNano, G200 manufactured by Toyo Technica), a nano indentation system (TI980 manufactured by Bruker), etc.

[0389] It should be noted that, as described above, the cured product obtained by curing the matrix raw material component (B') by hydrolysis condensation or the like is equivalent to the matrix component (B). Therefore, the elastic recovery rate η of the matrix raw material component (B') measured by the method described in the examples described later is ITB’ The value of and the corresponding elastic recovery rate η of the matrix component (B) ITB In good agreement, the elastic recovery rate η can be determined in this form ITB That is, the elastic recovery rate η of the matrix component (B) in this embodiment is ITB Preferably, it is 0.60 or more, and more preferably, it is 0.65 or more. In addition, from the aspect of being able to follow the deformation of the substrate and component (A) when the coating film is formed, η ITB It is preferably 0.95 or less.

[0390] As the elastic recovery rate η ITB’and elastic recovery rate η ITB The method of adjusting the content within the above range includes, but is not limited to, adjusting the structure and composition ratio of the constituent components of the matrix raw material component (B').

[0391] In the coating composition (I), the "hydrolyzable silicon compound (a) contained in the polymer nanoparticles (A)" and the "hydrolyzable silicon compound (b) contained in the matrix raw material component (B')" may be of the same kind or different kinds. Even when both are of the same kind, they can be distinguished by making the hydrolyzable silicon compound (a) contained in the polymer nanoparticles (A) and the hydrolyzable silicon compound (b) contained in the matrix raw material component (B').

[0392] [Inorganic oxide (D)]

[0393] In the coating composition (I), the matrix raw material component (B') contains an inorganic oxide (D). By including the inorganic oxide (D), not only the hardness of the matrix raw material component (B') can be increased, the wear resistance can be improved, but also the anti-fouling property of the coating film tends to be improved due to the hydrophilicity of the hydroxyl groups on the particle surface.

[0394] The inorganic oxide (D) in the coating composition (I) may be a single substance or a mixture regardless of its shape. From the perspective of interaction with the above-mentioned hydrolyzable silicon compound (b), it is preferred to further include silicon oxide particles, and from the perspective of dispersibility, it is preferred to further include colloidal silicon oxide as the form of silicon oxide particles. When the inorganic oxide (D) includes colloidal silicon oxide, it is preferably in the form of an aqueous dispersion, and either acidic or alkaline can be used.

[0395] The average particle size of the inorganic oxide (D) in the coating composition (I) is preferably 2 nm or more from the perspective of good storage stability of the coating composition (I). From the perspective of good transparency as a whole laminate, it is preferably 150 nm or less, more preferably 100 nm or less, and further preferably 50 nm or less. Therefore, the average particle size is preferably 2 nm or more and 100 nm or less, more preferably 2 nm or more and 50 nm or less. The method for determining the average particle size of the inorganic oxide (D) in the coating composition (I) is the same as the above method for the inorganic oxide (D) contained in the layer (C).

[0396] The remaining characteristics of the inorganic oxide (D) in the coating composition (I) are the same as the above-mentioned characteristics of the inorganic oxide (D) contained in the layer (C).

[0397] [Volume fraction of polymer nanoparticles (A) relative to the total of polymer nanoparticles (A) and matrix raw material component (B')]

[0398] In the coating composition (I), the volume fraction of the polymer nanoparticles (A) relative to the total of the polymer nanoparticles (A) and the matrix raw material component (B') is preferably 2% or more, more preferably 3% or more, and even more preferably 5% or more from the perspective of film-forming properties, and is preferably 80% or less, more preferably 70% or less, and even more preferably 45% or less from the perspective of transparency. The volume fraction of the polymer nanoparticles (A) in the coating composition (I) can be calculated, for example, based on the ratio of the polymer nanoparticles (A) in the entire coating film in the cross-sectional SEM image after forming the layer (C), and the component ratio of the polymer nanoparticles (A) in the components constituting the coating composition (I).

[0399] [Core / Shell Structure of Polymer Nanoparticles (A)]

[0400] In the coating composition (I), the polymer nanoparticle (A) preferably has a core / shell structure having a core layer and one or more shell layers covering the core layer. From the aspect of the interaction with the outermost matrix raw material component (B') of the core / shell structure, the polymer nanoparticle (A) also preferably has the above-mentioned functional group (e). The situation that the polymer nanoparticle (A) has a core / shell structure can be confirmed by, for example, a transmission electron microscope image of a coating cross section, etc.

[0401] [Other ingredients that may be contained in the coating composition (I)]

[0402] From the perspective of further improving the coating properties of the coating composition (I), in the coating composition (I), as the matrix raw material component (B'), in addition to the above-mentioned components, a thickener, a leveling agent, a thixotropic agent, a defoaming agent, a freeze stabilizer, a dispersant, a wetting agent, a rheology control agent, a film-forming aid, a rust inhibitor, a plasticizer, a lubricant, a preservative, a mildew inhibitor, an antistatic agent, an antistatic agent, etc. may be mixed as needed. From the perspective of improving the film-forming properties, it is preferred to use a wetting agent and a film-forming aid, and specifically, but not particularly limited to, diethylene glycol monobutyl ether, ethylene glycol monobutyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, ethylene glycol mono-2-ethylhexyl ether, 2,2,4-trimethyl-1,3-butanediol isobutyrate, diisopropyl glutarate, propylene glycol n-butyl ether, dipropylene glycol n-butyl ether, tripropylene glycol n-butyl ether, dipropylene glycol n-butyl ether, Glycol methyl ether, tripropylene glycol methyl ether, MEGAFACE F-443, F-444, F-445, F-470, F-471, F-472SF, F-474, F-475, F-477, F-479, F-480SF, F-482, F-483, F-489, F-172D, F-178K (trade names, manufactured by DIC Corporation), SN WET 366, SN WET 980, SN WET L, SN WET S, SN WET 125, SN WET 126, SN WET 970 (trade names, manufactured by SAN NOPCO Co., Ltd.), etc. These compounds can be used alone or in combination of two or more.

[0403] [Sunscreen (S2)]

[0404] The coating composition (I) may contain a sunscreen (S2). It is preferred that the coating composition (I) contains a sunscreen (S2). The sunscreen (S2) is not particularly limited, and for example, the substance described above as the sunscreen (S1) in the coating composition (J) can be suitably used.

[0405] [catalyst]

[0406] In the coating composition (I), as a matrix raw material component (B'), a catalyst may be included. When the coating composition (I) includes a catalyst that promotes the reaction of reactive groups, it is not easy to leave unreactive groups in the coating film, which can not only improve the hardness and wear resistance, but also improve the weather resistance, which is preferred from this aspect. The catalyst is not particularly limited, and when obtaining a hard coating film, it is preferably dissolved or dispersed. Such a catalyst is not particularly limited, and for example, organic acids, inorganic acids, organic bases, inorganic bases, metal alkoxides, metal chelates, etc. can be cited, and these catalysts can be used 1 or 2 or more in combination.

[0407] [Properties of coating composition (I)]

[0408] In the coating composition (I), from the viewpoint of coating properties, the solid content concentration is preferably 0.01 to 60% by mass, more preferably 1 to 40% by mass. In addition, from the viewpoint of coating properties, the viscosity of the coating composition (I) at 20° C. is preferably 0.1 to 100,000 mPa·s, more preferably 1 to 10,000 mPa·s.

[0409] <Method for preparing hard coating layer>

[0410] The method for preparing the hard coating in the present embodiment is not particularly limited. For example, polymer nanoparticles (A), matrix raw material components (B'), inorganic oxides (D), and other suitable components can be dispersed and dissolved in a solvent, and the obtained coating composition (I) is applied to the above-mentioned substrate, and a coating film is obtained by heat treatment, ultraviolet irradiation, infrared irradiation, etc. In addition, as the above-mentioned coating method, for example, spray spraying, flow coating, brush coating, dip coating, spin coating, screen printing, casting, gravure printing, flexographic printing, etc. can be cited but not limited to. It should be noted that the coating composition (I) after the above-mentioned coating is preferably made into a coating film by heat treatment or ultraviolet irradiation at a temperature of preferably room temperature to 250°C, more preferably 40°C to 150°C. In addition, the coating can not only be applied on a substrate that has been formed, but also can be pre-applied to a flat plate before forming processing, such as a pre-coated metal containing a rust-proof steel plate.

[0411] [Surface processing of hard coating]

[0412] In the hard coating layer in the present embodiment, from the aspect of weather resistance, the surface can be processed by silicon oxide to form a silicon oxide layer. There is no particular limitation on the method for forming the silicon oxide layer. As a specific example, silicon oxide processing based on PECVD that vapor deposits / cures silicone or silazane, and silicon oxide processing technology that modifies the surface into silicon oxide by irradiating 155nm ultraviolet rays can be cited. In particular, for the reason that a layer that is not easy to pass oxygen and water vapor can be made without deteriorating the surface, surface processing based on PECVD is preferred. Silicones or silazanes that can be used for PECVD can specifically include but are not limited to octamethylcyclotetrasiloxane, tetramethylcyclotetrasiloxane, decamethylcyclopentasiloxane, hexamethyldisiloxane, vinylmethoxysilane, vinylmethoxysilane, dimethyldimethoxysilane, TEOS, tetramethyldisiloxane, tetramethyltetravinylcyclotetrasiloxane, hexamethyldisiloxane, etc., and they can be used one or more than two.

[0413] In this embodiment, a functional layer may be further provided on at least one surface of the hard coat layer. Examples of the functional layer include, but are not limited to, an antireflection layer, an antifouling layer, a polarizing layer, and an impact absorbing layer.

[0414] [Haze value H1 of substrate with adhesive layer and haze value H2 of laminate]

[0415] In the laminate of the present embodiment, the haze value H1 of the substrate with the adhesive layer is greater than the haze value H2 of the laminate. By satisfying such a relationship, the laminate of the present embodiment forms a scattering layer at the interface between the substrate with the adhesive layer and the hard coating layer, thereby suppressing the generation of interference fringes and improving optical properties.

[0416] In the present embodiment, from the perspective of transparency, the haze value H1 of the substrate with the adhesive layer is preferably 60% or less, more preferably 50% or less, and further preferably 30% or less. From the same perspective, the haze value H2 of the laminate is preferably 5% or less, more preferably 2% or less, and further preferably 1% or less. As a method for adjusting each haze value to within the above range, for example, with respect to H1, a method for controlling the particle size of the adhesive emulsion particles (F), the particle size and shape of the inorganic oxide (G), the weight ratio of the adhesive emulsion particles (F) to the inorganic oxide (G), the content of the light-shielding agent, the content of the curing agent and other additives can be cited, and with respect to H2, a method for controlling the particle size of the polymer nanoparticles (A), the composition ratio of the polymer nanoparticles (A) to the matrix component (B), and the content of the inorganic oxide (D) in the matrix component (B) can be cited, but it is not limited thereto. In particular, when the amount of the inorganic oxide (G) or the inorganic oxide (D) is increased, each haze value tends to increase, and when the amount is decreased, each haze value tends to decrease.

[0417] Each haze value can be measured by the method described in the examples described later. It should be noted that, regarding the haze value H1, the substrate with an adhesive layer can be measured as an object, and regarding the haze value H2, the laminate (the substrate with an adhesive layer and the hard coat layer) can be measured as an object. The haze values ​​H1 and H2 can be measured respectively after forming the substrate with an adhesive layer and the laminate.

[0418] [Surface roughness Ra1 of the adhesive layer-attached substrate and surface roughness Ra2 of the laminate]

[0419] In the laminate of the present embodiment, the surface roughness Ra1 of the substrate with the adhesive layer is greater than the surface roughness Ra2 of the laminate. By satisfying such a relationship, the laminate of the present embodiment forms a scattering layer at the interface between the substrate with the adhesive layer and the hard coating layer, and as a result, the generation of interference fringes can be suppressed, thereby improving the optical properties.

[0420] In this embodiment, from the perspective of transparency, the surface roughness Ra1 of the substrate with the adhesive layer is preferably 500nm or less, more preferably 300nm or less, further preferably 200nm or less, and most preferably 150nm or less. In addition, in this embodiment, from the perspective of adhesion, the surface roughness Ra1 of the substrate with the adhesive layer is preferably 10nm or more, more preferably 20nm or more, and further preferably 40nm or more.

[0421] In addition, from the viewpoint of transparency, the surface roughness Ra2 of the laminate is preferably less than 100 nm, more preferably 50 nm or less, further preferably 30 nm or less, and further preferably 20 nm or less.

[0422] As a method for adjusting the surface roughness Ra1 and Ra2 to the above range, for example, with respect to Ra1, a method for controlling the particle size of the adhesive latex particles (F), the weight ratio of the adhesive latex particles (F) to the inorganic oxide (G), and the content of the sunscreen can be cited, and with respect to Ra2, a method for controlling the particle size of the polymer nanoparticles (A), the composition ratio of the polymer nanoparticles (A) to the matrix component (B), and the content of the inorganic oxide (D) in the matrix component (B) can be cited, but it is not limited thereto. In particular, if the amount of the inorganic oxide (G) or the inorganic oxide (D) is increased, the surface roughness Ra of each tends to increase, and if the above amount is reduced, the surface roughness Ra of each tends to decrease.

[0423] Each surface roughness Ra1 and Ra2 can be measured by the method described in the embodiment described later. It should be noted that, about surface roughness Ra1, the substrate with adhesive layer can be measured as an object, and about surface roughness Ra2, the laminate (substrate with adhesive layer and hard coat) can be measured as an object. Surface roughness Ra1 and Ra2 can be measured respectively after forming the substrate with adhesive layer and the laminate. In addition, the shape of the adhesive layer and the hard coat interface can be measured by the cross-sectional SEM image of the laminate, and the surface roughness Ra is calculated.

[0424] <Application of Laminated Body>

[0425] The laminate of the present embodiment has excellent wear resistance and durability. Therefore, the use of the hard coating film and the substrate with the hard coating film is not particularly limited, and examples thereof include building materials, vehicle parts, electronic equipment, and electrical products.

[0426] Examples of building material uses include, but are not limited to, window glass for construction machinery, window glass for buildings, houses, greenhouses, etc., roofs for garages and arcades, lighting such as lighting or signal lights, wallpaper surface materials, signs, sanitary products such as bathtubs and washstands, kitchen building materials, exterior wall materials, floor materials, cork materials, tiles, floor mats, interior floor materials such as linoleum.

[0427] As vehicle parts, there can be mentioned, but not limited to, parts used in various applications such as automobiles, aircraft, and trains. As specific examples, there can be mentioned various glasses such as front windshields, rear windshields, front doors, rear doors, rear side panels, sunroofs, front bumpers, rear bumpers, spoilers, door mirrors, front grilles, logo covers, exterior parts such as car bodies, interior parts such as center panels, door panels, instrument panels, center consoles, lamp parts such as headlights and taillights, lens parts for vehicle-mounted cameras, lighting covers, decorative films, and various glass replacement parts.

[0428] As electronic equipment and motor products, preferred examples include but are not limited to mobile phones, portable information terminals, personal computers, portable game consoles, OA equipment, solar cells, flat-panel displays, touch panels, DVDs, Blu-ray discs and other optical discs, polarizers, filters, lenses, prisms, optical fibers and other optical components, anti-reflection films, orientation films, polarizing films, phase difference films and other optical films, etc.

[0429] The laminate of the present embodiment can be applied to various fields such as machine parts, agricultural materials, fishery materials, transport containers, packaging containers, toys, and sundries in addition to the above-mentioned uses.

[0430] <<Second Embodiment>>

[0431] Here, a second mode of the present embodiment (hereinafter also referred to as “second embodiment”) will be described in detail.

[0432] <Hard Coating Film>

[0433] The hard coating film (hereinafter also referred to as "coating film (C)") of the present embodiment (hereinafter, unless otherwise specified, "present embodiment" in the <<Second embodiment>> refers to the second embodiment) is a hard coating film comprising polymer nanoparticles (A) and a matrix component (B), wherein the Martens hardness HM of the polymer nanoparticles (A) is A The Martens hardness HM of the matrix component (B) B Meet HM B / HM A >1, the Martens hardness HM of the hard coating film is 100N / mm 2In the above, the matrix component (B) includes an inorganic oxide (D), and the inorganic oxide (D) contains at least one inorganic component selected from the group consisting of Ce, Nb, Al, Zn, Ti, Zr, Sb, Mg, Sn, Bi, Co and Cu.

[0434] It should be noted that even in the case where it is difficult to confirm the above Martens hardness HM A and Martens hardness HM B In the case of the size relationship of the polymer nanoparticles (A) and the matrix component (B) described later, the size relationship of the Martens hardness can also be inferred by comparing the adhesion of the polymer nanoparticles (A) and the matrix component (B). The lower the adhesion, the higher the elasticity, so the lower the adhesion, the less likely the coating is to deform, indicating that the hardness is higher. Specifically, the hard coating film of the present embodiment can also be defined as follows. That is, the hard coating film of the present embodiment is a hard coating film comprising polymer nanoparticles (A) and a matrix component (B), and the adhesion F of the above-mentioned polymer nanoparticles (A) measured by the adhesion mode of a scanning probe microscope (SPM) is A Adhesion F to the above matrix component (B) B Satisfy F A / F B >1, the Martens hardness HM of the hard coating film is 100N / mm 2 In the above, the matrix component (B) includes an inorganic oxide (D), and the inorganic oxide (D) contains at least one inorganic component selected from the group consisting of Ce, Nb, Al, Zn, Ti, Zr, Sb, Mg, Sn, Bi, Co and Cu.

