Wear-resistant floor material prepared from electric furnace ferronickel slag and preparation method of wear-resistant floor material

By combining the modified nickel-ferroelectric slag with water-based epoxy resin, an interpenetrating network structure is formed, which solves the problems of low strength and insufficient adhesion in wear-resistant floor materials in the early stage, and has excellent wear resistance and Environmentally friendly polymer floor coatings achieve efficient utilization of nickel slag.

CN118909509APending Publication Date: 2024-11-08FUJIAN ACAD OF BUILDING RES CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410987677.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-08
Patent Text Reader

Abstract

The invention belongs to the field of comprehensive utilization of resources, and particularly relates to a wear-resistant floor material prepared from electric furnace ferronickel slag and a preparation method of the wear-resistant floor material. The wear-resistant floor material is prepared from the following raw material components: modified ferro-nickel electric furnace slag, water-borne epoxy resin, a water-borne coating additive, filler and deionized water, the preparation method comprises the following steps: grinding ferro-nickel electric furnace slag powder to a certain fineness, carrying out surface coating modification on the ferro-nickel electric furnace slag powder, and mixing the modified ferro-nickel electric furnace slag as a wear-resistant component with a water-borne epoxy resin emulsion and other components according to a certain ratio to prepare the wear-resistant floor coating. The interface compatibility of the ferro-nickel electric furnace slag and the water-based resin matrix can be effectively improved, and the wear-resistant floor coating with excellent wear resistance, construction performance and environmental protection performance is prepared. The method is simple in process and easy to popularize and apply, and has remarkable economic and social benefits.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of comprehensive resource utilization, and specifically relates to a wear-resistant floor material prepared by utilizing electric furnace nickel-iron slag and a preparation method thereof. Background Art

[0002] Nickel slag is the fourth largest smelting industrial waste slag in my country. Among them, electric furnace nickel-iron slag is the solid waste generated when nickel alloy is produced by electric furnace process. Its main components are SiO2, MgO, FeO, etc. It has general wear resistance, poor activity and low comprehensive utilization rate. Wear-resistant floor coating is a special coating, which is mainly used for floors that require high wear resistance and high strength. Traditional wear-resistant floor materials mainly use cement or polymer as binder, and add wear-resistant aggregates such as carborundum and corundum to prepare wear-resistant floor materials. Among them, cement-based wear-resistant floor materials have low strength and poor acid and alkali resistance. Polymer wear-resistant floor materials have many advantages such as high strength, high elasticity, high wear resistance, and excellent chemical resistance. However, due to their high cost, their application is subject to certain restrictions. Electric furnace nickel-iron slag is a waste slag with a lot of glass formed by water quenching and rapid cooling during the smelting process. If its high hardness and high wear resistance can be used to replace natural wear-resistant aggregates and used to prepare wear-resistant floor materials, its excellent performance can be guaranteed while its cost can be reduced. This is of great significance for realizing the resource utilization and reduction of electric furnace nickel slag.

[0003] At present, the reports on the use of nickel slag in wear-resistant floor materials are mainly concentrated on cement-based floor materials. For example, Li Hao and others from Yangzhou University added nickel slag as fine aggregate and powder into cement respectively, but the dosage was low, nickel slag was only 40% of fine aggregate, and powder was only 10% of total cementitious materials, and the maximum strength was only 35.8MPa. Yu Yan, Chen Guoquan and others used nickel slag to replace part of quartz sand to prepare cement-based self-leveling mortar. Although the final 28d compressive strength reached about 80MPa, its early strength was low, and the 3d strength only reached about 40MPa. Therefore, cement-based wear-resistant floor materials generally have many defects such as low early strength, insufficient elasticity, easy to dust and crack, etc.

[0004] Floor materials using polymers as adhesives have excellent physical and chemical properties. Among them, water-based polymers have gradually become the mainstream due to their advantages of environmental protection, safety, and non-toxicity, but the cost is relatively high. Nickel slag has high hardness and high wear resistance. If it can replace natural wear-resistant materials for water-based polymers to prepare wear-resistant floor materials, the cost can be greatly reduced. However, the adhesion between water-based polymers and inorganic wear-resistant fillers is general. If nickel slag is directly added as a wear-resistant filler to the water-based polymer matrix to prepare wear-resistant floor materials, the wear-resistant particles often fall off during the wear process, and it is difficult to exert the high wear resistance of nickel slag. The present invention uses modification technology to form an interpenetrating network structure between nickel slag and the water-based polymer matrix, significantly improves the binding force of the inorganic / organic interface, thereby giving full play to the high wear resistance of nickel slag and the flexibility of the water-based polymer matrix, and obtaining a rigid-flexible wear-resistant floor material. Research and application of nickel slag in polymer wear-resistant floor materials have not yet been found. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide an environmentally friendly wear-resistant polymer floor coating prepared by using nickel-iron slag from an electric furnace and a preparation method thereof.

