Quick-curing anticorrosive paint for high-humidity environment and preparation method thereof
By using anticorrosion coatings composed of bisphenol A type epoxy resin and polyamide curing agent in high humidity environments, combined with fillers such as zinc phosphate and talc powder, traditional anticorrosion coatings are solved in a slow curing speed and coating in high humidity environments. The problem of quality degradation achieves rapid curing and good anti-corrosion performance, avoids problems such as bubbles and shrinkage, and meets environmental protection requirements.
Patent Information
- Application Number
- CN202411357464.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-27
- Publication Date
- 2024-11-08
AI Technical Summary
Traditional anticorrosion coatings have slow curing speed in high humidity environments, resulting in a decrease in coating quality, affecting the anticorrosion effect, and have problems such as bubbles, shrinkage holes, and sags. In addition, environmental pollution is serious and construction is difficult.
Anticorrosion coatings composed of bisphenol A type epoxy resin, polyamide curing agent, zinc phosphate anti-rust pigment, talc powder and barium sulfate filler, dispersant, leveling agent and defoaming agent are used to modify amine curing agents in Rapid curing in high humidity environments to form a uniform and dense coating, meeting environmental protection requirements VOC≤420g/L.
Fast curing is achieved in an environment with humidity exceeding 80%, avoiding bubbles, shrinkage, and sagging, forming good anti-corrosion and mechanical properties, suitable for large-scale production, and comply with environmental protection standards.
Smart Images

Figure FT_1 
Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of anti-corrosion coatings, and in particular to an anti-corrosion coating for rapid curing in a high-humidity environment and a preparation method thereof. Background Art
[0002] In many industrial fields, such as marine engineering, chemical equipment, bridges, etc., the corrosion of metal materials is a serious problem. In order to protect metal materials, anti-corrosion coatings are usually used. However, in high humidity environments, traditional anti-corrosion coatings cure slowly, which can easily lead to a decrease in coating quality and affect the anti-corrosion effect. Therefore, it is of great significance to develop an anti-corrosion coating that can cure quickly in a high humidity environment. Although there are many types of anti-corrosion coatings on the market, there are still problems such as short application life, serious environmental pollution and difficulty in construction. In addition, they cannot cure quickly in an environment with a humidity of more than 80%, and there will be problems such as bubbles, shrinkage holes, and serious sagging. Therefore, it is urgent to develop an anti-corrosion coating that has excellent anti-corrosion properties, can cure quickly in a high humidity environment, and does not have problems such as shrinkage holes, bubbles, and sagging. Summary of the invention
[0003] The purpose of the present invention is to provide an anti-corrosion coating for rapid curing in a high-humidity environment and a preparation method thereof. The anti-corrosion coating can be rapidly cured in an environment with a humidity exceeding 80%, and at the same time, problems such as bubbles, shrinkage cavities, and sagging will not occur, forming a uniform and dense coating, and meeting the environmental protection requirement of VOC≤420g / L, and having good anti-corrosion performance.
[0004] In a first aspect, the present invention provides an anticorrosive coating for rapid curing in a high humidity environment, comprising independently packaged component A and component B, wherein the components are composed as follows in parts by weight: Component A: 20-40 parts of bisphenol A epoxy resin; Solvent 10-20 parts; 10-20 parts of anti-rust pigment; Pigment 5-10 parts; Filler 10-40 parts; 1 to 5 parts of additives; Component B: Polyamide curing agent 8 to 12 parts.
[0005] In the above-mentioned anti-corrosion coating for rapid curing in high humidity environment, the bisphenol A type epoxy resin is Hexion 828 epoxy resin.
[0006] In the above-mentioned anticorrosive coating for rapid curing in a high-humidity environment, the solvent is a mixture of xylene and n-butanol, preferably a mixture of xylene and n-butanol in a mass ratio of 3:1; The anti-rust pigment is zinc phosphate; The pigment is titanium dioxide; The filler is talc and barium sulfate, preferably talc and barium sulfate in a weight ratio of 15: (10-20); The particle size of the filler is 1000-2500 meshes.
[0007] In the above-mentioned anticorrosive coating for rapid curing in high humidity environment, the 1 to 5 parts of auxiliary agents include the following components in parts by weight: Dispersant 0.3-1.5 parts; 0.3-1.5 parts of leveling agent; 0.4 to 2 parts of defoaming agent.