[0435] Since the hard coating film of the present embodiment is constructed as described above, it has high wear resistance, durability and weather resistance. The hard coating film of the present embodiment exhibits high levels of wear resistance, durability and weather resistance, and can be used as, but not limited to, hard coatings for building materials, automobile parts, electronic equipment, motor products, etc., and is particularly preferably used as automobile parts.

[0436] In the hard coating film of the present embodiment, the polymer nanoparticles (A) are preferably dispersed in the matrix component (B). "Dispersion" in the present embodiment means that the polymer nanoparticles (A) are used as the dispersed phase and the matrix component (B) is used as the continuous phase, so that the polymer nanoparticles (A) are evenly distributed in the matrix component (B), or distributed in the matrix component (B) while forming a structure. The above dispersion can be confirmed by cross-sectional SEM observation of the hard coating film. In the hard coating film of the present embodiment, the polymer nanoparticles (A) are dispersed in the matrix component (B) and tend to have high wear resistance.

[0437] It should be noted that in this specification, the Martens hardness HM is 100N / mm 2The above coating film is particularly called a "hard coating film".

[0438] [Martens hardness]

[0439] The Martens hardness in the present embodiment is the hardness obtained according to ISO14577-1, and is the value calculated by the indentation depth of 2mN under the measuring conditions (Vickers tetrahedral pyramid diamond indenter, load increase condition 2mN / 20sec, load reduction condition 2mN / 20sec). The Martens hardness in the present embodiment can be measured using, for example, a micro-hardness meter Fischerscope (Fischer Instruments manufactures HM2000S), an ultra-micro indentation hardness tester (Elionix Co., Ltd. manufactures ENT-NEXUS), a nano-indenter (Toyo Technica manufactures iNano, G200), and a nano-indentation system (Bruker manufactures TI980), and the shallower the indentation depth, the higher the Martens hardness, and the deeper the indentation depth, the lower the Martens hardness.

[0440] [Adhesion]

[0441] The adhesion in this embodiment can be measured using a scanning probe microscope (SPM). Since the lower the adhesion, the higher the elasticity, the lower the adhesion, the less likely the coating is to deform and the higher the hardness. The adhesion measurement method can be measured using, but not limited to, SPM-970, SPM-9700HT manufactured by Shimadzu Corporation, Dimension ICON manufactured by Bruker AXS, AFM5000II manufactured by Hitachi High-Tech Science, etc.

[0442] [Other hardness]

[0443] By determining the magnitude relation of measured values ​​as indexes with other hardnesses, the magnitude relation of Martens hardness and adhesive force in the above-mentioned present embodiment can also be inferred.As other hardnesses, as long as the index that the deformation of material is not easy to be represented after the material is applied with force is not particularly limited, the index represented by the logarithmic decrement rate measured by the Vickers hardness, indentation hardness, and the pendulum type viscoelasticity instrument represented by the rigid pendulum type physical property testing machine can be enumerated, which is measured by a microhardness meter, a nanoindentation tester as a representative, and measured by a pendulum type viscoelasticity instrument.In addition, the index represented by the phase, friction, viscoelasticity, adsorption, hardness and elastic modulus measured by a scanning probe microscope (SPM) can also be enumerated.In these indexes, if it is confirmed that the hardness of the matrix component (B) is higher than the hardness of polymer nanoparticles (A), then with regard to Martens hardness and adhesive force, it can also be inferred that the matrix component (B) is harder than polymer nanoparticles (A).

[0444] [Martens hardness HM of polymer nanoparticles (A) A Martens hardness HM of matrix component (B) B ]

[0445] The Martens hardness HM of the polymer nanoparticles (A) in this embodiment is A Martens hardness HM of matrix component (B) B The following relationship (1) is satisfied.

[0446] HM B / HM A >1 Formula (1)

[0447] Formula (1) indicates that soft polymer nanoparticles (A) exist in a hard matrix component (B). By making the hardness three-dimensionally inclined, the coating (C) can be endowed with wear resistance that is not exhibited in conventional coatings. The reason for this is not intended to be limiting, but it is presumed that the soft nanoparticles absorb impacts and the hard matrix component suppresses deformation. As HM A The range is preferably 50N / mm from the perspective of impact absorption. 2 More preferably 100 N / mm 2 Above, preferably 2000 N / mm from the viewpoint of film forming properties 2 Below, more preferably 800N / mm 2 Below, more preferably 350N / mm 2 Below. As HM B The range is preferably 100 N / mm from the perspective of impact absorption. 2 More preferably 150N / mm 2 The above, preferably 4000 N / mm from the viewpoint of film forming properties 2 Below, more preferably 2000N / mm 2 the following.

[0448] It should be noted that the coating film (C) can be obtained in the form of a cured product, which is obtained by curing the coating composition (I) described later by hydrolysis condensation or the like. For the polymer nanoparticles (A), the composition thereof generally does not change during the curing process. Therefore, the Martens hardness HM of the polymer nanoparticles (A) in the coating composition (I) measured by the method described in the examples described later is A The value of is related to the Martens hardness HM of the polymer nanoparticles (A) in the coating film (C) A The Martens hardness HM in the coating film (C) can be determined in this form. A The value of .

[0449] In addition, the matrix component (B) corresponds to a cured product obtained by curing the matrix raw material component (B') described later by hydrolysis condensation or the like. Therefore, the Martens hardness HM of the matrix raw material component (B') measured by the method described in the examples described later is B’ The value of the corresponding matrix component (B) is the Martens hardness HM B In good agreement, the Martens hardness HM can be determined in this form B The value of .

[0450] The above HM A and H.M. B The values ​​of can be adjusted to the above-mentioned magnitude relationship by the structures and composition ratios of the constituent components of the polymer nanoparticles (A) and the matrix raw material component (B') described later, and the method is not particularly limited.

[0451] [Adhesion force F of polymer nanoparticles (A) A Adhesion F to matrix component (B) B ]

[0452] The adhesion force F of the polymer nanoparticles (A) in this embodiment is A Adhesion F to the matrix component (B) B The following relationship (2) is satisfied.

[0453] F A / F B >1 Formula (2)

[0454] Similar to the above formula (1), formula (2) also indicates that soft polymer nanoparticles (A) exist in a hard matrix component (B), and by making the hardness have a three-dimensional inclination in this way, the coating (C) can be endowed with wear resistance that is not exhibited in conventional coatings. The reason for this is not intended to be limiting, but it is presumed that the soft nanoparticles absorb impacts and the hard matrix component suppresses deformation.

[0455] As mentioned above, the adhesion force F of the polymer nanoparticles (A) A Adhesion F to matrix component (B) B The hardness of each component can be adjusted to the above-mentioned size relationship by adjusting the structure and composition ratio of the constituent components of the polymer nanoparticles (A) and the matrix raw material component (B') described later, and the method is not particularly limited.

[0456] [Martens hardness HM of coating film (C)]

[0457] The Martens hardness HM of the coating film (C) is 100 N / mm from the viewpoint of wear resistance. 2As described above, the higher the Martens hardness HM, the less deformation due to impact and the less damage associated with destruction, which is advantageous from this point of view. The Martens hardness HM of the coating film (C) is preferably 150 N / mm from the perspective of wear resistance. 2 More than, more preferably 200N / mm 2 Above, preferably 4000 N / mm from the viewpoint of flexural resistance 2 Below, more preferably 2000N / mm 2 Below, more preferably 1500 N / mm 2 As follows. As a method for adjusting the Martens hardness HM of the coating film (C) to the above range, there can be cited, but not limited to, for example, mixing the polymer nanoparticles (A) satisfying the specific relationship represented by the formula (3) described later with the matrix raw material component (B') described later and dispersing and dissolving the obtained composition in a solvent, applying the obtained coating composition to a substrate, and forming a coating film by heat treatment, ultraviolet irradiation, infrared irradiation, etc. In particular, if the content of the matrix component (B) increases relative to the total amount of the polymer nanoparticles (A) and the matrix component (B), the Martens hardness HM of the coating film (C) tends to increase, and if the content of the matrix component (B) decreases, the Martens hardness HM of the coating film (C) tends to decrease.

[0458] [Haze change in Taber abrasion test]

[0459] The Taber abrasion test in this embodiment is measured according to the method described in ASTMD1044, and is measured under the conditions of abrasion wheel CS-10F and a load of 500g. The smaller the change in haze, the better the wear resistance of the material. When the change in haze at 1000 rotations relative to the haze before the test, that is, the difference between the haze at a rotation speed of 1000 times and the haze before the Taber abrasion test is 10 or less, it is suitable for the standard of automobile windows and can be suitably used as a hard coating film for automobile windows. When it is 2 or less, it is suitable for the standards of ANSI / SAE Z.26.1, ECE R43, and JIS R3211 / R3212, and can be suitably used for all automobile window materials. It is preferred that the difference between the haze at a rotation speed of 1000 times and the haze before the Taber abrasion test is 10 or less, more preferably 6 or less, and further more preferably 2 or less. Methods for adjusting the haze change to within the above range include, but are not limited to, mixing polymer nanoparticles (A) satisfying the specific relationship represented by formula (3) described later with a matrix raw material component (B') described later, dispersing and dissolving the resulting composition in a solvent, applying the resulting coating composition on a substrate, and forming a coating film by heat treatment, ultraviolet irradiation, infrared irradiation, etc.

[0460] [Difference between the haze at 500 rotations and the haze at 10 rotations in Taber abrasion test (hereinafter also referred to as "ΔA")]

[0461] The ΔA of the coating (C) represents the difference between the haze at a rotation speed of 500 times and the haze at a rotation speed of 10 times in the above-mentioned Taber abrasion test. The lower the ΔA, the better the long-term pollution resistance, and thus it is preferred. That is, from the perspective of showing higher pollution resistance, it is preferred that ΔA is less than 10, more preferably less than 7, and further preferably less than 5. The detailed reason is still unclear, and it is speculated that, for example, the lower the ΔA, the less likely the pollutant is to fall into the film, and there is a tendency for the pollutant to be excellent in cleaning. As a method for adjusting the ΔA of the coating (C) to within the above range, for example, polymer nanoparticles (A) that satisfy the specific relationship represented by the formula (3) described later are mixed with the matrix raw material component (B') described later and the obtained composition is dispersed and dissolved in a solvent, the obtained coating composition is applied to a substrate, and a coating is made by heat treatment, ultraviolet irradiation, infrared irradiation, etc. In particular, the composition of the polymer nanoparticles (A), the composition of the matrix raw material component (B') described later, and the mixing ratio can be mentioned. In addition, the mixing conditions include, for example, the solvent composition, the mixing order, the stirring time, the solid content concentration, etc., and the film-forming conditions include, for example, the drying temperature, humidity, and drying time in the case of heat treatment, the irradiation intensity, irradiation time, and humidity in the case of ultraviolet irradiation, and the irradiation intensity, irradiation time, and humidity in the case of infrared irradiation.

[0462] [Elastic recovery rate η of coating film (C) IT ]

[0463] Elastic recovery rate η of coating film (C) IT is the total mechanical work done by the depression W total The amount of work done by the elastic recovery deformation of the concave elast The ratio is defined as “W elast / W total The ratio η IT "Parameters recorded. Elastic recovery rate η IT The higher the value, the more the coating can recover to its original state after deformation, and the higher the self-repair ability of the deformation. IT Under the measurement conditions (Vickers tetrahedral diamond indenter, load increase condition 2mN / 20sec, load decrease condition 2mN / 20sec), it is preferably 0.50 or more. As long as it is within this range, the larger the value, the more preferred. More specifically, the elastic recovery rate η ITMore preferably, it is 0.55 or more, further preferably 0.60 or more, and further preferably 0.65 or more. The elastic recovery rate of the coating film in this embodiment can be measured by, but not limited to, for example, using a micro hardness meter Fischerscope (HM2000S manufactured by Fischer Instruments), an ultra-micro indentation hardness tester (ENT-NEXUS manufactured by Elionix Co., Ltd.), a nanoindenter (iNano, G200 manufactured by Toyo Technica), a nanoindentation system (TI980 manufactured by Bruker), etc. to perform an indentation test on the surface of the hard coating film. As a method for measuring the elastic recovery rate η IT The method for adjusting to the above range may include, but is not limited to, mixing polymer nanoparticles (A) satisfying the specific relationship represented by formula (3) described later with the matrix raw material component (B') described later, dispersing and dissolving the obtained composition in a solvent, applying the obtained coating composition on a substrate, and forming a coating film by heat treatment, ultraviolet irradiation, infrared irradiation, etc.

[0464] [Thickness of coating film (C)]

[0465] In this embodiment, from the perspective of further demonstrating the wear resistance of the hard coating film and fully ensuring the conformability to the deformation of the substrate, it is preferred to appropriately adjust the film thickness. Specifically, from the perspective of wear resistance, the film thickness of the coating (C) is preferably 1.0 μm or more, more preferably 3.0 μm or more. In addition, from the perspective of weather resistance and substrate conformability, the film thickness of the coating (C) is preferably 100.0 μm or less, more preferably 50.0 μm or less, and further preferably 20.0 μm or less.

[0466] [Polymer nanoparticles (A)]

[0467] By using the polymer nanoparticles (A) in this embodiment, impact absorption can be imparted to the hard coating film, and the haze change of the hard coating film in the Taber abrasion test can be reduced. Regarding the polymer nanoparticles (A), as long as the particle size is of the order of nm (less than 1 μm), there is no particular limitation on the shape. It should be noted that the Martens hardness HM of the polymer nanoparticles (A) is A The above range can be controlled by the structure and composition ratio of the constituent components of the polymer nanoparticles (A), and the method is not particularly limited.

[0468] [Average particle size of polymer nanoparticles (A)]

[0469] The average particle size of the polymer nanoparticles (A) in this embodiment is not particularly limited as long as it is of the order of nm (less than 1 μm), and is obtained by observing the particle size by cross-sectional SEM or dynamic light scattering. From the perspective of optical properties, the average particle size of the polymer nanoparticles (A) is preferably greater than 10 nm, more preferably greater than 15 nm, and further preferably greater than 20 nm. From the perspective of transparency, the average particle size is preferably less than 400 nm, more preferably less than 200 nm, and further preferably less than 100 nm. Regarding the method for measuring the average particle size of the polymer nanoparticles (A), for example, but not limited to, the cumulative particle size can be measured using a dynamic light scattering particle size distribution measuring device (model: ELSZ-1000) manufactured by Otsuka Electronics Co., Ltd. using an aqueous dispersion of the polymer nanoparticles (A).

[0470] [Volume Fraction of Polymer Nanoparticles (A) in Coating Film (C)]

[0471] In the present embodiment, the volume fraction of the polymer nanoparticles (A) in the coating (C) is preferably 2% or more from the aspect of film-forming properties, and preferably 80% or less from the aspect of transparency. That is, the volume fraction of the polymer nanoparticles (A) in the coating (C) is preferably 2% or more and 80% or less, more preferably 3% or more and 70% or less, and further preferably 5% or more and 45% or less. The volume fraction of the polymer nanoparticles (A) in the coating (C) can be calculated, for example, based on the proportion of the polymer nanoparticles (A) in the entire coating in the cross-sectional SEM image of the coating (C) and the component ratio of the polymer nanoparticles (A) in the components constituting the coating (C).

[0472] [Constitutional components of polymer nanoparticles (A)]

[0473] [Hydrolyzable silicon compound (a)]

[0474] The polymer nanoparticles (A) in the present embodiment preferably contain a hydrolyzable silicon compound (a). The hydrolyzable silicon compound (a) is not particularly limited as long as it is a hydrolyzable silicon compound, a hydrolyzate thereof, or a condensate thereof.

[0475] From the viewpoint of improving abrasion resistance and weather resistance, the hydrolyzable silicon compound (a) is preferably a compound containing an atomic group represented by the following formula (a-1), or a hydrolyzate or condensate thereof.

[0476] -R 1 n1 SiX 1 3-n1 (a-1)

[0477] In formula (a-1), R 1represents a hydrogen atom, an alkyl group, an alkenyl group, an alkynyl group or an aryl group having 1 to 10 carbon atoms, and R 1 It may have a substituent containing a halogen, hydroxyl, mercapto, amino, (meth)acryloyl or epoxy group, X 1 represents a hydrolyzable group, and n1 represents an integer of 0 to 2. The hydrolyzable group is not particularly limited as long as it is a group that generates a hydroxyl group by hydrolysis, and examples of such a group include halogen, alkoxy, acyloxy, amino, phenoxy, and oxime groups.