[0006] The present invention is achieved in that:

[0007] The present invention first provides an environmentally friendly wear-resistant polymer floor coating prepared by using electric furnace nickel-iron slag, and its raw material components include: modified nickel-iron electric furnace slag, water-based epoxy resin, water-based coating additive, filler and deionized water; the preparation method of the modified nickel-iron electric furnace slag is as follows:

[0008] The nickel-iron electric furnace slag is dried and mixed with calcium oxide at a mass ratio of 1:0.03-0.08. The mixture is ground and then passed through sieves with particle sizes of (0.1-0.3) mm, (0.3-0.6) mm and (0.6-1.0) mm respectively. The sieved materials are then mixed at a mass ratio of 6:3:1 to prepare modified nickel-iron electric furnace slag.

[0009] Furthermore, the modified nickel-iron electric furnace slag is pretreated before being mixed with other raw material components, and the pretreatment method is as follows: diluting the aqueous epoxy resin emulsion with deionized water, and immersing the modified nickel-iron electric furnace slag in the diluted emulsion, wherein the mass ratio of the modified nickel-iron electric furnace slag to the aqueous epoxy resin emulsion is 7:3, stirring evenly so that each particle is evenly coated, and then drying so that the epoxy resin forms a uniform film on the surface of the modified nickel-iron electric furnace slag, thereby preparing a composite modified nickel-iron electric furnace slag.

[0010] Furthermore, the raw material components include by weight:

[0011] Water-based epoxy resin emulsion: 50-60 parts

[0012] Deionized water: 10-20 parts

[0013] Composite modified nickel-iron electric furnace slag: 10-20 parts

[0014] Heavy calcium carbonate: 12-20 parts

[0015] Talc: 8-15 parts

[0016] Glass fiber: 1-3 parts

[0017] Dispersant: 0.5-0.8 parts

[0018] Thickener: 0.3-0.6 parts

[0019] Leveling agent: 0.2-0.5 parts

[0020] Defoaming agent: 0.05-0.2 parts.

[0021] The present invention also provides a method for preparing the environmentally friendly wear-resistant polymer floor coating, which specifically comprises the following steps:

[0022] Step 1: Dry the nickel-iron electric furnace slag and mix it with calcium oxide in a certain proportion, the mass ratio of which is 1:0.03-0.08, put the mixture into a grinder, and grind it for 1h-3h. The mixture is respectively sized to (0.1-0.3) mm, (0.3-0.6) mm and (0.6-1.0) mm, and then (0.1-0.3) mm: (0.3-0.6) mm: (0.6-1.0) mm are mixed in a mass ratio of 6:3:1 to prepare modified nickel-iron electric furnace slag.

[0023] Step 2: dilute part of the aqueous epoxy resin emulsion with deionized water, and soak the modified nickel-iron electric furnace slag in the diluted emulsion, wherein the mass ratio of the modified nickel-iron electric furnace slag to the aqueous epoxy resin emulsion is 6:4-7:3, stir evenly so that each particle is evenly coated, and then dry so that the epoxy resin forms a uniform film on the surface of the modified nickel-iron electric furnace slag to prepare a composite modified nickel-iron electric furnace slag.

[0024] Step 3: Add the raw material components in the order of water-based epoxy resin emulsion, deionized water, composite modified nickel-iron electric furnace slag, glass fiber, and water-based coating additive, stir and mix well, and finally use a high shear mixer for final mixing.

[0025] The purpose of step 1 of mixing by particle size is to make the mixture as dense as possible and to minimize the gaps, thereby reducing the amount of resin used.

[0026] The main purpose of step 2 is to use resin to pre-wrap the nickel-iron electric furnace slag particles so that they are not easy to fall off during subsequent use, making the product have better wear resistance. If the proportion of water-based epoxy resin emulsion continues to increase, there will be no significant improvement in the modification effect, and the cost performance will decrease; if the proportion of water-based epoxy resin emulsion decreases, the effect will be relatively poor; when the mass ratio of modified nickel-iron electric furnace slag to water-based epoxy resin emulsion is 6:4-7:3, the modification effect is best.