[0008] In the above-mentioned anti-corrosion coating for rapid curing in a high-humidity environment, the dispersant is BYK-110 or BYK-163; The leveling agent is BYK-306 or BYK-333; The defoamer is BYK-141 or BYK-052.
[0009] In the above-mentioned anti-corrosion coating for rapid curing in high humidity environment, the polyamide curing agent is Hansen 3115A.
[0010] In a second aspect, the present invention provides a method for preparing the anticorrosive coating for rapid curing in a high humidity environment as described in any one of the above, comprising: The preparation method of component A comprises the following steps: (1) mixing the bisphenol A epoxy resin and the solvent to disperse them; (2) adding the anti-rust pigment, the pigment, the filler and the auxiliary agent to the system obtained in step 1) and dispersing them to obtain the component A; The preparation method of component B comprises the following steps: The polyamide curing agent is taken to obtain the component B.
[0011] In the above-mentioned method for preparing an anticorrosive coating for rapid curing in a high-humidity environment, in step (1), in the dispersion step, the temperature is maintained at ≤50°C, and the dispersion is carried out at 1000-2000 rpm for 30 minutes; In step (2), in the dispersion step, the temperature is maintained at ≤50°C, and the mixture is stirred or sand-milled at 1000-2000 rpm for 30 minutes to 1 hour; The method further comprises the following steps in step (2): cooling the dispersed system to 40° C. and stirring evenly.
[0012] In a third aspect, the present invention provides a metal corrosion protection method, comprising the following steps: Component A and component B in any of the above-mentioned anti-corrosion coatings for rapid curing in high-humidity environments are mixed evenly, and coated on a metal surface for curing.
[0013] In the above-mentioned metal anticorrosion method, the curing is carried out in a high humidity environment with a humidity ≥ 80% RH.
[0014] The present invention has the following beneficial effects: (1) The present invention uses a modified amine curing agent, which can react quickly with the epoxy resin in a high humidity environment to achieve rapid curing of the coating.
[0015] (2) The anti-rust pigments and fillers selected in the present invention can improve the anti-corrosion performance and mechanical properties of the coating.
[0016] (3) The preparation method of the present invention is simple, easy to operate, and suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 The present invention is a process flow chart for preparing an anti-corrosion coating that cures quickly in a high-humidity environment. DETAILED DESCRIPTION
[0018] As described in the background technology, the traditional anti-corrosion coating has a slow curing speed in a high humidity environment with a humidity of more than 80%, which easily leads to a decrease in the quality of the coating and affects the anti-corrosion effect. Based on this, the present invention provides an anti-corrosion coating for rapid curing in a high humidity environment, including independently packaged components A and B, and the components are composed as follows in parts by weight: component A: 20 to 40 parts of bisphenol A epoxy resin; 10 to 20 parts of solvent; 10 to 20 parts of anti-rust pigment; 5 to 10 parts of pigment; 10 to 40 parts of filler; 1 to 5 parts of auxiliary agent; component B: 8 to 12 parts of polyamide curing agent. The anti-corrosion coating can be quickly cured in an environment with a humidity of more than 80%, and at the same time, there will be no problems such as bubbles, shrinkage holes, and sagging, forming a uniform and dense coating, and meeting the environmental protection requirements of VOC≤420g / L, and has good anti-corrosion performance.
[0019] In the present invention, the high humidity environment refers to an environment with humidity ≥ 80%RH. Humidity refers to "relative humidity", which is expressed as RH (Relative Humidity), which refers to the ratio of the actual water vapor pressure in the air to the saturated water vapor pressure at the current temperature. It reflects the degree of air from saturated air, and represents the ratio of the absolute humidity in the air to the saturated absolute humidity at the same temperature and pressure, as a percentage value, that is, the ratio of the mass of water vapor contained in a certain humid air to the mass of water vapor contained in saturated air at the same temperature and pressure.
[0020] According to the present invention, preferably, the anti-corrosion coating for rapid curing in a high-humidity environment comprises independently packaged component A and component B, and the components are composed as follows in parts by weight: component A: 25 parts of bisphenol A epoxy resin; 18.3 parts of solvent; 15 parts of anti-rust pigment; 10 parts of pigment; 30 parts of filler; 2 parts of additive; component B: 10 parts of polyamide curing agent.
[0021] In some embodiments of the present invention, the bisphenol A epoxy resin is Epikote 828 epoxy resin. Epikote 828 is a liquid epoxy resin with a viscosity (mpa·s) of 12000-14000 at 5°C and an epoxy equivalent of 184-190 g / ep. Epoxy resin is a film-forming substance, also known as a base material.