[0478] Specific examples of compounds containing the atomic group represented by formula (a-1) include, but are not limited to, trimethoxysilane, triethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, propyltrimethoxysilane, propyltriethoxysilane, isobutyltriethoxysilane, hexyltrimethoxysilane, hexyltriethoxysilane, octyltrimethoxysilane, octyltriethoxysilane, decyltrimethoxysilane, decyltriethoxysilane, cyclohexyltrimethoxysilane, cyclohexyltriethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, dimethoxysilane, diethoxysilane, methyldimethoxysilane, methyldiethoxysilane, Dimethyldimethoxysilane, dimethyldiethoxysilane, dimethoxydiphenylsilane, diethoxydiphenylsilane, bis(trimethoxysilyl)methane, bis(triethoxysilyl)methane, bis(triphenoxysilyl)ethane, 1,1-bis(triethoxysilyl)ethane, 1,2-bis(triethoxysilyl)ethane, 1,1-bis(triethoxysilyl)propane, 1,2-bis(triethoxysilyl)propane, 1,3-bis(triethoxysilyl)propane, 1,4-bis(triethoxysilyl)butane, 1,5-bis(triethoxysilyl)pentane, 1,1-bis(trimethoxysilyl)ethane, 1,2-bis(trimethoxysilyl) 1,1-bis(trimethoxysilyl)propane, 1,2-bis(trimethoxysilyl)propane, 1,3-bis(trimethoxysilyl)propane, 1,4-bis(trimethoxysilyl)butane, 1,5-bis(trimethoxysilyl)pentane, 1,3-bis(triphenoxysilyl)propane, 1,4-bis(trimethoxysilyl)benzene, 1,4-bis(triethoxysilyl)benzene, 1,6-bis(trimethoxysilyl)hexane, 1,6-bis(triethoxysilyl)hexane, 1,7-bis(trimethoxysilyl)heptane, 1,7-bis(triethoxysilyl)heptane, 1,8-bis(trimethoxysilyl)octane, 1, 8-Bis(triethoxysilyl)octane, 3-chloropropyltrimethoxysilane, 3-chloropropyltriethoxysilane, trifluoropropyltrimethoxysilane, trifluoropropyltriethoxysilane, 3-hydroxypropyltrimethoxysilane, 3-hydroxypropyltriethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropylmethyldiethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane,4-epoxycyclohexyl)ethyl triethoxysilane, 3-acryloxypropyl trimethoxysilane, 3-acryloxypropyl triethoxysilane, 3-methacryloxypropyl trimethoxysilane, 3-methacryloxypropyl triethoxysilane, 3-methacryloxypropyl methyl dimethoxysilane, 3-methacryloxypropyl methyl dimethoxysilane, vinyl trimethoxysilane, vinyl triethoxysilane, p-phenylene trimethoxysilane, p-phenylene triethoxysilane, N-2-(aminoethyl)-3-aminopropyl methyl dimethoxysilane, N-2 -(Aminoethyl)-3-aminopropylmethyldiethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane, N-phenyl-3-aminopropyltriethoxysilane, 3-trimethoxysilyl-N-(1,3-dimethyl-butylene)propylamine, 3-triethoxysilyl-N-(1,3-dimethyl-butylene)propylamine, triacetoxysilane, Tris(trichloroacetoxy)silane, tris(trifluoroacetoxy)silane, tris(trimethoxysilylpropyl)isocyanurate, tris(triethoxysilylpropyl)isocyanurate, methyltriacetoxysilane, methyltris(trichloroacetoxy)silane, trichlorosilane, tribromosilane, methyltrifluorosilane, tris(methylethylketoxime)silane, phenyltris(methylethylketoxime)silane, bis(methylethylketoxime)silane, methylbis(methylethylketoxime)silane, hexamethyldisilane, hexamethylcyclotrisilazane, bis(dimethylamino)dimethylsilane, bis(diethylamino)dimethylsilane, (Dimethylamino) methylsilane, bis(diethylamino) methylsilane, 2-[(triethoxysilyl) propyl] dibenzylresorcinol, 2-[(trimethoxysilyl) propyl] dibenzylresorcinol, 2,2,6,6-tetramethyl-4-[3-(triethoxysilyl) propoxy] piperidine, 2,2,6,6-tetramethyl-4-[3-(trimethoxysilyl) propoxy] piperidine, 2-hydroxy-4-[3-(triethoxysilyl) propoxy] benzophenone, 2-hydroxy-4-[3-(trimethoxysilyl) propoxy] benzophenone, etc.

[0479] The hydrolyzable silicon compound (a) preferably includes a compound represented by the following formula (a-2), a hydrolyzate thereof, and a condensate thereof, from the viewpoint of being able to impart high hardness to the hard coating film and further improving the wear resistance.

[0480] SiX 2 4(a-2)

[0481] In formula (a-2), X 2The hydrolyzable group is not particularly limited as long as it is a group that generates a hydroxyl group by hydrolysis, and examples thereof include halogen, alkoxy, acyloxy, amino, phenoxy, and oxime groups.

[0482] Specific examples of the compound represented by formula (a-2) include, but are not limited to, tetramethoxysilane, tetraethoxysilane, tetra(n-propoxy)silane, tetra(isopropoxy)silane, tetra(n-butoxy)silane, tetra(isobutoxy)silane, tetra-sec-butoxysilane, tetra-tert-butoxysilane, tetraacetoxysilane, tetra(trichloroacetoxy)silane, tetra(trifluoroacetoxy)silane, tetrachlorosilane, tetrabromosilane, tetrafluorosilane, tetra(methyl ethyl ketoxime)silane, and partially hydrolyzed condensates of tetramethoxysilane or tetraethoxysilane (e.g., trade names "M-Silicate 51", "Silicate 35", "Silicate 45", "Silicate 40", and "FR-3" manufactured by Tama Chemical Industries, Ltd.; trade names "MS51", "MS56", "MS57", and "MS56S" manufactured by Mitsubishi Chemical Corporation; trade names "Methyl Silicate 51", "Methyl Silicate 35", "Si ... 53A", "Ethyl Silicate 40", "Ethyl Silicate 48", "EMS-485", "N-103X", "PX", "PS-169", "PS-162R", "PC-291", "PC-301", "PC-302R", "PC-309", "EMSi48"), etc.

[0483] As described above, in this embodiment, the hydrolyzable silicon compound (a) preferably includes one or more selected from the group consisting of compounds containing the atomic group represented by the above formula (a-1), their hydrolysis products and condensation products, and compounds represented by the above formula (a-2), their hydrolysis products and condensation products.

[0484] [Content of the hydrolyzable silicon compound (a) in the polymer nanoparticles (A)]

[0485] The content of the hydrolyzable silicon compound (a) in the present embodiment represents the solid content weight ratio of the hydrolyzable silicon compound (a) contained in the polymer nanoparticles (A). The higher the content, the better the wear resistance, weather resistance and heat resistance. The content is preferably 50% by mass or more, more preferably 60% by mass or more. The content of the hydrolyzable silicon compound (a) in the polymer nanoparticles (A) can be measured by, but not limited to, IR analysis, NMR analysis, elemental analysis, etc. of the polymer nanoparticles (A).

[0486] [Matrix component (B)]

[0487] By using the matrix component (B) in this embodiment, impact absorption can be imparted to the hard coating film, and the amount of change in haze of the hard coating film in the Taber abrasion test can be reduced. B The above range can be controlled by the structure and composition ratio of the constituent components of the matrix raw material component (B') described later, and the method is not particularly limited.

[0488] [Constituents of the matrix component (B)]

[0489] [Hydrolyzable silicon compound (b)]

[0490] The matrix component (B) in the present embodiment is not particularly limited as long as it is a component that can disperse the polymer nanoparticles (A). In the present embodiment, from the aspect of high toughness, the matrix component (B) preferably contains a hydrolyzable silicon compound (b). In this specification, "the matrix component (B) contains a hydrolyzable silicon compound (b)" means that the matrix component (B) contains a polymer having a structural unit derived from the hydrolyzable silicon compound (b). The hydrolyzable silicon compound (b) is not particularly limited as long as it is a hydrolyzable silicon compound, its hydrolyzate and condensate.

[0491] As the matrix component (B), in addition to the above-mentioned polymers, various components other than the polymer nanoparticles (A) may be included. Among them, as other polymers that may be included in addition to the above-mentioned polymers, water-soluble resins such as polyvinyl alcohol, polyethylene glycol, polyvinyl pyrrolidone, and polyacrylic acid; acrylic resins such as PMMA, PAN, and polyacrylamide; polymers such as polystyrene, polyurethane, polyamide, polyimide, polyvinylidene chloride, polyester, polycarbonate, polyether, polyethylene, polysulfone, polypropylene, polybutadiene, PTFE, PVDF, and EVA; and copolymers thereof, etc.

[0492] From the perspective of further improving wear resistance and weather resistance, the hydrolyzable silicon compound (b) preferably contains one or more selected from the group consisting of a compound containing an atomic group represented by the following formula (b-1), its hydrolysis products and condensation products, and a compound represented by the following formula (b-2), its hydrolysis products and condensation products.

[0493] -R 2 n2 SiX 3 3-n2 (b-1)

[0494] In formula (b-1), R 2 represents a hydrogen atom, an alkyl group, an alkenyl group, an alkynyl group or an aryl group having 1 to 10 carbon atoms, and R 2It may have a substituent containing a halogen, hydroxyl, mercapto, amino, (meth)acryloyl or epoxy group, X 3 represents a hydrolyzable group, and n2 represents an integer of 0 to 2. The hydrolyzable group is not particularly limited as long as it is a group that generates a hydroxyl group by hydrolysis, and examples of such a group include a halogen atom, an alkoxy group, an acyloxy group, an amino group, a phenoxy group, and an oxime group.

[0495] SiX 4 4(b-2)

[0496] In formula (b-2), X 4 The hydrolyzable group is not particularly limited as long as it is a group that generates a hydroxyl group by hydrolysis, and examples of such a group include halogen, alkoxy, acyloxy, amino, phenoxy, and oxime groups.

[0497] Specific examples of the compound containing the atomic group represented by the general formula (b-1) include, but are not limited to, trimethoxysilane, triethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, propyltrimethoxysilane, propyltriethoxysilane, isobutyltriethoxysilane, hexyltrimethoxysilane, hexyltriethoxysilane, octyltrimethoxysilane, octyltriethoxysilane, decyltrimethoxysilane, decyltriethoxysilane, cyclohexyltrimethoxysilane, cyclohexyltriethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, dimethoxysilane, diethoxysilane, methyldimethoxysilane, methyldiethoxysilane, dimethoxysilane Methyldimethoxysilane, dimethyldiethoxysilane, dimethoxydiphenylsilane, diethoxydiphenylsilane, bis(trimethoxysilyl)methane, bis(triethoxysilyl)methane, bis(triphenoxysilyl)ethane, 1,1-bis(triethoxysilyl)ethane, 1,2-bis(triethoxysilyl)ethane, 1,1-bis(triethoxysilyl)propane, 1,2-bis(triethoxysilyl)propane, 1,3-bis(triethoxysilyl)propane, 1,4-bis(triethoxysilyl)butane, 1,5-bis(triethoxysilyl)pentane, 1,1-bis(trimethoxysilyl)ethane, 1,2-bis(trimethoxysilyl) )ethane, 1,1-bis(trimethoxysilyl)propane, 1,2-bis(trimethoxysilyl)propane, 1,3-bis(trimethoxysilyl)propane, 1,4-bis(trimethoxysilyl)butane, 1,5-bis(trimethoxysilyl)pentane, 1,3-bis(triphenoxysilyl)propane, 1,4-bis(trimethoxysilyl)benzene, 1,4-bis(triethoxysilyl)benzene, 1,6-bis(trimethoxysilyl)hexane, 1,6-bis(triethoxysilyl)hexane, 1,7-bis(trimethoxysilyl)heptane, 1,7-bis(triethoxysilyl)heptane, 1,8-bis(trimethoxysilyl)octane, 1, 8-Bis(triethoxysilyl)octane, 3-chloropropyltrimethoxysilane, 3-chloropropyltriethoxysilane, trifluoropropyltrimethoxysilane, trifluoropropyltriethoxysilane, 3-hydroxypropyltrimethoxysilane, 3-hydroxypropyltriethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropylmethyldiethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane,4-epoxycyclohexyl)ethyl triethoxysilane, 3-acryloxypropyl trimethoxysilane, 3-acryloxypropyl triethoxysilane, 3-methacryloxypropyl trimethoxysilane, 3-methacryloxypropyl triethoxysilane, 3-methacryloxypropyl methyl dimethoxysilane, 3-methacryloxypropyl methyl dimethoxysilane, vinyl trimethoxysilane, vinyl triethoxysilane, p-phenylene trimethoxysilane, p-phenylene triethoxysilane, N-2-(aminoethyl)-3-aminopropyl methyl dimethoxysilane, N-2 -(Aminoethyl)-3-aminopropylmethyldiethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane, N-phenyl-3-aminopropyltriethoxysilane, 3-trimethoxysilyl-N-(1,3-dimethyl-butylene)propylamine, 3-triethoxysilyl-N-(1,3-dimethyl-butylene)propylamine, triacetoxysilane, Tris(trichloroacetoxy)silane, tris(trifluoroacetoxy)silane, tris(trimethoxysilylpropyl)isocyanurate, tris(triethoxysilylpropyl)isocyanurate, methyltriacetoxysilane, methyltris(trichloroacetoxy)silane, trichlorosilane, tribromosilane, methyltrifluorosilane, tris(methylethylketoxime)silane, phenyltris(methylethylketoxime)silane, bis(methylethylketoxime)silane, methylbis(methylethylketoxime)silane, hexamethyldisilane, hexamethylcyclotrisilazane, bis(dimethylamino)dimethylsilane, bis(diethylamino)dimethylsilane, (Dimethylamino) methylsilane, bis(diethylamino) methylsilane, 2-[(triethoxysilyl) propyl] dibenzylresorcinol, 2-[(trimethoxysilyl) propyl] dibenzylresorcinol, 2,2,6,6-tetramethyl-4-[3-(triethoxysilyl) propoxy] piperidine, 2,2,6,6-tetramethyl-4-[3-(trimethoxysilyl) propoxy] piperidine, 2-hydroxy-4-[3-(triethoxysilyl) propoxy] benzophenone, 2-hydroxy-4-[3-(trimethoxysilyl) propoxy] benzophenone, etc.

[0498] Specific examples of the compound represented by formula (b-2) include, but are not limited to, tetramethoxysilane, tetraethoxysilane, tetra(n-propoxy)silane, tetra(isopropoxy)silane, tetra(n-butoxy)silane, tetra(isobutoxy)silane, tetra-sec-butoxysilane, tetra-tert-butoxysilane, tetraacetoxysilane, tetra(trichloroacetoxy)silane, tetra(trifluoroacetoxy)silane, tetrachlorosilane, tetrabromosilane, tetrafluorosilane, tetra(methyl ethyl ketoxime)silane, and partially hydrolyzed condensates of tetramethoxysilane or tetraethoxysilane (e.g., trade names "M-Silicate 51", "Silicate 35", "Silicate 45", "Silicate 40", and "FR-3" manufactured by Tama Chemical Industries, Ltd.; trade names "MS51", "MS56", "MS57", and "MS56S" manufactured by Mitsubishi Chemical Corporation; trade names "Methyl Silicate 51", "Methyl Silicate 35", "Si ..." and "Silicate 35" manufactured by Mitsubishi Chemical Corporation; and trade names "Methyl Silicate 51", "Methyl Silicate 5 53A", "Ethyl Silicate 40", "Ethyl Silicate 48", "EMS-485", "N-103X", "PX", "PS-169", "PS-162R", "PC-291", "PC-301", "PC-302R", "PC-309", "EMSi48"), etc.

[0499] As described above, in this embodiment, the hydrolyzable silicon compound (b) preferably includes one or more selected from the group consisting of compounds containing the atomic group represented by the above formula (b-1), their hydrolysis products and condensation products, and compounds represented by the above formula (b-2), their hydrolysis products and condensation products.

[0500] In the present embodiment, the "hydrolyzable silicon compound (a) contained in the polymer nanoparticles (A)" and the "hydrolyzable silicon compound (b) contained in the matrix component (B)" may be of the same kind or of different kinds. Even when the two are of the same kind, they can be distinguished by making the hydrolyzable silicon compound (a) contained in the polymer nanoparticles (A) and the hydrolyzable silicon compound (b) contained in the matrix component (B).

[0501] [Inorganic oxide (D)]

[0502] The matrix component (B) in the present embodiment includes an inorganic oxide (D). By including an inorganic oxide (D), not only the hardness of the matrix component (B) can be improved, the wear resistance can be improved, but also the tendency of improving the pollution resistance of the coating film by the hydrophilicity of the hydroxyl groups on the particle surface. In addition, the inorganic oxide (D) contains at least one inorganic component (hereinafter also referred to as "inorganic component") selected from the group consisting of Ce, Nb, Al, Zn, Ti, Zr, Sb, Mg, Sn, Bi, Co and Cu. By including this inorganic component, the inorganic oxide (D) can improve weather resistance without damaging wear resistance and durability. When commercial products are used, examples include, but are not limited to, ultrafine particle material products of cerium oxide, zinc oxide, aluminum oxide, bismuth oxide, cobalt oxide, copper oxide, tin oxide, and titanium oxide manufactured by CIK Nano Tek Co., Ltd.; titanium oxide "Tainoc" (trade name), cerium oxide "Needral" (trade name), tin oxide "Ceramace" (trade name), niobium oxide sol, and zirconium oxide sol manufactured by Taki Chemical Co., Ltd. From the perspective of improving weather resistance, the inorganic oxide (D) preferably contains at least one inorganic component selected from the group consisting of Ce, Nb, Zn, Ti, and Zr, and more preferably contains Ce.