[0027] The invention has the following advantages: the invention can effectively improve the interfacial compatibility between nickel-iron electric furnace slag and water-based resin matrix, and prepare a wear-resistant floor coating with excellent wear resistance, construction performance and environmental protection performance. The invention has a simple process, is easy to promote and apply, and has significant economic and social benefits. DETAILED DESCRIPTION

[0028] The technical scheme of the present invention will be described clearly and completely below in conjunction with specific embodiments. If no specific conditions are specified in the examples, the conditions are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0029] A method for preparing an environmentally friendly wear-resistant polymer floor coating using electric furnace nickel-iron slag, specifically comprising the following steps:

[0030] Step 1: Preparation of wear-resistant components: Dry the nickel-iron electric furnace slag and mix it with calcium oxide in a certain proportion, the mass ratio of which is 1:0.03-0.08, put the mixture into a grinder and grind it for 1h-3h, and respectively pass the mixture into particle sizes of (0.1-0.3)mm, (0.3-0.6)mm and (0.6-1.0)mm, and then mix (0.1-0.3)mm: (0.3-0.6)mm: (0.6-1.0)mm in a mass ratio of 6:3:1 to prepare a wear-resistant component.

[0031] Step 2: Mix 100 grams of epoxy resin emulsion with 500 milliliters of deionized water, soak the wear-resistant components mixed in proportion into the diluted epoxy resin emulsion, the mass ratio of the wear-resistant components to the epoxy resin emulsion is 6:4-7:3, stir evenly so that each particle is evenly coated, dry at 60°C so that the epoxy resin forms a uniform film on the surface of the nickel-iron electric furnace slag, and dry for 24 hours to prepare a composite modified nickel-iron electric furnace slag.

[0032] Step 3: The weight proportions of the components are as follows:

[0033] Water-based epoxy resin emulsion: 50-60 parts

[0034] Deionized water: 10-20 parts

[0035] Composite modified nickel-iron electric furnace slag: 10-20 parts

[0036] Heavy calcium carbonate: 12-20 parts

[0037] Talc: 8-15 parts

[0038] Glass fiber: 1-3 parts

[0039] Dispersant: 0.5-0.8 parts

[0040] Thickener: 0.3-0.6 parts

[0041] Leveling agent: 0.2-0.5 parts

[0042] Defoamer: 0.05-0.2 parts

[0043] Step 4:

[0044] Preliminary mixing: Pour the water-based epoxy resin emulsion and deionized water into the stirrer according to the proportion in step 3, stir for 5 minutes, stir at a speed of 300 rpm, and stir at a temperature of (20-25)°C.

[0045] Add filler: gradually add heavy calcium carbonate and talcum powder, stirring time (10-20) minutes, stirring speed 500 rpm, stirring temperature room temperature (20-25) °C.

[0046] Add modified nickel-iron electric slag: gradually add the composite modified nickel-iron electric slag prepared in step 2, the addition amount is about 10%-30% of the total mass of epoxy resin emulsion, deionized water, heavy calcium carbonate and talcum powder, stirring time (10-30) minutes, stirring speed 500rpm, stirring temperature room temperature (20-25) °C.

[0047] Adding glass fiber: Add glass fiber, stir for (5-15) minutes, stir at 300 rpm, and stir at room temperature (20-25) °C.

[0048] Add additives: gradually add dispersant, thickener, leveling agent and defoamer, stirring time for 5 minutes, stirring speed 300 rpm, stirring temperature room temperature (20-25) ℃.

[0049] High shear stirring: Use a high shear stirrer for final mixing, with a stirring time of (15-30) minutes, a stirring speed of 1500 rpm, and a stirring temperature of room temperature (20-25)°C.

[0050] Embodiment 1:

[0051] Water-based epoxy resin emulsion: 50 parts

[0052] Deionized water: 10 parts

[0053] Heavy calcium carbonate: 15 parts

[0054] Talc: 10 parts

[0055] Composite modified nickel-iron electric furnace slag: 12 parts (the mass ratio of nickel-iron electric furnace slag to calcium oxide is 1:0.05, and the mass ratio of modified nickel-iron electric furnace slag to water-based epoxy resin emulsion is 6:4)

[0056] Glass fiber: 2 parts

[0057] Dispersant: 0.5 parts

[0058] Thickener: 0.5 parts

[0059] Leveling agent: 0.3 parts

[0060] Defoaming agent: 0.08 parts.