[0503] From the perspective of the balance between wear resistance, durability and weather resistance, the inorganic component in the inorganic oxide (D) in the present embodiment preferably contains at least one inorganic oxide (D') selected from the group consisting of Ce, Nb, Zn, Ti and Zr. The content of the inorganic oxide (D') in the hard coating film is not particularly limited. From the perspective of the balance between wear resistance, durability and weather resistance, it is preferably 1% by mass or more, and more preferably 2% by mass or more. In addition, from the perspective of transparency, it is preferably 50% by mass or less, and more preferably 30% by mass or less. Here, the above content can be determined as the total amount of Ce, Nb, Zn, Ti and Zr when the hard coating film is 100% by mass.

[0504] As a specific example of the inorganic oxide (D) in the present embodiment, in addition to the oxides of aluminum, titanium, zirconium, zinc, cerium, tin, antimony, niobium, magnesium, bismuth, cobalt, copper, etc. as the inorganic components, oxides of silicon, indium, gallium, germanium, molybdenum, etc. can also be cited, but are not limited to this. Regardless of their shape, they can be used alone or in the form of a mixture. As an inorganic oxide (D), there is no particular limitation as long as it contains an inorganic component. From the perspective of the interaction with the above-mentioned hydrolyzable silicon compound (b), it is preferably further included with dry silica, colloidal silica as the representative of silica particles, from the perspective of dispersibility, as the form of silica particles, it is preferably further included colloidal silica. When the inorganic oxide (D) contains colloidal silica, it is preferably in the form of an aqueous dispersion, and any of acidic and alkaline can be used.

[0505] [Average particle size of inorganic oxide (D)]

[0506] The average particle size of the inorganic oxide (D) in the present embodiment is preferably 2 nm or more from the perspective of good storage stability of the composition of the hard coating film, and preferably 150 nm or less from the perspective of good transparency. That is, the average particle size of the inorganic oxide (D) is preferably 2 nm or more and 150 nm or less, more preferably 2 nm or more and 100 nm or less, and further preferably 2 nm or more and 50 nm or less. The method for measuring the average particle size (D) of the inorganic oxide can be, for example, but not limited to, the following method: observe the water-dispersed colloidal silica using a transmission microscope photograph magnified 50,000 to 100,000 times, and photograph 100 to 200 inorganic oxides as particles, and measure the average value of the major and minor diameters of the inorganic oxide particles.

[0507] In addition, when the inorganic oxide (D) contains two or more inorganic oxides, the average value of the average particle diameters of the respective inorganic oxides is taken as the average particle diameter of the inorganic oxide (D) in the hard coating film or the coating composition.

[0508] [Colloidal Silica Which May Be Contained in the Inorganic Oxide (D)]

[0509] The acidic colloidal silica using water as a dispersion solvent suitable for use in the present embodiment is not particularly limited, and can be prepared by a sol-gel method or a commercially available product. When prepared by a sol-gel method, reference can be made to Werner Stober et al; J. Colloid and Interface Sci., 26, 62-69 (1968), Rickey D. Badley et al; Lang muir 6, 792-801 (1990), Journal of the Color Society, 61 [9] 488-493 (1988), etc. When commercially available products are used, for example, Snowtex-O, Snowtex-OS, Snowtex-OXS, Snowtex-O-40, Snowtex-OL, Snowtex OYL, Snowtex-OUP, Snowtex-PS-SO, Snowtex-PS-MO, Snowtex-AK-XS, Snowtex-AK, Snowtex-AK-L, Snowtex-AK-YL, Snowtex-AK-PS-S (trade names, manufactured by Nissan Chemical Industries, Ltd.), Adelite AT-20Q (trade name, manufactured by Asahi Denka Industries, Ltd.), Klebosol 20H12, Klebosol 30CAL25 (trade names, manufactured by Clariant (Japan) Ltd.), etc. may be mentioned.

[0510] In addition, as the basic colloidal silica, there are silicas stabilized by the addition of alkali metal ions, ammonium ions, or amines, and examples thereof include, but are not limited to, Snowtex-20, Snowtex-30, Snowtex-XS, Snowtex-50, Snowtex-30L, Snowtex-XL, Snowtex-YL, Snowtex ZL, Snowtex-UP, Snowtex-ST-PS-S, Snowtex ST-PS-M, Snowtex-C, Snowtex-CXS, Snowtex-CM, Snowtex-N, Snowtex-NXS, Snowtex-NS, and Snowtex-N-40 (trade names, manufactured by Nissan Chemical Industries, Ltd.), Adelite AT-20, Adelite AT-30, Adelite AT-20N, Adelite AT-30N, Adelite AT-20A, Adelite AT-30A, Adelite AT-40, and Adelite AT-50 (trade name, manufactured by Asahi Electric Industries, Ltd.), Klebosol 30R9, Klebosol 30R50, Klebosol 50R50 (trade name, manufactured by Clariant Japan Ltd.), Ludox HS-40, Ludox HS-30, Ludox LS, Ludox AS-30, Ludox SM-AS, Ludox AM, Ludox HSA and Ludox SM (trade name, manufactured by DuPont), etc.

[0511] In addition, there is no particular limitation on the colloidal silica using a water-soluble solvent as a dispersion medium, and examples thereof include MA-ST-M (methanol dispersion type with a particle size of 20 to 25 nm), IPA-ST (isopropanol dispersion type with a particle size of 10 to 15 nm), EG-ST (ethylene glycol dispersion type with a particle size of 10 to 15 nm), EGST-ZL (ethylene glycol dispersion type with a particle size of 70 to 100 nm), NPC-ST (ethylene glycol monopropyl ether dispersion type with a particle size of 10 to 15 nm), and TOL-ST (toluene dispersion type with a particle size of 10 to 15 nm) manufactured by Nissan Chemical Industries, Ltd.

[0512] The dry silica particles are not particularly limited, and examples thereof include AEROSIL manufactured by NIPPON AEROSIL CO., LTD. and REOLOSIL manufactured by TOKUYAMA CO., LTD.

[0513] Furthermore, these silicon oxide particles may contain an inorganic base (sodium hydroxide, potassium hydroxide, lithium hydroxide, ammonia, etc.) or an organic base (tetramethylammonium, triethylamine, etc.) as a stabilizer.

[0514] [Shape of Inorganic Oxide (D)]

[0515] In addition, the shape of the inorganic oxide (D) in this embodiment can be, but is not limited to, spherical, square, polyhedral, elliptical, flat, linear, beaded, pearly, etc., and is particularly preferably spherical from the perspective of hardness and transparency of the hard coating film.

[0516] [Functional group (e)]

[0517] In the polymer nanoparticles (A) in the present embodiment, it is preferred to have a functional group (e) that interacts with the matrix component (B) from the aspect of being able to improve the dispersibility of the polymer nanoparticles (A) in the matrix component (B) and improving the wear resistance. The situation that the polymer nanoparticles (A) have the functional group (e) can be confirmed by, for example, composition analysis based on IR, GC-MS, thermal decomposition GC-MS, LC-MS, GPC, MALDI-MS, TOF-SIMS, TG-DTA, NMR and analysis based on their combination.

[0518] Specific examples of the functional group (e) in the present embodiment include, but are not limited to, hydroxyl, carboxyl, amino, amide, and functional groups containing ether bonds. From the perspective of interaction, functional groups having hydrogen bonds are preferred, and from the perspective of high hydrogen bonding properties, amide groups are more preferred, and secondary amide groups and / or tertiary amide groups are further preferred.

[0519] Examples of the compound containing the functional group (e) and its reactant include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 2-hydroxyethyl vinyl ether or 4-hydroxybutyl vinyl ether, 2-hydroxyethyl allyl ether, (meth)acrylic acid, 2-carboxyethyl (meth)acrylate, 2-dimethylaminoethyl (meth)acrylate, 2-diethylaminoethyl (meth)acrylate, 2-di-n-propylaminoethyl (meth)acrylate, 3-dimethylaminopropyl (meth)acrylate, 4-dimethylaminobutyl (meth)acrylate, N-[2-(meth)acryloyloxy]ethylmorpholine, vinylpyridine, N-vinylcarbazole, N-vinylquinoline, N-methylacrylamide, N-methylmethacrylamide, N-ethylacrylamide, N,N-dimethylacrylamide, N,N-dimethylmethacrylamide 、N,N-diethylacrylamide, N-ethylmethacrylamide, N-methyl-N-ethylacrylamide, N-methyl-N-ethylmethacrylamide, N-isopropylacrylamide, N-n-propylacrylamide, N-isopropylmethacrylamide, N-n-propylmethacrylamide, N-methyl-N-n-propylacrylamide, N-methyl-N-isopropylacrylamide, N-acryloylpyrrolidine, N-methacryloylpyrrolidine, N-acryloylpiperidine, N-methacryloylpiperidine, N-acryloylhexahydroazepine, N-acryloylmorpholine, N-methacryloylmorpholine, N-vinylpyrrolidone, N-vinylcaprolactam, N,N'-methylenebisacrylamide, N,N'-methylenebismethacrylamide, N-vinylacetamide, acetylacetoneacrylamide, acetylacetonemethacrylamide, N-methylolacrylamide, N-methylolmethacrylamide, Blemmer PE-90, PE-200, PE-350, PME-100, PME-200, PME-400, AE-350 (trade names, manufactured by Nippon Oil & Fats Co., Ltd.), MA-30, MA-50, MA-100, MA-150, RA-1120, RA-2614, RMA-564, RMA-568, RMA-1114, MPG130-MA (trade names, manufactured by Nippon Emulsifier Co., Ltd.), etc. It should be noted that in this specification, (meth)acrylate is a simple description of acrylate or methacrylate, and (meth)acrylic acid is a simple description of acrylic acid or methacrylic acid.

[0520] [Core / Shell Structure of Polymer Nanoparticles (A)]

[0521] The polymer nanoparticles (A) in this embodiment preferably have a core / shell structure having a core layer and one or more shell layers covering the core layer. From the perspective of interaction with the outermost matrix component (B) of the core / shell structure, the polymer nanoparticles (A) preferably have a functional group (e).

[0522] [Other compounds that may be contained in the polymer nanoparticles (A)]

[0523] From the aspect of improving the stability of particles by making the particles have electrostatic repulsion, the polymer nanoparticles (A) of the present embodiment can include the polymer shown below. For example, polyurethane, polyester, poly(meth)acrylate, poly(meth)acrylic acid, polyvinyl acetate, polybutadiene, polyvinyl chloride, chlorinated polypropylene, polyethylene, polystyrene polymers, or copolymers of poly(meth)acrylate-organic silicon, polystyrene-(meth)acrylate, styrene maleic anhydride can be cited.

[0524] Among the polymers that can be included in the polymer nanoparticles (A), as compounds that are particularly excellent in electrostatic repulsion, polymers or copolymers of (meth) acrylic acid and (meth) acrylic acid esters can be cited. As specific examples, polymers or copolymers of methyl acrylate, (meth) acrylic acid, methyl methacrylate, butyl methacrylate, cyclohexyl methacrylate, 2-ethylhexyl acrylate, n-butyl acrylate, 2-hydroxyethyl (meth) acrylic acid, 2-hydroxypropyl (meth) acrylic acid, 3-hydroxybutyl (meth) acrylic acid, 4-hydroxybutyl (meth) acrylic acid, 3-hydroxybutyl (meth) acrylic acid, and 4-hydroxybutyl (meth) acrylic acid can be cited but are not limited to. At this time, in order to further improve the electrostatic repulsion, part or all of the (meth) acrylic acid can be neutralized using amines such as ammonia or triethylamine, dimethylethanolamine, or salts such as NaOH and KOH.

[0525] In addition, the polymer nanoparticles (A) may contain an emulsifier. The emulsifier is not particularly limited, and examples thereof include acidic emulsifiers such as alkylbenzenesulfonic acid, alkylsulfonic acid, alkylsulfonated succinic acid, polyoxyethylene alkylsulfuric acid, polyoxyethylene alkylarylsulfuric acid, polyoxyethylene distyrylphenyl ether sulfonic acid, etc.; anionic surfactants such as alkali metal (Li, Na, K, etc.) salts of acidic emulsifiers, ammonium salts of acidic emulsifiers, and fatty acid soaps; cationic surfactants in the form of quaternary ammonium salts, pyridinium salts, and imidazolinium salts such as alkyltrimethylammonium bromide, alkylpyridinium bromide, and lauric acid imidazolinium; nonionic surfactants such as polyoxyethylene alkylaryl ether, polyoxyethylene sorbitan fatty acid ester, polyoxyethylene oxypropylene block copolymer, and polyoxyethylene distyrylphenyl ether; reactive emulsifiers having free radical polymerizable double bonds, etc.

[0526] Examples of the reactive emulsifier having a radical polymerizable double bond include, but are not limited to, Eleminol JS-2 (trade name, manufactured by Sanyo Chemical Industry Co., Ltd.), Latemul S-120, S-180A or S-180 (trade name, manufactured by Kao Corporation), Aquaron HS-10, KH-1025, RN-10, RN-20, RN30, RN50 (trade name, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), Adeka Reasoap SE1025, SR-1025, NE-20, NE-30, NE-40 (trade names, manufactured by Asahi Denka Kogyo Co., Ltd.), ammonium salts of p-styrenesulfonic acid, sodium salts of p-styrenesulfonic acid, potassium salts of p-styrenesulfonic acid, alkylsulfonic acid (meth)acrylates such as 2-sulfoethyl acrylate, methylpropanesulfonic acid (meth)acrylamide, ammonium salts of allylsulfonic acid, sodium salts of allylsulfonic acid, potassium salts of allylsulfonic acid, etc.

[0527] [Other components that may be contained in the coating film (C)]

[0528] In the coating film (C) of the present embodiment, depending on the application, as the matrix component (B), a solvent, an emulsifier, a plasticizer, a pigment, a dye, a filler, an anti-aging agent, a conductive material, an organic ultraviolet absorber, a light stabilizer, a release regulator, a softener, a surfactant, a flame retardant, an antioxidant, and a catalyst may be included. In outdoor applications, high weather resistance is required, so it is preferred to include an organic ultraviolet absorber and a light stabilizer.

[0529] Specific examples of organic ultraviolet absorbers and light stabilizers include, but are not limited to, 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-methoxybenzophenone-5-sulfonic acid, 2-hydroxy-4-n-octyloxybenzophenone, 2-hydroxy-4-n-dodecyloxybenzophenone, 2-hydroxy-4-benzyloxybenzophenone, bis(5-benzoyl-4-hydroxy-2-methoxyphenyl)methane, 2,2'-dihydroxy-4-methoxybenzophenone, 2,2'-dihydroxy-4, Benzophenone-based ultraviolet absorbers such as 4'-dimethoxybenzophenone (trade name "UVINUL3049" manufactured by BASF), 2,2',4,4'-tetrahydroxybenzophenone (trade name "UVINUL3050" manufactured by BASF), 4-dodecyloxy-2-hydroxybenzophenone, 5-benzoyl-2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxy-2'-carboxybenzophenone, 2-hydroxy-4-stearyloxybenzophenone, and 4,6-dibenzoylresorcinol;2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-(2'-hydroxy-5'-tert-butylphenyl)benzotriazole, 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)benzotriazole, 2-(2-hydroxy-5-tert-octylphenyl)benzotriazole, 2-(2-hydroxy-3,5-di-tert-octylphenyl)benzotriazole, 2-[2'-hydroxy-3',5'-bis(α,α'-dimethylbenzyl)phenyl]benzotriazole), methyl-3-[3-tert-butyl-5-(2H-phenyl)benzotriazole] 3-[(2H-benzotriazol-2-yl)-4-hydroxyphenyl]propionate and polyethylene glycol (molecular weight 300) condensate (trade name "TINUVIN1130" manufactured by BASF), isooctyl-3-[3-(2H-benzotriazol-2-yl)-5-tert-butyl-4-hydroxyphenyl]propionate (trade name "TINUVIN384" manufactured by BASF), 2-(3-dodecyl-5-methyl-2-hydroxyphenyl)benzotriazole (trade name "TINUVIN IN571”), 2-(2'-hydroxy-3'-tert-butyl-5'-methylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3',5'-di-tert-amylphenyl)benzotriazole, 2-(2'-hydroxy-4'-octyloxyphenyl)benzotriazole, 2-[2'-hydroxy-3'-(3",4",5",6"-tetrahydrophthalimidomethyl)-5'-methylphenyl]benzotriazole, 2,2-methylenebis[4-(1,1,3,3-tetramethylbutyl)-6-(2H -benzotriazole-2-yl)phenol], 2-(2H-benzotriazole-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol (trade name "TINUVIN900" manufactured by BASF), TINUVIN384-2, TINUVIN326, TINUVIN327, TINUVIN109, TINUVIN970, TINUVIN328, TINUVIN171, TINUVIN970, TINUVIN PS, TINUVIN P, TINUVIN99-2, TINUVIN928 (trade name, manufactured by BASF) and other benzotriazole-based ultraviolet absorbers;2-[4-[(2-hydroxy-3-dodecyloxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2-[4-[(2-hydroxy-3-tridecyloxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2,4-bis(2-hydroxy-4-butylhydroxyphenyl)-6-(2,4-bisbutylhydroxyphenyl)-1,3,5-triazine (manufactured by BASF Corporation) triazine-based ultraviolet absorbers such as TINUVIN 460 (trade name, manufactured by BASF), 2-(2-hydroxy-4-[1-octyloxycarbonylethoxy]phenyl)-4,6-bis(4-phenylphenyl)-1,3,5-triazine (trade name, manufactured by BASF), TINUVIN 400, TINUVIN 405, TINUVIN 477, and TINUVIN 1600 (trade name, manufactured by BASF); malonate-based ultraviolet absorbers such as HOSTAVIN PR25, HOSTAVIN B-CAP, and HOSTAVIN VSU (trade name, manufactured by Clariant); and HOSTAVIN 3206 LIQ, HOSTAVIN VSU P, and HOSTAVIN 3212 Anilide-based ultraviolet absorbers such as LIQ (trade name, manufactured by Clariant); salicylate-based ultraviolet absorbers such as amyl salicylate, menthyl salicylate, homomenthyl salicylate, octyl salicylate, phenyl salicylate, benzyl salicylate, and p-isopropylphenyl salicylate; cyanoacrylate-based ultraviolet absorbers such as ethyl 2-cyano-3,3-diphenylacrylate (trade name "UVINUL3035" manufactured by BASF), (2-ethylhexyl)-2-cyano-3,3-diphenylacrylate (trade name "UVINUL3039" manufactured by BASF), and 1,3-bis((2'-cyano-3',3'-diphenylacryloyl)oxy)-2,2-bis-(((2'-cyano-3',3'-diphenylacryloyl)oxy)methyl)propane (trade name "UVINUL3030" manufactured by BASF);2-Hydroxy-4-acryloxybenzophenone, 2-hydroxy-4-methacryloxybenzophenone, 2-hydroxy-5-acryloxybenzophenone, 2-hydroxy-5-methacryloxybenzophenone, 2-hydroxy-4-(acryloxy-ethoxy)benzophenone, 2-hydroxy-4-(methacryloxy-ethoxy)benzophenone, 2-hydroxy-4-(methacryloxy-diethoxy)benzophenone, 2-hydroxy-4-(acryloxy-triethoxy)benzophenone, 2-(2'-hydroxy-5'-methacryloxyethylphenyl)-2H-benzotriazole (products manufactured by Otsuka Chemical Co., Ltd.) Radically polymerizable ultraviolet absorbers having a radically polymerizable double bond in the molecule, such as 2-(2'-hydroxy-5'-methacryloxyethyl-3-tert-butylphenyl)-2H-benzotriazole, 2-(2'-hydroxy-5'-methacryloxypropyl-3-tert-butylphenyl)-5-chloro-2H-benzotriazole, and 3-methacryloyl-2-hydroxypropyl-3-[3'-(2"-benzotriazolyl)-4-hydroxy-5-tert-butyl]phenyl propionate (trade name "CGL-104" manufactured by Ciba-Geigy Co., Ltd. of Japan); UV-G101, UV-G 301, UV-G137, UV-G12, UV-G13 (trade names of Nippon Shokubai Co., Ltd.), and other ultraviolet-absorbing polymers; bis(2,2,6,6-tetramethyl-4-piperidinyl) succinate, bis(2,2,6,6-tetramethylpiperidinyl) sebacate, bis(1,2,2,6,6-pentamethyl-4-piperidinyl) 2-(3,5-di-tert-butyl-4-hydroxybenzyl)-2-butylmalonate, 1-[2-[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propynyloxy]ethyl]-4-[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propynyloxy]-2,2 , 6,6-tetramethylpiperidine, a mixture of bis(1,2,2,6,6-pentamethyl-4-piperidinyl) sebacate and methyl-1,2,2,6,6-pentamethyl-4-piperidinyl-sebacate (trade name "TINUVIN292" manufactured by BASF), bis(1-octyloxy-2,2,6,6-tetramethyl-4-piperidinyl) sebacate, TINUVIN123, TINUVIN144, TINUVIN152, TINUVIN249, TINUVIN292, TINUVIN5100 (trade name, manufactured by BASF) and other hindered amine light stabilizers;Free radical polymerizable hindered amine light stabilizers such as 1,2,2,6,6-pentamethyl-4-piperidinyl methacrylate, 1,2,2,6,6-pentamethyl-4-piperidinyl methacrylate, 2,2,6,6-tetramethyl-4-piperidinyl methacrylate, 2,2,6,6-tetramethyl-4-piperidinyl acrylate, 1,2,2,6,6-pentamethyl-4-iminopiperidinyl methacrylate, 2,2,6,6-tetramethyl-4-iminopiperidinyl methacrylate, 4-cyano-2,2,6,6-tetramethyl-4-piperidinyl methacrylate, 4-cyano-1,2,2,6,6-pentamethyl-4-piperidinyl methacrylate; Udouble E-133, Udouble E-135, Udouble S-2000, Udouble S-2834, Udouble S-2840, Udouble S-2818, Udouble S-2860 (trade name, manufactured by Nippon Shokubai Co., Ltd.) and other light-stable polymers; ultraviolet absorbers reactive with silanol groups, isocyanate groups, epoxy groups, semicarbazide groups, hydrazide groups, etc., and one or more of them can be used in combination. ;

[0530] [Transparency of hard coating film]

[0531] When the hard coating film of the present embodiment is used as a transparent material, it is preferred to have a transparency that does not adversely affect the appearance of the material or the visibility through the material. From the perspective of changes in appearance, the transparency of the hard coating film can be evaluated by the total light transmittance maintenance rate obtained by the following formula. In the present embodiment, the total light transmittance maintenance rate of the hard coating film is preferably 90% or more, more preferably 95% or more from the perspective of ensuring lighting, and particularly preferably 98% or more from the perspective of ensuring visibility through the material. For example, by adopting the above-mentioned preferred method as polymer nanoparticles (A) and matrix components (B), the total light transmittance maintenance rate of the hard coating film can be adjusted to the above-mentioned range.

[0532] Total light transmittance maintenance rate of hard coating film (%) = (total light transmittance of substrate with hard coating film (%) / total light transmittance of substrate (%)) × 100

[0533] [Fouling resistance of hard coating film]

[0534] When the hard coating film of the present embodiment is used as a transparent material, it is required that the visibility after long-term use is not adversely affected. That is, in the above-mentioned use, it is preferred that the hard coating film has good pollution resistance. The pollution resistance here refers to the degree of adhesion of coal dust after long-term use. For example, JIS test powder 1 (12 types of carbon black) can be attached to the coating film after the abrasion test, and the total light transmittance maintenance rate after the test obtained by the following formula can be evaluated.

[0535] Total light transmittance maintenance rate after carbon black test (%) = (total light transmittance after test / total light transmittance before test) × 100

[0536] The higher the total light transmittance maintenance rate after the carbon black test, the less carbon black is attached after long-term use, and there is a tendency for the stain resistance to be excellent.

[0537] [Moisture resistance of hard coating film]

[0538] In applications where the hard coating film of the present embodiment is used for a long period of time, it is required to maintain the performance of the hard coating film under the use environment. For example, in the application of automotive window materials, it is assumed that it will be used under high temperature and high humidity, so it is preferred that the appearance and adhesion do not change after exposure to 50°C and 95% RH for 2 weeks in accordance with JIS-R3211 and R3222.

[0539] <Substrate with hard coating>

[0540] The substrate with a hard coating film of the present embodiment includes a substrate and the hard coating film of the present embodiment formed on one side and / or both sides of the substrate. The substrate with a hard coating film has a hard coating film on at least one side and / or both sides of the substrate.

[0541] The substrate with a hard coating film of the present embodiment has high wear resistance, durability and weather resistance due to the above-mentioned structure. The substrate with a hard coating film of the present embodiment can show high levels of wear resistance, durability and weather resistance, and is therefore useful as a hard film for, for example, but not limited to, building materials, automobile parts, electronic equipment, motor products, etc., and is particularly preferably used for automobile parts.

[0542] [Base material]

[0543] The substrate for coating the hard coating film of the present embodiment is not particularly limited, and resin, metal, glass, etc. can be cited. As the shape of the substrate, for example, a plate-like shape, a shape including concave and convex shapes, a shape including a curved surface, a hollow shape, a porous body shape, a combination thereof, etc. can be cited, but not limited to. In addition, regardless of the type of substrate, for example, sheets, films, fibers, etc. can be cited. Among them, from the aspects of imparting hard coating properties and formability, resin is preferred. That is, the structure having a substrate containing a resin and a hard coating film of the present embodiment has excellent wear resistance, formability, and stain resistance. The resin used as the substrate can be cited, but not limited to, for example, thermoplastic resins and thermosetting resins. The thermoplastic resin used as the substrate can be cited, but not limited to, for example, polyethylene, polypropylene, polystyrene, ABS resin, vinyl chloride resin, methyl methacrylate resin, nylon, fluororesin, polycarbonate, polyester resin, etc. In addition, examples of thermosetting resins used as the substrate include, but are not limited to, phenol resins, urea resins, melamine resins, unsaturated polyester resins, epoxy resins, silicone resins, silicone rubbers, SB rubbers, natural rubbers, thermosetting elastomers, and the like.

[0544] [Adhesive layer]

[0545] The substrate with hard coating film of the present embodiment may further have an adhesive layer between the substrate and the hard coating film. As the adhesive layer, a commonly used adhesive layer can be used, without particular limitation, for example, thermoplastic resins, thermosetting resins, rubber-elastomers, etc., among which acrylic resins, acrylic urethane resins, urethane resins, silicone resins, etc. are preferred. In addition, the above-mentioned adhesive layer may contain any appropriate additives as required. As additives, for example, crosslinking agents, tackifiers, plasticizers, pigments, dyes, fillers, anti-aging agents, conductive materials, ultraviolet absorbers, inorganic oxides, light stabilizers, peeling regulators, softeners, surfactants, flame retardants, antioxidants, etc. may be cited but are not limited to. Examples of crosslinking agents include, but are not limited to, isocyanate crosslinking agents, epoxy crosslinking agents, carbodiimide crosslinking agents, oxazoline crosslinking agents, aziridine crosslinking agents, amine crosslinking agents, peroxide crosslinking agents, melamine crosslinking agents, urea crosslinking agents, metal alkoxide crosslinking agents, metal chelate crosslinking agents, and metal salt crosslinking agents.

[0546] [Adhesive emulsion particles (F)]

[0547] In the present embodiment, the above-mentioned adhesive layer preferably includes adhesive latex particles (F). The adhesive latex particles (F) play a role in imparting flexibility and improving adhesion to the substrate. The adhesive latex particles (F) are not particularly limited, and are, for example, particles composed of polycarbonyl compounds such as polyurethane, polyester, poly(meth)acrylate, polyvinyl acetate, polybutadiene, polyvinyl chloride, chlorinated polypropylene, polyethylene, polystyrene, polystyrene-(meth)acrylate copolymers, rosin derivatives, alcohol adducts of styrene-maleic anhydride copolymers, cellulose resins, silicone compounds, etc. In the present embodiment, the adhesive latex particles (F) are preferably poly(meth)acrylate.

[0548] The preparation method of the adhesive latex particles (F) in the present embodiment is not particularly limited, and preferably a structure obtained by polymerizing a vinyl monomer in the presence of water and an emulsifier. When the adhesive latex particles (F) obtained in this way are included in the adhesive layer, there is a tendency to maintain better adhesion to the substrate.

[0549] The vinyl monomer is not particularly limited, and examples thereof include (meth)acrylates, aromatic vinyl compounds, cyanide vinyl compounds, and monomers containing functional groups such as carboxyl group-containing vinyl monomers, hydroxyl group-containing vinyl monomers, epoxy group-containing vinyl monomers, carbonyl group-containing vinyl monomers, and vinyl monomers having secondary amide groups and / or tertiary amide groups.

[0550] The (meth)acrylate is not particularly limited, and examples thereof include alkyl (meth)acrylates having 1 to 50 carbon atoms in the alkyl portion and (poly)oxyethylene di(meth)acrylates having 1 to 100 oxyethylene groups.

[0551] The alkyl (meth)acrylate is not particularly limited, and examples thereof include methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, methylcyclohexyl (meth)acrylate, cyclohexyl (meth)acrylate, lauryl (meth)acrylate, and dodecyl (meth)acrylate.

[0552] The (poly)oxyethylene di(meth)acrylate is not particularly limited, and examples thereof include ethylene glycol dimethacrylate, diethylene glycol di(meth)acrylate, methoxydiethylene glycol (meth)acrylate, and tetraethylene glycol di(meth)acrylate.

[0553] The aromatic vinyl compound is not particularly limited, and examples thereof include styrene and 4-vinyltoluene.

[0554] The vinyl cyanide compound is not particularly limited, and examples thereof include acrylonitrile and methacrylonitrile.

[0555] There is no particular limitation on the carboxyl-containing vinyl monomer, and for example, (methyl) acrylic acid, crotonic acid, itaconic acid, maleic acid, fumaric acid, maleic anhydride, or half fats of dibasic acids such as itaconic acid, maleic acid, and fumaric acid can be cited. When using a carboxyl-containing vinyl monomer, a carboxyl group can be introduced into the adhesive emulsion particles (F) in the present embodiment, and the stability of the emulsion can be improved by providing electrostatic repulsion between the particles, and there is a tendency to improve resistance to external dispersion destruction such as agglomeration during stirring. At this time, from the perspective of further improving the electrostatic repulsion, a part or all of the above-mentioned introduced carboxyl groups can also be neutralized with amines such as ammonia or triethylamine, dimethylethanolamine, or bases such as NaOH and KOH.

[0556] The hydroxyl group-containing vinyl monomer is not particularly limited, and examples thereof include hydroxyalkyl (meth)acrylic acid esters such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate; hydroxyalkyl fumarate such as di-2-hydroxyethyl fumarate and mono-2-hydroxyethyl monobutyl fumarate; allyl alcohol, (poly)oxyethylene mono(meth)acrylate having 1 to 100 oxyethylene groups; (poly)oxypropylene mono(meth)acrylate having 1 to 100 oxypropylene groups; and "PRAXCELL FM, FA Monomer" (trade name of caprolactone addition monomer manufactured by Daicel Chemical Co., Ltd.), and other hydroxyalkyl esters of α,β-ethylenically unsaturated carboxylic acids.

[0557] The (poly)oxyethylene (meth)acrylate is not particularly limited, and examples thereof include ethylene glycol (meth)acrylate, ethylene glycol methoxy (meth)acrylate, diethylene glycol (meth)acrylate, diethylene glycol methoxy (meth)acrylate, tetraethylene glycol (meth)acrylate, and tetraethylene glycol methoxy (meth)acrylate.

[0558] The (poly)oxypropylene (meth)acrylate is not particularly limited, and examples thereof include propylene glycol (meth)acrylate, propylene glycol methoxy (meth)acrylate, dipropylene glycol (meth)acrylate, dipropylene glycol methoxy (meth)acrylate, tetrapropylene glycol (meth)acrylate, and tetrapropylene glycol methoxy (meth)acrylate.

[0559] The epoxy group-containing vinyl monomer is not particularly limited, and examples thereof include glycidyl group-containing vinyl monomers, etc. The glycidyl group-containing vinyl monomer is not particularly limited, and examples thereof include glycidyl (meth)acrylate, allyl glycidyl ether, and allyl dimethyl glycidyl ether.

[0560] The carbonyl group-containing vinyl monomer is not particularly limited, and examples thereof include acetylacetone acrylamide and the like.

[0561] Specific examples of vinyl monomers other than the above are not particularly limited, and examples thereof include olefins such as ethylene, propylene, and isobutylene, dienes such as butadiene, halogenated olefins such as vinyl chloride, vinylidene chloride, vinyl fluoride, tetrafluoroethylene, and chlorotrifluoroethylene, vinyl acetate, vinyl propionate, vinyl n-butyrate, vinyl benzoate, vinyl p-tert-butylbenzoate, vinyl pivalate, vinyl 2-ethylhexanoate, vinyl versatate, and vinyl laurate, carboxylic acid vinyl esters such as isopropenyl acetate and isopropenyl propionate, ethyl vinyl ether, isobutylene, and the like. Vinyl ethers such as allyl vinyl ether, cyclohexyl vinyl ether, allyl esters such as allyl acetate and allyl benzoate, allyl ethers such as allyl ethyl ether and allyl phenyl ether, and 4-(meth)acryloyloxy-2,2,6,6-tetramethylpiperidine, 4-(meth)acryloyloxy-1,2,2,6,6-pentamethylpiperidine, perfluoromethyl (meth)acrylate, perfluoropropyl (meth)acrylate, perfluoropropyl methyl (meth)acrylate, vinyl pyrrolidone, trimethylolpropane tri(meth)acrylate, allyl (meth)acrylate, etc., or a combination thereof.