[0061] The performance results are as follows:

[0062] Hardness: Pencil hardness test 4H.

[0063] Adhesion:>4.5MPa (pull-off method).

[0064] Wear resistance: wear loss 20mg / 1000 revolutions (using CS-17 grinding wheel, 1kg load).

[0065] Compressive strength: 105MPa (test method: ASTM D695).

[0066] Tensile strength: 55 MPa (test method: ASTM D638).

[0067] Embodiment 2:

[0068] Water-based epoxy resin emulsion: 60 parts

[0069] Deionized water: 15 parts

[0070] Heavy calcium carbonate: 16 parts

[0071] Talc: 12 parts

[0072] Composite modified nickel-iron electric furnace slag: 19 parts (the mass ratio of nickel-iron electric furnace slag to calcium oxide is 1:0.03, and the mass ratio of modified nickel-iron electric furnace slag to water-based epoxy resin emulsion is 7:3)

[0073] Glass fiber: 2 parts

[0074] Dispersant: 0.5 parts

[0075] Thickener: 0.5 parts

[0076] Leveling agent: 0.5 parts

[0077] Defoaming agent: 0.2 parts.

[0078] The performance results are as follows:

[0079] Hardness: Pencil hardness test 6H.

[0080] Adhesion:>4.5MPa (pull-off method).

[0081] Wear resistance: wear loss 12mg / 1000 revolutions (using CS-17 grinding wheel, 1kg load).

[0082] Compressive strength: 130MPa (test method: ASTM D695).

[0083] Tensile strength: 65 MPa (test method: ASTM D638).

[0084] Embodiment 3:

[0085] Water-based epoxy resin emulsion: 55 parts

[0086] Deionized water: 12 parts

[0087] Heavy calcium carbonate: 15 parts

[0088] Talc: 10 parts

[0089] Composite modified nickel-iron electric furnace slag: 18 parts (the mass ratio of nickel-iron electric furnace slag to calcium oxide is 1:0.08, and the mass ratio of modified nickel-iron electric furnace slag to water-based epoxy resin emulsion is 7:3)

[0090] Glass fiber: 2 parts

[0091] Dispersant: 0.5 parts

[0092] Thickener: 0.5 parts

[0093] Leveling agent: 0.3 parts

[0094] Defoaming agent: 0.1 part.

[0095] The performance results are as follows:

[0096] Hardness: Pencil hardness test 6H.

[0097] Adhesion:>4.5MPa (pull-off method).

[0098] Wear resistance: wear loss 15mg / 1000 revolutions (using CS-17 grinding wheel, 1kg load).

[0099] Compressive strength: 110MPa (test method: ASTM D695).

[0100] Tensile strength: 62MPa (test method: ASTM D638).

[0101] Comparative Example 1:

[0102] Water-based epoxy resin emulsion: 50 parts

[0103] Deionized water: 10 parts

[0104] Heavy calcium carbonate: 15 parts

[0105] Talc: 10 parts

[0106] Unmodified nickel-iron electric furnace slag: 12 parts

[0107] Glass fiber: 2 parts

[0108] Dispersant: 0.5 parts

[0109] Thickener: 0.5 parts

[0110] Leveling agent: 0.3 parts

[0111] Defoaming agent: 0.08 parts.

[0112] The performance results are as follows:

[0113] Hardness: Pencil hardness test H.

[0114] Adhesion:>4.5MPa (pull-off method).

[0115] Wear resistance: wear loss 41 mg / 1000 revolutions (using CS-17 grinding wheel, 1 kg load).

[0116] Compressive strength: 103MPa (test method: ASTM D695).

[0117] Tensile strength: 48 MPa (test method: ASTM D638).

[0118] Compared with Example 1, the unmodified nickel-iron electric furnace slag is relatively weakly combined with the waterborne epoxy resin emulsion, so its hardness and wear resistance are relatively poor.

[0119] Comparative Example 2:

[0120] Water-based epoxy resin emulsion: 60 parts

[0121] Deionized water: 15 parts

[0122] Heavy calcium carbonate: 16 parts

[0123] Talc: 12 parts

[0124] Composite modified nickel-iron electric furnace slag (the mass ratio of nickel-iron electric furnace slag to calcium oxide is 1:0.03, and the mass ratio of the wear-resistant component to the epoxy resin emulsion used in the composite modification is 9:1): 19 parts

[0125] Glass fiber: 2 parts

[0126] Dispersant: 0.5 parts

[0127] Thickener: 0.5 parts

[0128] Leveling agent: 0.5 parts

[0129] Defoaming agent: 0.2 parts.