[0562] The vinyl monomer having a secondary amide group and / or a tertiary amide group is not particularly limited, and examples thereof include N-alkyl or N-alkylene-substituted (meth)acrylamide, etc. Specifically, examples thereof include N-methylacrylamide, N-methylmethacrylamide, N-ethylacrylamide, N,N-dimethylacrylamide, N,N-dimethylmethacrylamide, N,N-diethylacrylamide, N-ethylmethacrylamide, N-methyl-N-ethylacrylamide, N-methyl-N-ethylmethacrylamide, N-isopropylacrylamide, N-n-propylacrylamide, N-isopropylmethacrylamide, N-n-propylmethacrylamide, N-methyl-N-n-propylacrylamide, N-methyl N-acryloyl-N-isopropylacrylamide, N-acryloylpyrrolidine, N-methacryloylpyrrolidine, N-acryloylpiperidine, N-methacryloylpiperidine, N-acryloylhexahydroazepine, N-acryloylmorpholine, N-methacryloylmorpholine, N-vinylpyrrolidone, N-vinylcaprolactam, N,N'-methylenebisacrylamide, N,N'-methylenebismethacrylamide, N-vinylacetamide, acetylacetoneacrylamide, acetylacetonemethacrylamide, N-methylolacrylamide, N-methylolmethacrylamide, etc.

[0563] The silicone compound is not particularly limited, and examples thereof include trimethoxysilane, triethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, cyclohexyltrimethoxysilane, cyclohexyltriethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, dimethoxysilane, diethoxysilane, methyldimethoxysilane, methyldiethoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane, dimethoxydiphenylsilane, diethoxydiphenylsilane, 3-propylene Hydrolysis condensates of acyloxypropyltrimethoxysilane, 3-acryloxypropyltriethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, p-phenylvinyltrimethoxysilane, p-phenylvinyltriethoxysilane, tetramethoxysilane, tetraethoxysilane, and the like.

[0564] The adhesive latex particles (F) may contain an emulsifier. The emulsifier is not particularly limited, and examples thereof include acidic emulsifiers such as alkylbenzenesulfonic acid, alkylsulfonic acid, alkylsulfonated succinic acid, polyoxyethylene alkylsulfuric acid, polyoxyethylene alkylarylsulfuric acid, polyoxyethylene distyrylphenyl ether sulfonic acid, etc.; anionic surfactants such as alkali metal (Li, Na, K, etc.) salts of acidic emulsifiers, ammonium salts of acidic emulsifiers, fatty acid soaps, etc.; cationic surfactants in the form of quaternary ammonium salts, pyridinium salts, and imidazolinium salts such as alkyltrimethylammonium bromide, alkylpyridinium bromide, and imidazolinium laurate; nonionic surfactants such as polyoxyethylene alkylaryl ether, polyoxyethylene sorbitan fatty acid ester, polyoxyethyleneoxypropylene block copolymer, and polyoxyethylene distyrylphenyl ether; reactive emulsifiers having free radical polymerizable double bonds, etc.

[0565] Examples of the reactive emulsifier having a radical polymerizable double bond include, but are not limited to, Eleminol JS-2 (trade name, manufactured by Sanyo Chemical Industry Co., Ltd.), Latemul S-120, S-180A or S-180 (trade name, manufactured by Kao Corporation), Aquaron HS-10, KH-1025, RN-10, RN-20, RN30, RN50 (trade name, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), Adeka Reasoap SE1025, SR-1025, NE-20, NE-30, NE-40 (trade names, manufactured by Asahi Denka Kogyo Co., Ltd.), ammonium salts of p-styrenesulfonic acid, sodium salts of p-styrenesulfonic acid, potassium salts of p-styrenesulfonic acid, alkylsulfonic acid (meth)acrylates such as 2-sulfoethyl acrylate, methylpropanesulfonic acid (meth)acrylamide, ammonium salts of allylsulfonic acid, sodium salts of allylsulfonic acid, potassium salts of allylsulfonic acid, etc.

[0566] [Average particle size of adhesive emulsion particles (F)]

[0567] The average particle size of the adhesive emulsion particles (F) in the present embodiment is obtained by observing the particle size by cross-sectional SEM or dynamic light scattering. The average particle size of the adhesive emulsion particles (F) is preferably less than 300 nm. By adjusting the average particle size of the adhesive emulsion particles (F) to the above range, there is a tendency to form a coating film with better adhesion by increasing the contact area with the substrate. In addition, from the perspective of improving the transparency of the obtained coating film, the average particle size is more preferably less than 200 nm. Regarding the method for measuring the average particle size of the adhesive emulsion particles (F), for example, the cumulative particle size can be measured using a dynamic light scattering particle size distribution measuring device (model: ELSZ-1000) manufactured by Otsuka Electronics Co., Ltd. using an aqueous dispersion of adhesive emulsion particles (F), but it is not limited to this.

[0568] [Inorganic oxide (G)]

[0569] From the viewpoint of improving adhesion due to interaction with the hard coating film, the adhesive layer preferably further contains an inorganic oxide (G).

[0570] Specific examples of the inorganic oxide (G) in this embodiment include, but are not limited to, oxides of silicon, aluminum, titanium, zirconium, zinc, cerium, tin, indium, gallium, germanium, antimony, molybdenum, etc. They may be a single substance or a mixture. Among the above substances, the inorganic oxide (G) is preferably silicon oxide particles.

[0571] The average particle size of the inorganic oxide (G) in the present embodiment is preferably 2 nm or more from the perspective of good storage stability of the raw material composition of the adhesive layer, and is preferably 150 nm or less from the perspective of good transparency of the entire substrate with a hard coating film. Therefore, the average particle size is preferably 2 nm or more and 100 nm or less, and more preferably 2 nm or more and 50 nm or less.

[0572] Silicon oxide particles represented by dry silica and colloidal silica are preferred but not particularly limited from the viewpoint of strong interaction with the hydrolyzable silicon compound (b) and adhesion to the hard coating film. Colloidal silica is preferred because it can be used in the form of an aqueous dispersion.

[0573] [Colloidal Silica Suitable for Use as Inorganic Oxide (G)]

[0574] The acidic colloidal silica using water as a dispersion solvent suitable for use in the present embodiment is not particularly limited, and can be prepared by a sol-gel method or a commercially available product. When prepared by a sol-gel method, reference can be made to Werner Stober et al; J. Colloid and Interface Sci., 26, 62-69 (1968), Rickey D. Badley et al; Lang muir 6, 792-801 (1990), Journal of the Color Society, 61 [9] 488-493 (1988), etc.

[0575] When commercially available products are used, for example, Snowtex-O, Snowtex-OS, Snowtex-OXS, Snowtex-O-40, Snowtex-OL, Snowtex OYL, Snowtex-OUP, Snowtex-PS-SO, Snowtex-PS-MO, Snowtex-AK-XS, Snowtex-AK, Snowtex-AK-L, Snowtex-AK-YL, Snowtex-AK-PS-S (trade names, manufactured by Nissan Chemical Industries, Ltd.), Adelite AT-20Q (trade name, manufactured by Asahi Denka Industries, Ltd.), Klebosol 20H12, Klebosol 30CAL25 (trade names, manufactured by Clariant (Japan) Ltd.), etc. may be mentioned.

[0576] In addition, the alkaline colloidal silica includes silica stabilized by the addition of alkali metal ions, ammonium ions, or amines, and examples thereof include, but are not particularly limited to, Snowtex-20, Snowtex-30, Snowtex-XS, Snowtex-50, Snowtex-30L, Snowtex-XL, Snowtex-YL, Snowtex ZL, Snowtex-UP, Snowtex-ST-PS-S, Snowtex ST-PS-M, Snowtex-C, Snowtex-CXS, Snowtex-CM, Snowtex-N, Snowtex-NXS, Snowtex-NS, and Snowtex-N-40 (trade names, manufactured by Nissan Chemical Industries, Ltd.), Adelite AT-20, Adelite AT-30, Adelite AT-20N, Adelite AT-30N, Adelite AT-20A, Adelite AT-30A, and Adelite AT-40, Adelite AT-50 (trade names, manufactured by Asahi Electric Industries, Ltd.), Klebosol 30R9, Klebosol 30R50, Klebosol 50R50 (trade names, manufactured by Clariant (Japan) Ltd.), Ludox HS-40, Ludox HS-30, Ludox LS, Ludox AS-30, Ludox SM-AS, Ludox AM, Ludox HSA and Ludox SM (trade names, manufactured by DuPont), etc.

[0577] In addition, there is no particular limitation on the colloidal silica using a water-soluble solvent as a dispersion medium, and examples thereof include MA-ST-M (methanol dispersion type with a particle size of 20 to 25 nm), IPA-ST (isopropanol dispersion type with a particle size of 10 to 15 nm), EG-ST (ethylene glycol dispersion type with a particle size of 10 to 15 nm), EGST-ZL (ethylene glycol dispersion type with a particle size of 70 to 100 nm), NPC-ST (ethylene glycol monopropyl ether dispersion type with a particle size of 10 to 15 nm), and TOL-ST (toluene dispersion type with a particle size of 10 to 15 nm) manufactured by Nissan Chemical Industries, Ltd.

[0578] The dry silica particles are not particularly limited, and examples thereof include AEROSIL manufactured by NIPPONAEROSIL Co., Ltd. and REOLOSIL manufactured by Tokuyama Co., Ltd.

[0579] The silicon oxide particles may contain an inorganic base (sodium hydroxide, potassium hydroxide, lithium hydroxide, ammonia, etc.) or an organic base (tetramethylammonium, triethylamine, etc.) as a stabilizer.

[0580] [Shape of Inorganic Oxide (G)]

[0581] In addition, the shape of the inorganic oxide (G) in this embodiment can be, but is not limited to, spherical, square, polyhedral, elliptical, flat, linear, beaded, pearly, etc. From the perspective of the hardness, transparency, and adhesion of the hard coating film, spherical, pearly, and beaded shapes are particularly preferred.

[0582] From the viewpoint of adhesion, the thickness of the adhesive layer is preferably from 0.1 μm to 100.0 μm, and more preferably from 0.3 μm to 50.0 μm.

[0583] The coating film (C) may further have a functional layer on at least one surface thereof. Examples of the functional layer include, but are not limited to, an antireflection layer, an antifouling layer, a polarizing layer, and an impact absorbing layer.

[0584] In the substrate with a hard coating film, the surface may be subjected to silicon oxidation processing to form a silicon oxide layer from the viewpoint of weather resistance. The method for forming the silicon oxide layer is as follows.

[0585] [Components that may be contained in the adhesive layer]

[0586] The adhesive layer of the present embodiment can include solvents, emulsifiers, plasticizers, pigments, dyes, fillers, anti-aging agents, conductive materials, ultraviolet absorbers, light stabilizers, peeling regulators, softeners, surfactants, flame retardants, antioxidants, and catalysts according to the purpose. Especially in outdoor use, high weather resistance is required, so it is preferred to include ultraviolet absorbers and light stabilizers. Specifically, it can include but is not limited to 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-methoxybenzophenone-5-sulfonic acid, 2-hydroxy-4-n-octyloxybenzophenone, 2-hydroxy-4-n-dodecyloxybenzophenone, 2-hydroxy-4-benzyloxybenzophenone, bis(5-benzoyl-4-hydroxy-2-methoxyphenyl)methane, 2,2'-dihydroxy-4-methoxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone Benzophenone-based ultraviolet absorbers such as benzophenone (trade name "UVINUL3049" manufactured by BASF), 2,2',4,4'-tetrahydroxybenzophenone (trade name "UVINUL3050" manufactured by BASF), 4-dodecyloxy-2-hydroxybenzophenone, 5-benzoyl-2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxy-2'-carboxybenzophenone, 2-hydroxy-4-stearyloxybenzophenone, and 4,6-dibenzoylresorcinol;2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-(2'-hydroxy-5'-tert-butylphenyl)benzotriazole, 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)benzotriazole, 2-(2-hydroxy-5-tert-octylphenyl)benzotriazole, 2-(2-hydroxy-3,5-di-tert-octylphenyl)benzotriazole, 2-[2'-hydroxy-3',5'-bis(α,α'-dimethylbenzyl)phenyl]benzotriazole), methyl-3-[3-tert-butyl-5-(2H-phenyl)benzotriazole] 3-[(2H-benzotriazol-2-yl)-4-hydroxyphenyl]propionate and polyethylene glycol (molecular weight 300) condensate (trade name "TINUVIN1130" manufactured by BASF), isooctyl-3-[3-(2H-benzotriazol-2-yl)-5-tert-butyl-4-hydroxyphenyl]propionate (trade name "TINUVIN384" manufactured by BASF), 2-(3-dodecyl-5-methyl-2-hydroxyphenyl)benzotriazole (trade name "TINUVIN IN571”), 2-(2'-hydroxy-3'-tert-butyl-5'-methylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3',5'-di-tert-amylphenyl)benzotriazole, 2-(2'-hydroxy-4'-octyloxyphenyl)benzotriazole, 2-[2'-hydroxy-3'-(3",4",5",6"-tetrahydrophthalimidomethyl)-5'-methylphenyl]benzotriazole, 2,2-methylenebis[4-(1,1,3,3-tetramethylbutyl)-6-(2H -benzotriazole-2-yl)phenol], 2-(2H-benzotriazole-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol (trade name "TINUVIN900" manufactured by BASF), TINUVIN384-2, TINUVIN326, TINUVIN327, TINUVIN109, TINUVIN970, TINUVIN328, TINUVIN171, TINUVIN970, TINUVIN PS, TINUVIN P, TINUVIN99-2, TINUVIN928 (trade name, manufactured by BASF) and other benzotriazole-based ultraviolet absorbers;2-[4-[(2-hydroxy-3-dodecyloxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2-[4-[(2-hydroxy-3-tridecyloxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2,4-bis(2-hydroxy-4-butylhydroxyphenyl)-6-(2,4-bisbutylhydroxyphenyl)-1,3,5-triazine (manufactured by BASF Corporation) triazine-based ultraviolet absorbers such as TINUVIN 460 (trade name, manufactured by BASF), 2-(2-hydroxy-4-[1-octyloxycarbonylethoxy]phenyl)-4,6-bis(4-phenylphenyl)-1,3,5-triazine (trade name, manufactured by BASF), TINUVIN 400, TINUVIN 405, TINUVIN 477, and TINUVIN 1600 (trade name, manufactured by BASF); malonate-based ultraviolet absorbers such as HOSTAVIN PR25, HOSTAVIN B-CAP, and HOSTAVIN VSU (trade name, manufactured by Clariant); and HOSTAVIN 3206 LIQ, HOSTAVIN VSU P, and HOSTAVIN 3212 Anilide-based ultraviolet absorbers such as LIQ (trade name, manufactured by Clariant); salicylate-based ultraviolet absorbers such as amyl salicylate, menthyl salicylate, homomenthyl salicylate, octyl salicylate, phenyl salicylate, benzyl salicylate, and p-isopropylphenyl salicylate; cyanoacrylate-based ultraviolet absorbers such as ethyl 2-cyano-3,3-diphenylacrylate (trade name "UVINUL3035" manufactured by BASF), (2-ethylhexyl)-2-cyano-3,3-diphenylacrylate (trade name "UVINUL3039" manufactured by BASF), and 1,3-bis((2'-cyano-3',3'-diphenylacryloyl)oxy)-2,2-bis-(((2'-cyano-3',3'-diphenylacryloyl)oxy)methyl)propane (trade name "UVINUL3030" manufactured by BASF);2-Hydroxy-4-acryloxybenzophenone, 2-hydroxy-4-methacryloxybenzophenone, 2-hydroxy-5-acryloxybenzophenone, 2-hydroxy-5-methacryloxybenzophenone, 2-hydroxy-4-(acryloxy-ethoxy)benzophenone, 2-hydroxy-4-(methacryloxy-ethoxy)benzophenone, 2-hydroxy-4-(methacryloxy-diethoxy)benzophenone, 2-hydroxy-4-(acryloxy-triethoxy)benzophenone, 2-(2'-hydroxy-5'-methacryloxyethylphenyl)-2H-benzotriazole (products manufactured by Otsuka Chemical Co., Ltd.) Radically polymerizable ultraviolet absorbers having a radically polymerizable double bond in the molecule, such as 2-(2'-hydroxy-5'-methacryloxyethyl-3-tert-butylphenyl)-2H-benzotriazole, 2-(2'-hydroxy-5'-methacryloxypropyl-3-tert-butylphenyl)-5-chloro-2H-benzotriazole, and 3-methacryloyl-2-hydroxypropyl-3-[3'-(2"-benzotriazolyl)-4-hydroxy-5-tert-butyl]phenyl propionate (trade name "CGL-104" manufactured by Ciba-Geigy Co., Ltd. of Japan); UV-G101, UV-G 301, UV-G137, UV-G12, UV-G13 (trade names of Nippon Shokubai Co., Ltd.), and other ultraviolet-absorbing polymers; bis(2,2,6,6-tetramethyl-4-piperidinyl) succinate, bis(2,2,6,6-tetramethylpiperidinyl) sebacate, bis(1,2,2,6,6-pentamethyl-4-piperidinyl) 2-(3,5-di-tert-butyl-4-hydroxybenzyl)-2-butylmalonate, 1-[2-[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propynyloxy]ethyl]-4-[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propynyloxy]-2,2 , 6,6-tetramethylpiperidine, a mixture of bis(1,2,2,6,6-pentamethyl-4-piperidinyl) sebacate and methyl-1,2,2,6,6-pentamethyl-4-piperidinyl-sebacate (trade name "TINUVIN292" manufactured by BASF), bis(1-octyloxy-2,2,6,6-tetramethyl-4-piperidinyl) sebacate, TINUVIN123, TINUVIN144, TINUVIN152, TINUVIN249, TINUVIN292, TINUVIN5100 (trade name, manufactured by BASF) and other hindered amine light stabilizers;Free radical polymerizable hindered amine light stabilizers such as 1,2,2,6,6-pentamethyl-4-piperidinyl methacrylate, 1,2,2,6,6-pentamethyl-4-piperidinyl methacrylate, 2,2,6,6-tetramethyl-4-piperidinyl methacrylate, 2,2,6,6-tetramethyl-4-piperidinyl acrylate, 1,2,2,6,6-pentamethyl-4-iminopiperidinyl methacrylate, 2,2,6,6-tetramethyl-4-iminopiperidinyl methacrylate, 4-cyano-2,2,6,6-tetramethyl-4-piperidinyl methacrylate, 4-cyano-1,2,2,6,6-pentamethyl-4-piperidinyl methacrylate; Udouble E-133, Udouble E-135, Udouble S-2000, Udouble S-2834, Udouble S-2840, Udouble S-2818, Udouble S-2860 (trade name, manufactured by Nippon Shokubai Co., Ltd.) and other light-stable polymers; UV absorbers reactive with silanol groups, isocyanate groups, epoxy groups, semicarbazide groups, and hydrazide groups; inorganic UV absorbers such as cerium oxide, niobium oxide, aluminum oxide, zinc oxide, titanium oxide, zirconium oxide, antimony oxide, magnesium oxide, tin oxide, bismuth oxide, cobalt oxide, and copper oxide, etc., and one of them or two or more thereof can be used in combination. ;

[0587] <Coating composition>

[0588] The coating film (C) of the present embodiment is obtained, for example, by using the following coating composition (I). The coating composition (I) is a coating composition comprising polymer nanoparticles (A) and a matrix raw material component (B'), wherein the elastic recovery rate η of the polymer nanoparticles (A) measured by an indentation test according to ISO14577-1 is ITA The Martens hardness HM of the polymer nanoparticles (A) is 0.30 or more and 0.90 or less. A The Martens hardness HM of the matrix raw material component (B') B’ Meet HM B’ / HM A >1, the matrix raw material component (B') comprises an inorganic oxide (D), and the inorganic oxide (D) contains at least one inorganic component selected from the group consisting of Ce, Nb, Al, Zn, Ti, Zr, Sb, Mg, Sn, Bi, Co and Cu. Due to such a configuration, the coating composition (I) exhibits high wear resistance, durability and weather resistance.

[0589] [Hardness of polymer nanoparticles (A) HM A Hardness HM of the matrix raw material component (B') B ]

[0590] In the coating composition (I), the Martens hardness HM of the polymer nanoparticles (A) is A Martens hardness HM of the matrix raw material component (B') B’ The following relationship (3) is satisfied.

[0591] HM B’ / HM A >1 Formula (3)

[0592] As described above, in the coating composition (I), since the above relationship is satisfied, in the coating film (C) obtained by using the coating composition (I), the Martens hardness HM of the polymer nanoparticles (A) is A Martens hardness HM of the matrix raw material component (B') B’ The Martens hardness of each component in the coating composition (I) can be separated into polymer nanoparticles (A) and matrix raw material component (B') by centrifugation, ultrafiltration or the like, and the separated components can be measured by the method described in the examples described below.

[0593] The above HM A and H.M. B The values ​​of can be adjusted to the above-mentioned magnitude relationship by adjusting the structures and composition ratios of the constituent components of the polymer nanoparticles (A) and the matrix raw material component (B'), and the method is not particularly limited.

[0594] [Elastic recovery rate η of polymer nanoparticles (A) ITA ]

[0595] The elastic recovery rate η of the polymer nanoparticles (A) in this embodiment is ITA The coating film of the polymer nanoparticles (A) after film formation is used as W in ISO14577-1. elast / W total The ratio η IT The parameters recorded are measured and obtained by measuring the total mechanical work W of the depression. total The amount of work done by the elastic recovery deformation of the concave elast Elastic recovery rate η ITA The higher the elastic recovery rate, the more the coating film can recover to its original state when it is impacted, and the higher the self-repair ability against impact. From the perspective of effectively exerting the self-repair ability, the elastic recovery rate η of the polymer nanoparticles (A) ITA Under the measurement conditions (Vickers quadrangular pyramid diamond indenter, load increase condition 2mN / 20sec, load decrease condition 2mN / 20sec), η is preferably 0.30 or more, from the perspective of being able to follow the deformation of the substrate or matrix raw material component (B') when the coating is formed, ITAIt is preferably 0.90 or less. The elastic recovery rate η of the polymer nanoparticles (A) ITA More preferably, it is 0.50 or more, and even more preferably, it is 0.60 or more. The elastic recovery rate of the polymer nanoparticles (A) can be determined by, but not limited to, the following methods: separating the polymer nanoparticles (A) and the matrix raw material component (B') by centrifugal separation, ultrafiltration, etc., dispersing the separated polymer nanoparticles (A) in a solvent to obtain a composition, applying the composition and drying it, and measuring the film after film formation using a micro hardness meter Fischerscope (HM2000S manufactured by Fischer Instruments), an ultra-micro indentation hardness tester (ENT-NEXUS manufactured by Elionix Co., Ltd.), a nanoindenter (iNano, G200 manufactured by Toyo Technica), a nanoindentation system (TI980 manufactured by Bruker), etc. As a method for measuring the elastic recovery rate η ITA The method of adjusting the content within the above range includes, but is not limited to, adjusting the structure and composition ratio of the components of the polymer nanoparticles (A).

[0596] It should be noted that the coating film (C) can be obtained in the form of a cured product obtained by curing the coating composition (I) by hydrolysis condensation or the like. The composition of the polymer nanoparticles (A) generally does not change during the curing process. Therefore, the elastic recovery rate η of the polymer nanoparticles (A) in the coating composition (I) measured by the method described in the examples described later is ITA The value of is related to the elastic recovery rate η of the polymer nanoparticles (A) in the coating film (C) ITA The elastic recovery rate η in the coating film (C) can be determined in this form. ITA The value of .

[0597] [Solvent (H)]

[0598] The coating composition (I) in this embodiment preferably contains a solvent (H). The solvent (H) that can be used is not particularly limited, and a common solvent can be used. Examples of the solvent include, but are not limited to, water; ethylene glycol, butyl cellosolve, isopropyl alcohol, n-butanol, 2-butanol, ethanol, methanol, modified ethanol, 2-methoxy-1-propanol, 1-methoxy-2-propanol, diacetone alcohol, glycerol, monoalkyl monoglycerol ether, propylene glycol monomethyl ether, diethylene glycol monobutyl ether, propylene glycol monoethyl ether, propylene glycol monobutyl ether, dipropylene glycol monoethyl ether, dipropylene glycol monobutyl ether, diethylene glycol monophenyl ether, tetraethylene glycol monophenyl ether, etc. Alcohols; aromatic hydrocarbons such as toluene and xylene; aliphatic hydrocarbons such as hexane, cyclohexane, and heptane; esters such as ethyl acetate and n-butyl acetate; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; ethers such as tetrahydrofuran and dioxane; amides such as dimethylacetamide and dimethylformamide; halides such as chloroform, dichloromethane, and carbon tetrachloride; dimethyl sulfoxide and nitrobenzene; etc., and one of them or two or more thereof can be used in combination. Among them, from the perspective of reducing the environmental load when removing the solvent, solvents containing water and alcohols are particularly preferred.

[0599] The constituent components, size, composition ratio, etc. of the polymer nanoparticles (A) contained in the coating composition (I) are described below. The details of aspects not mentioned below are the same as the above description of the polymer nanoparticles (A) contained in the coating film (C).

[0600] In addition, the matrix raw material component (B') contained in the coating composition (I) is cured by hydrolysis condensation or the like in the process of obtaining the coating film (C). That is, the matrix raw material component (B') contained in the coating composition (I) has a relationship of forming a corresponding matrix component (B) in the obtained coating film (C). The constituent components, size, composition ratio, etc. of the matrix raw material component (B') are also described below, and the details of the aspects not mentioned below are the same as the above description of the matrix component (B) contained in the coating film (C).

[0601] In the coating composition (I), the polymer nanoparticles (A) preferably contain the above-mentioned hydrolyzable silicon compound (a), and the matrix raw material component (B') contains the above-mentioned hydrolyzable silicon compound (b). In addition, as the hydrolyzable silicon compound (a) in the coating composition (I), it is also preferred to contain one or more selected from the compounds containing the atomic group represented by the above-mentioned formula (a-1), their hydrolyzates and condensates, and the compounds represented by the above-mentioned formula (a-2), their hydrolyzates and condensates. Similarly, as the hydrolyzable silicon compound (b) in the coating composition (I), it is also preferred to contain one or more selected from the compounds containing the atomic group represented by the above-mentioned formula (b-1), their hydrolyzates and condensates, and the compounds represented by the above-mentioned formula (b-2), their hydrolyzates and condensates.

[0602] The details of the hydrolyzable silicon compounds (a) and (b) in the coating composition (I) are the same as those described above with respect to the polymer nanoparticles (A) and the matrix component (B) contained in the coating film (C).

[0603] [Content of the hydrolyzable silicon compound (a) in the polymer nanoparticles (A)]

[0604] In the coating composition (I), the content of the hydrolyzable silicon compound (a) represents the solid content weight ratio of the hydrolyzable silicon compound (a) contained in the polymer nanoparticles (A). The higher the content, the better the wear resistance, weather resistance and heat resistance. From this point of view, the higher the content, the more preferred. The above content is preferably 50% by mass or more, more preferably 60% by mass or more. The content of the hydrolyzable silicon compound (a) in the polymer nanoparticles (A) can be measured by, but not limited to, IR analysis, NMR analysis, elemental analysis, etc. of the polymer nanoparticles (A).

[0605] [Functional group (e)]

[0606] In the coating composition (I), the polymer nanoparticle (A) preferably has a functional group (e) that interacts with the matrix raw material component (B'). When the polymer nanoparticle (A) has the functional group (e), the matrix raw material component (B') is easily adsorbed on the surface of the polymer nanoparticle (A), forming a protective colloid and tending to stabilize, so the storage stability of the coating composition (I) tends to improve as a result. In addition, when the polymer nanoparticle (A) has the functional group (e), the interaction between the polymer nanoparticle (A) and the matrix raw material component (B') is enhanced, thereby the tackifying property relative to the solid content concentration of the coating composition (I) can be improved, and there is a tendency to sag when being coated into a complex shape, and the film thickness of the coating (C) has a tendency to become uniform. The situation that the polymer nanoparticle (A) has the functional group (e) can be confirmed by, for example, composition analysis based on IR, GC-MS, thermal decomposition GC-MS, LC-MS, GPC, MALDI-MS, TOF-SIMS, TG-DTA, NMR, and analysis based on their combination, etc.

[0607] Specific examples of the functional group (e) in the present embodiment include, but are not limited to, hydroxyl, carboxyl, amino, amide, and functional groups containing ether bonds. From the perspective of interaction, functional groups having hydrogen bonds are preferred, and from the perspective of high hydrogen bonding properties, amide groups are more preferred, and secondary amide groups and / or tertiary amide groups are further preferred.

[0608] Examples of the compound containing the functional group (e) and its reactant include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 2-hydroxyethyl vinyl ether or 4-hydroxybutyl vinyl ether, 2-hydroxyethyl allyl ether, (meth)acrylic acid, 2-carboxyethyl (meth)acrylate, 2-dimethylaminoethyl (meth)acrylate, 2-diethylaminoethyl (meth)acrylate, 2-di-n-propylaminoethyl (meth)acrylate, 3-dimethylaminopropyl (meth)acrylate, 4-dimethylaminobutyl (meth)acrylate, N-[2-(meth)acryloyloxy]ethylmorpholine, vinylpyridine, N-vinylcarbazole, N-vinylquinoline, N-methylacrylamide, N-methylmethacrylamide, N-ethylacrylamide, N,N-dimethylacrylamide, N,N-dimethylmethacrylamide 、N,N-diethylacrylamide, N-ethylmethacrylamide, N-methyl-N-ethylacrylamide, N-methyl-N-ethylmethacrylamide, N-isopropylacrylamide, N-n-propylacrylamide, N-isopropylmethacrylamide, N-n-propylmethacrylamide, N-methyl-N-n-propylacrylamide, N-methyl-N-isopropylacrylamide, N-acryloylpyrrolidine, N-methacryloylpyrrolidine, N-acryloylpiperidine, N-methacryloylpiperidine, N-acryloylhexahydroazepine, N-acryloylmorpholine, N-methacryloylmorpholine, N-vinylpyrrolidone, N-vinylcaprolactam, N,N'-methylenebisacrylamide, N,N'-methylenebismethacrylamide, N-vinylacetamide, acetylacetoneacrylamide, acetylacetonemethacrylamide, N-methylolacrylamide, N-methylolmethacrylamide, Blemmer PE-90, PE-200, PE-350, PME-100, PME-200, PME-400, AE-350 (trade names, manufactured by Nippon Oil & Fats Co., Ltd.), MA-30, MA-50, MA-100, MA-150, RA-1120, RA-2614, RMA-564, RMA-568, RMA-1114, MPG130-MA (trade names, manufactured by Nippon Emulsifier Co., Ltd.), etc. It should be noted that in this specification, (meth)acrylate is a simple description of acrylate or methacrylate, and (meth)acrylic acid is a simple description of acrylic acid or methacrylic acid.

[0609] [Elastic recovery rate η of the matrix raw material component (B') ITB’ and the elastic recovery rate η of the matrix component (B) ITB ]

[0610] Elastic recovery rate η of the matrix raw material component (B') in the coating composition (I) ITB’ It is the "Welast / W total The ratio η IT The parameter recorded in the form of " is obtained by measuring the coating film of the matrix raw material component (B') after film formation, and the total mechanical work W of the depression is used. total The amount of work done by the elastic recovery deformation of the concave elast Elastic recovery rate η ITB’ The higher the value, the more the coating can recover to its original state when it is impacted, and the higher the self-repair ability against impact. From the perspective of effectively exerting the self-repair ability, the elastic recovery rate η of the matrix raw material component (B') ITB’ Under the measurement conditions (Vickers tetrahedral diamond indenter, load increase condition 2mN / 20sec, load reduction condition 2mN / 20sec), it is preferably 0.60 or more, more preferably 0.65 or more. In addition, from the aspect of being able to follow the deformation of the substrate and component (A) when the coating is made, η ITB’ Preferably, it is less than 0.95. The elastic recovery rate of the matrix raw material component (B') can be measured by, but not limited to, the following methods: separating the polymer nanoparticles (A) and the matrix raw material component (B') by centrifugal separation or the like, dissolving the separated matrix raw material component (B') in a solvent to obtain a composition, applying the composition and drying it, and measuring the film after film formation using a micro hardness meter Fischerscope (HM2000S manufactured by Fischer Instruments), an ultra-micro indentation hardness tester (ENT-NEXUS manufactured by Elionix Co., Ltd.), a nano indenter (iNano, G200 manufactured by Toyo Technica), a nano indentation system (TI980 manufactured by Bruker), etc.

[0611] It should be noted that, as described above, the cured product obtained by curing the matrix raw material component (B') by hydrolysis condensation or the like is equivalent to the matrix component (B). Therefore, the elastic recovery rate η of the matrix raw material component (B') measured by the method described in the examples described later is ITB’ The value of and the corresponding elastic recovery rate η of the matrix component (B) ITB In good agreement, the elastic recovery rate η can be determined in this form ITB That is, the elastic recovery rate η of the matrix component (B) in this embodiment is ITB Preferably, it is 0.60 or more, and more preferably, it is 0.65 or more. In addition, from the aspect of being able to follow the deformation of the substrate and component (A) when the coating film is formed, η ITB It is preferably 0.95 or less.

[0612] As the elastic recovery rate η ITB’and elastic recovery rate η ITB The method of adjusting the content within the above range includes, but is not limited to, adjusting the structure and composition ratio of the constituent components of the matrix raw material component (B').

[0613] In the coating composition (I), the "hydrolyzable silicon compound (a) contained in the polymer nanoparticles (A)" and the "hydrolyzable silicon compound (b) contained in the matrix raw material component (B')" may be of the same kind or different kinds. Even when both are of the same kind, they can be distinguished by making the hydrolyzable silicon compound (a) contained in the polymer nanoparticles (A) and the hydrolyzable silicon compound (b) contained in the matrix raw material component (B').

[0614] [Inorganic oxide (D)]

[0615] In the coating composition (I), the matrix raw material component (B') includes an inorganic oxide (D). By including an inorganic oxide (D), not only the hardness of the matrix raw material component (B') can be improved, the wear resistance can be improved, but also the hydrophilicity of the hydroxyl group on the particle surface has a tendency to improve the anti-pollution property of the coating film. In addition, the inorganic oxide (D) contains at least one inorganic component selected from the group consisting of Ce, Nb, Al, Zn, Ti, Zr, Sb, Mg, Sn, Bi, Co and Cu. By including this inorganic component, the inorganic oxide (D) can improve weather resistance without damaging wear resistance and durability. From the aspect of improving performance in weather resistance, the inorganic oxide (D) preferably includes at least one inorganic component selected from the group consisting of Ce, Nb, Zn, Ti and Zr, more preferably includes Ce.