[0130] The performance results are as follows:

[0131] Hardness: Pencil hardness test 3H.

[0132] Adhesion:>4.5MPa (pull-off method).

[0133] Wear resistance: wear loss 29mg / 1000 revolutions (using CS-17 grinding wheel, 1kg load).

[0134] Compressive strength: 122MPa (test method: ASTM D695).

[0135] Tensile strength: 61 MPa (test method: ASTM D638).

[0136] Compared with Example 2, the proportion of the modified solution used in the composite modification stage of the nickel-iron electric furnace slag in this comparative example deviates from the recommended proportion, so its composite modification effect does not reach the optimal state, and its hardness and wear resistance are not as good as those in Example 2.

[0137] Although the specific implementation modes of the present invention are described above, those skilled in the art should understand that the specific implementation modes described are only illustrative and are not intended to limit the scope of the present invention. Equivalent modifications and changes made by those skilled in the art in accordance with the spirit of the present invention should be included in the scope of protection of the claims of the present invention.

Claims

1. An environmentally friendly wear-resistant polymer floor coating prepared using electric furnace nickel-iron slag, characterized in that: The raw material components include: modified nickel-iron electric furnace slag, water-based epoxy resin, water-based coating additive, filler and deionized water; the preparation method of the modified nickel-iron electric furnace slag is as follows: The nickel-iron electric furnace slag is dried and mixed with calcium oxide at a mass ratio of 1:0.03-0.08, the mixture is ground and then passed through sieves with particle sizes of 0.1-0.3mm, 0.3-0.6mm and 0.6-1.0mm respectively, and then the sieved materials are mixed at a mass ratio of 6:3:1 to prepare modified nickel-iron electric furnace slag.

2. The environmentally friendly wear-resistant polymer floor coating prepared by using electric furnace nickel-iron slag according to claim 1, characterized in that: The modified nickel-iron electric furnace slag is pretreated before being mixed with other raw material components. The pretreatment method is as follows: diluting the aqueous epoxy resin emulsion with deionized water, and immersing the modified nickel-iron electric furnace slag in the diluted emulsion, wherein the mass ratio of the modified nickel-iron electric furnace slag to the aqueous epoxy resin emulsion is 6:4-7:3, stirring evenly so that each particle is evenly coated, and then drying so that the epoxy resin forms a uniform film on the surface of the modified nickel-iron electric furnace slag to prepare a composite modified nickel-iron electric furnace slag.

3. The environmentally friendly wear-resistant polymer floor coating prepared by using electric furnace nickel-iron slag according to claim 2, characterized in that: The raw material components include by weight: Water-based epoxy resin emulsion: 50-60 parts Deionized water: 10-20 parts Composite modified nickel-iron electric furnace slag: 10-20 parts Heavy calcium carbonate: 12-20 parts Talc: 8-15 parts Glass fiber: 1-3 parts Dispersant: 0.5-0.8 parts Thickener: 0.3-0.6 parts Leveling agent: 0.2-0.5 parts Defoaming agent: 0.05-0.2 parts.

4. A method for preparing an environmentally friendly wear-resistant polymer floor coating as claimed in any one of claims 1 to 3, characterized in that: The specific steps include: Step 1: Dry the nickel-iron electric furnace slag and mix it with calcium oxide in a certain proportion, the mass ratio of which is 1:0.03-0.08, put the mixture into a grinder, and grind it for 1h-3h. The mixture is respectively sized to (0.1-0.3) mm, (0.3-0.6) mm and (0.6-1.0) mm, and then (0.1-0.3) mm: (0.3-0.6) mm: (0.6-1.0) mm are mixed in a mass ratio of 6:3:1 to prepare modified nickel-iron electric furnace slag. Step 2: dilute part of the aqueous epoxy resin emulsion with deionized water, and soak the modified nickel-iron electric furnace slag in the diluted emulsion, wherein the mass ratio of the modified nickel-iron electric furnace slag to the aqueous epoxy resin emulsion is 6:4-7:3, stir evenly so that each particle is evenly coated, and then dry so that the epoxy resin forms a uniform film on the surface of the modified nickel-iron electric furnace slag to prepare a composite modified nickel-iron electric furnace slag. Step 3: Add the raw material components in the order of water-based epoxy resin emulsion, deionized water, composite modified nickel-iron electric furnace slag, glass fiber, and water-based coating additive, stir and mix well, and finally use a high shear mixer for final mixing.