[0616] In the coating composition (I), the inorganic component in the inorganic oxide (D) preferably contains at least one inorganic oxide (D') selected from the group consisting of Ce, Nb, Zn, Ti and Zr from the perspective of the balance of wear resistance, durability and weather resistance. The content of the inorganic oxide (D') in the coating composition is not particularly limited. From the perspective of the balance of wear resistance, durability and weather resistance, it is preferably 1% by mass or more, more preferably 2% by mass or more, and from the perspective of transparency, it is preferably 50% by mass or less, more preferably 30% by mass or less. Here, the above content can be determined as the total amount of Ce, Nb, Zn, Ti and Zr when the solid content of the coating composition is 100% by mass.

[0617] As the inorganic oxide (D) in the coating composition (I), there is no particular limitation as long as it contains an inorganic component. That is, as the inorganic oxide (D) in the coating composition (I), regardless of the shape, it can be a single substance or a mixture. From the aspect of the interaction with the above-mentioned hydrolyzable silicon compound (b), it is preferred to further include silicon oxide particles, and from the aspect of dispersibility, as the form of silicon oxide particles, it is preferred to further include colloidal silicon oxide. When the inorganic oxide (D) includes colloidal silicon oxide, it is preferably in the form of an aqueous dispersion, and any of acidic and alkaline can be used.

[0618] The average particle size of the inorganic oxide (D) in the coating composition (I) is preferably 2 nm or more from the aspect of good storage stability of the coating composition (I), and preferably 150 nm or less from the aspect of good transparency. That is, the average particle size is preferably 2 nm or more and 150 nm or less, more preferably 2 nm or more and 100 nm or less, and further preferably 2 nm or more and 50 nm or less. The method for measuring the average particle size of the inorganic oxide (D) in the coating composition (I) is the same as the above method for the inorganic oxide (D) contained in the coating film (C).

[0619] The remaining characteristics of the inorganic oxide (D) in the coating composition (I) are the same as the above-mentioned characteristics of the inorganic oxide (D) contained in the coating film (C).

[0620] [Volume fraction of polymer nanoparticles (A) relative to the total of polymer nanoparticles (A) and matrix raw material component (B')]

[0621] In the coating composition (I), the volume fraction of the polymer nanoparticles (A) relative to the total of the polymer nanoparticles (A) and the matrix raw material component (B') is preferably 2% or more from the aspect of film-forming properties, and is preferably 80% or less from the aspect of the transparency of the coating film obtained by film formation. That is, the volume fraction of the polymer nanoparticles (A) in the coating composition (I) is preferably 2% or more and 80% or less, more preferably 3% or more and 70% or less, and further preferably 5% or more and 45% or less. The volume fraction of the polymer nanoparticles (A) in the coating composition (I) can be calculated, for example, based on the proportion of the polymer nanoparticles (A) in the entire coating film in the cross-sectional SEM image after the coating film (C) is formed, and the component ratio of the polymer nanoparticles (A) in the components constituting the coating composition (I).

[0622] [Core / Shell Structure of Polymer Nanoparticles (A)]

[0623] In the coating composition (I), the polymer nanoparticle (A) preferably has a core / shell structure having a core layer and one or more shell layers covering the core layer. From the aspect of the interaction with the outermost matrix raw material component (B') of the core / shell structure, the polymer nanoparticle (A) also preferably has the above-mentioned functional group (e). The situation that the polymer nanoparticle (A) has a core / shell structure can be confirmed by, for example, a transmission electron microscope image of a coating cross section, etc.

[0624] [Other ingredients that may be contained in the coating composition (I)]

[0625] From the perspective of further improving the coating properties of the coating composition (I), in the coating composition (I), as the matrix raw material component (B'), in addition to the above-mentioned components, a thickener, a leveling agent, a thixotropic agent, a defoaming agent, a freeze stabilizer, a dispersant, a wetting agent, a rheology control agent, a film-forming aid, a rust inhibitor, a plasticizer, a lubricant, a preservative, a mildew inhibitor, an antistatic agent, an antistatic agent, etc. may be mixed as needed. From the perspective of improving the film-forming properties, it is preferred to use a wetting agent and a film-forming aid, and specifically, but not particularly limited to, diethylene glycol monobutyl ether, ethylene glycol monobutyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, ethylene glycol mono-2-ethylhexyl ether, 2,2,4-trimethyl-1,3-butanediol isobutyrate, diisopropyl glutarate, propylene glycol n-butyl ether, dipropylene glycol n-butyl ether, tripropylene glycol n-butyl ether, dipropylene glycol n-butyl ether, Glycol methyl ether, tripropylene glycol methyl ether, MEGAFACE F-443, F-444, F-445, F-470, F-471, F-472SF, F-474, F-475, F-477, F-479, F-480SF, F-482, F-483, F-489, F-172D, F-178K (trade names, manufactured by DIC Corporation), SN WET 366, SN WET 980, SN WET L, SN WET S, SN WET 125, SN WET 126, SN WET 970 (trade names, manufactured by SAN NOPCO Co., Ltd.), etc. These compounds can be used alone or in combination of two or more.

[0626] [catalyst]

[0627] In the coating composition (I), as a matrix raw material component (B'), a catalyst may be included. When the coating composition (I) includes a catalyst that promotes the reaction of reactive groups, it is not easy to leave unreactive groups in the coating film, which can not only improve the hardness and wear resistance, but also improve the weather resistance, which is preferred from this aspect. The catalyst is not particularly limited, and when obtaining a hard coating film, it is preferably dissolved or dispersed. Such a catalyst is not particularly limited, and for example, organic acids, inorganic acids, organic bases, inorganic bases, metal alkoxides, metal chelates, etc. can be cited, and these catalysts can be used 1 or 2 or more in combination.

[0628] [Properties of coating composition (I)]

[0629] In the coating composition (I), from the viewpoint of coating properties, the solid content concentration is preferably 0.01 to 60% by mass, more preferably 1 to 40% by mass. In addition, from the viewpoint of coating properties, the viscosity of the coating composition (I) at 20° C. is preferably 0.1 to 100,000 mPa·s, more preferably 1 to 10,000 mPa·s.

[0630] <Method for Preparing Hard Coating Film>

[0631] The method for preparing the hard coating film and the substrate with the hard coating film of the present embodiment is not particularly limited. For example, the polymer nanoparticles (A), the matrix raw material component (B'), the inorganic oxide (D), and other suitable components can be dispersed and dissolved in a solvent, and the obtained coating composition (I) can be applied to the above-mentioned substrate, and formed into a coating film by heat treatment, ultraviolet irradiation, infrared irradiation, etc. In addition, as the above-mentioned coating method, for example, spray spraying, flow coating, brush coating, dip coating, spin coating, screen printing, casting, gravure printing, flexographic printing, etc. can be cited but not limited to. It should be noted that the coating composition (I) after the above-mentioned coating is preferably formed into a coating film by heat treatment at a temperature of preferably room temperature to 250°C, more preferably 40°C to 150°C, or ultraviolet irradiation, infrared irradiation, etc.

[0632] [Surface processing]

[0633] In the hard coating film or substrate with a hard coating film of the present embodiment, from the aspect of weather resistance, the surface can be processed by silicon oxide to form a silicon oxide layer. There is no particular limitation on the method for forming the silicon oxide layer. As a specific example, silicon oxide processing based on PECVD that vaporizes / cures silicone or silazane, and silicon oxide processing technology that modifies the surface into silicon oxide by irradiating 155nm ultraviolet rays can be cited. In particular, for the reason that a layer that is not easy to pass oxygen and water vapor can be made without deteriorating the surface, surface processing based on PECVD is preferred. Silicones or silazanes that can be used for PECVD can specifically include but are not limited to octamethylcyclotetrasiloxane, tetramethylcyclotetrasiloxane, decamethylcyclopentasiloxane, hexamethyldisiloxane, vinylmethoxysilane, vinylmethoxysilane, dimethyldimethoxysilane, TEOS, tetramethyldisiloxane, tetramethyltetravinylcyclotetrasiloxane, hexamethyldisilazane, etc., and they can be used one or more than two.

[0634] <Application of hard coating film and substrate with hard coating film>

[0635] The hard coating film and the substrate with the hard coating film of the present embodiment have excellent wear resistance and durability. Therefore, the use of the hard coating film and the substrate with the hard coating film is not particularly limited, and examples thereof include building materials, vehicle parts, electronic equipment, motor products, etc.

[0636] Examples of building material uses include, but are not limited to, window glass for construction machinery, window glass for buildings, houses, greenhouses, etc., roofs for garages and arcades, lighting such as lighting or signal lights, wallpaper surface materials, signs, sanitary products such as bathtubs and washstands, kitchen building materials, exterior wall materials, floor materials, cork materials, tiles, floor mats, interior floor materials such as linoleum.

[0637] As vehicle parts, there can be mentioned, but not limited to, parts used in various applications such as automobiles, aircraft, and trains. As specific examples, there can be mentioned various glasses such as front windshields, rear windshields, front doors, rear doors, rear side panels, sunroofs, front bumpers, rear bumpers, spoilers, door mirrors, front grilles, logo covers, exterior parts such as car bodies, interior parts such as center panels, door panels, instrument panels, center consoles, lamp parts such as headlights and taillights, lens parts for vehicle-mounted cameras, lighting covers, decorative films, and various glass replacement parts.

[0638] As electronic equipment and motor products, preferred examples include but are not limited to mobile phones, portable information terminals, personal computers, portable game consoles, OA equipment, solar cells, flat-panel displays, touch panels, DVDs, Blu-ray discs and other optical discs, polarizers, filters, lenses, prisms, optical fibers and other optical components, anti-reflection films, orientation films, polarizing films, phase difference films and other optical films, etc.

[0639] The substrate with a clear coating agent, a clear coating film, and a laminate according to the present embodiment can be suitably used in various fields such as machine parts, agricultural materials, fishery materials, transport containers, packaging containers, toys, and sundries in addition to the above-mentioned uses.

[0640] <Window material>

[0641] The window material of the present embodiment (hereinafter also referred to as "window material (J)") comprises a polycarbonate resin and a coating film disposed on the polycarbonate resin, wherein the coating film comprises polymer nanoparticles (A) and a matrix component (B), wherein the polymer nanoparticles (A) comprise a hydrolyzable silicon compound (a), and the matrix component (B) comprises a hydrolyzable silicon compound (b), and the Martens hardness of the window material is HM J 100N / mm 2 Above 4000N / mm 2 The elastic recovery rate η of the above window material measured by the indentation test according to ISO14577-1 is as follows: ITJ The matrix component (B) contains an inorganic oxide (D), and the inorganic oxide (D) contains at least one inorganic component selected from the group consisting of Ce, Nb, Al, Zn, Ti, Zr, Sb, Mg, Sn, Bi, Co and Cu. Due to such a configuration, the window material (J) has high wear resistance, durability and weather resistance. Since the window material (J) can show high levels of wear resistance, durability and weather resistance, it is preferably, but not limited to, suitable for, for example, a window material for automobiles.

[0642] Hereinafter, the window material (J) is sometimes described while referring to the constituent components of the polymer nanoparticles (A) and the matrix component (B) contained in the window material (J), and the details of the constituent components are the same as those described above for the polymer nanoparticles (A) and the matrix component (B) contained in the coating (C).

[0643] In the window material (J), the polymer nanoparticles (A) are preferably dispersed in the matrix component (B). The dispersion state can be confirmed by SEM observation of a cross section of the coating film.

[0644] In the window material (J), the polymer nanoparticles (A) contain the above-mentioned hydrolyzable silicon compound (a), and the matrix component (B) contains the above-mentioned hydrolyzable silicon compound (b). In addition, as the hydrolyzable silicon compound (a) in the window material (J), it is also preferred to contain one or more selected from the compounds containing the atomic group represented by the above-mentioned formula (a-1), their hydrolysis products and condensation products, and the compounds represented by the above-mentioned formula (a-2), their hydrolysis products and condensation products. Similarly, as the hydrolyzable silicon compound (b) in the window material (J), it is also preferred to contain one or more selected from the compounds containing the atomic group represented by the above-mentioned formula (b-1), their hydrolysis products and condensation products, and the compounds represented by the above-mentioned formula (b-2), their hydrolysis products and condensation products.

[0645] The details of the hydrolyzable silicon compounds (a) and (b) in the window material (J) are the same as those described above with respect to the polymer nanoparticles (A) and the matrix component (B) contained in the coating film (C).

[0646] [Martens hardness HM of window material (J) J ]

[0647] Martens hardness HM of window material (J) J , preferably 150N / mm from the perspective of wear resistance 2 More than, more preferably 200N / mm 2 Above, preferably 4000 N / mm from the viewpoint of flexural resistance 2 Below, more preferably 2000N / mm 2 Below, more preferably 1500 N / mm 2 As the Martens hardness HM of the window material (J) J The method of adjusting to the above range includes, but is not limited to, mixing the polymer nanoparticles (A) and the matrix raw material component (B') that satisfy the specific relationship represented by the above formula (3) and dispersing and dissolving the obtained composition in a solvent, applying the obtained coating composition on a substrate, and forming a coating film by heat treatment, ultraviolet irradiation, infrared irradiation, etc. In particular, when the content of the matrix component (B) increases relative to the total amount of the polymer nanoparticles (A) and the matrix component (B), the Martens hardness HM of the window material (J) increases. J As the content of matrix component (B) decreases, the Martens hardness HM of the window material (J) J Tends to decrease.

[0648] Elastic recovery rate η of window material (J) ITJ is the total mechanical work done by the depression W total The amount of work done by the elastic recovery deformation of the concave elast The ratio is defined as “Welast / W total The ratio η IT "Parameters recorded. Elastic recovery rate η ITJ The higher the value, the more the window material can recover to its original state after deformation, and the higher its self-repair ability against deformation. From the perspective of effectively exerting its self-repair ability, the elastic recovery rate η ITJ Under the measurement conditions (Vickers tetrahedral diamond indenter, load increase condition 2mN / 20sec, load decrease condition 2mN / 20sec), it is 0.50 or more. As long as it is within this range, the larger the value, the better. ITJ Preferably, it is 0.55 or more, more preferably 0.60 or more, and further preferably 0.65 or more. The elastic recovery rate of the window material in this embodiment can be measured by, but not limited to, for example, using a micro-hardness tester Fischerscope (HM2000S manufactured by Fischer Instruments), an ultra-micro indentation hardness tester (ENT-NEXUS manufactured by Elionix Co., Ltd.), a nanoindenter (iNano, G200 manufactured by Toyo Technica), a nanoindentation system (TI980 manufactured by Bruker), etc. to perform an indentation test on the surface of the window material. As a method for measuring the elastic recovery rate η ITJ The method for adjusting to the above range may include, but is not limited to, mixing polymer nanoparticles (A) satisfying the specific relationship represented by the above formula (3) with the matrix raw material component (B') described later and dispersing and dissolving the obtained composition in a solvent, applying the obtained coating composition on a substrate, and forming a coating film by heat treatment, ultraviolet irradiation, infrared irradiation, etc.

[0649] In the window material (J), it is preferred to adjust the content of the hydrolyzable silicon compound (a). Here, the content of the hydrolyzable silicon compound (a) represents the weight ratio of the hydrolyzable silicon compound (a) contained in the polymer nanoparticles (A) relative to the solid content of the polymer nanoparticles (A). The higher the content, the better the wear resistance and weather resistance. From this perspective, the higher the content, the more preferred. The content is preferably 50% by mass or more, more preferably 60% by mass or more. The content of the hydrolyzable silicon compound (a) in the polymer nano...

Claims

1. A coating composition comprising: A mixture of adhesive latex particles (F) and an inorganic oxide (G) and / or a complex of the inorganic oxide (G) and the adhesive latex particles (F); Sunscreen (S1); and Isocyanate compounds, in, The average particle size of the mixture and / or the composite is 2 nm or more and 2000 nm or less. The mass ratio of the inorganic oxide (G) to the adhesive latex particles (F) is 1:0.1 to 1:10, The inorganic oxide (G) is spherical and / or interconnected silicon oxide.

2. The coating composition according to claim 1, wherein The sunscreen (S1) contains an ultraviolet absorber.

3. The coating composition according to claim 1 or 2, further comprising a hindered amine light stabilizer.

4. The coating composition according to claim 1 or 2, wherein The aspect ratio of the inorganic oxide (G), that is, the major axis / minor axis, is 3-25.

5. The coating composition according to claim 1 or 2, wherein The isocyanate compound is a water-dispersible isocyanate compound.

6. The coating composition according to claim 5, wherein The water-dispersible isocyanate compound is a blocked isocyanate.

7. The coating composition according to claim 1 or 2, wherein The adhesive latex particles (F) have a functional group (e) containing a secondary amide group and / or a tertiary amide group.

8. The coating composition according to claim 1 or 2, wherein The adhesive latex particles (F) have a functional group containing a hydroxyl group.

Citation Information

Patent Citations

  • Hard coating composition and hard coating film using the same

    CN107400449A

  • Coating film

    CN107429119A

  • Laminated polyester film

    JP2015147407A