[0022] In some embodiments of the present invention, the solvent is a mixture of xylene and n-butanol, preferably xylene and n-butanol in a mass ratio of 3:1.
[0023] In some embodiments of the present invention, the anti-rust pigment is zinc phosphate; zinc phosphate is a white non-toxic anti-rust pigment, a new generation of non-toxic and pollution-free anti-rust pigment with excellent anti-corrosion effect, and can replace traditional anti-rust pigments containing toxic lead, chromium and other substances.
[0024] In some embodiments of the present invention, the pigment is titanium dioxide (titanium dioxide), a white pigment.
[0025] In some embodiments of the present invention, the filler is talcum powder and barium sulfate, preferably talcum powder and barium sulfate in a weight ratio of 15: (10-20), including but not limited to talcum powder and barium sulfate in a weight ratio of 20:10, 20:15 or 15:10; wherein the particle size of the filler is 1000-2500 mesh, including but not limited to 1250 mesh. Talc and barium sulfate are used as fillers. Talc increases the hardness, filling property, polishability and reduces the cost of the paint; barium sulfate can reduce the cost and improve the acid resistance, alkali resistance and adhesion of the paint; the combination of the two is more conducive to performance improvement.
[0026] According to the present invention, the 1-5 parts of auxiliary agents include the following components by weight: 0.3-1.5 parts of dispersant; 0.3-1.5 parts of leveling agent; 0.4-2 parts of defoaming agent. Preferably, the auxiliary agents include: 1 part of dispersant; 0.5 parts of leveling agent; 0.5 parts of defoaming agent.
[0027] In some embodiments of the present invention, the dispersant is BYK-110 or BYK-163. The dispersant has wetting and dispersing capabilities, which affect the viscosity and fineness of the coating. Dispersant BYK-110 or BYK-163 can quickly reduce the viscosity of the base material and improve the fineness of the filler. BYK-110 is a copolymer solution containing acidic groups, which has excellent inorganic pigment dispersibility, significantly shortens the grinding and dispersion time, efficiently reduces the pigment grinding viscosity, significantly improves the grinding fluidity, has excellent color development performance and hiding power, and has excellent chroma, gloss, compatibility and wettability. The wetting dispersant BYK-163 is a polymer copolymer coating additive containing pigment affinity groups, which can increase the gloss, color intensity, transparency and hiding power of the coating, while reducing the viscosity of the abrasive.
[0028] In some embodiments of the present invention, the leveling agent is BYK-306 or BYK-333. The organosilicon leveling agent BYK-306 is a polyether-modified polyoxydimethylsiloxane solution. The leveling agent can promote the coating to form a flat, smooth and uniform coating film during the drying and film-forming process. Whether the coating can achieve a flat and smooth property is called leveling. BYK-306 or BYK-333 as a leveling agent can strongly reduce surface tension and has a very strong leveling effect.
[0029] In some embodiments of the present invention, the defoamer is BYK-141 or BYK-052. The defoamer can reduce the surface tension of the system, so that the original foam is reduced or eliminated. BYK-141 or BYK-052 is used as a defoamer to eliminate microbubbles, and has a strong defoaming function and can quickly eliminate bubbles.
[0030] In some embodiments of the present invention, the polyamide curing agent is Hansen 3115A. Polyamide curing agent is used as a curing agent for epoxy resin. Hansen 3115A curing agent is a high molecular weight, high viscosity reactive polyamide based on dimer fatty acid and polyamine, with a viscosity of 55,000-70,000 mPa.s; amine value: 232-243 mgKOH / g active hydrogen equivalent 156.
[0031] Second, as Figure 1 As shown, the present invention provides a method for preparing the anticorrosive coating for rapid curing in a high humidity environment as described in any one of the above, comprising the following steps: (1) mixing the bisphenol A epoxy resin and the solvent to disperse them; (2) adding the anti-rust pigment, the pigment, the filler and the auxiliary agent to the system obtained in step 1) and dispersing them to obtain the component A; The preparation method of component B comprises the following steps: The polyamide curing agent is taken to obtain the component B.
[0032] In the above-mentioned method for preparing an anticorrosive coating for rapid curing in a high-humidity environment, in step (1), in the dispersion step, the temperature is maintained at ≤ 50° C., and the dispersion is performed at 1000 to 2000 rpm (e.g., 1500 rpm) for 30 minutes; In step (2), in the dispersion step, the temperature is maintained at ≤50°C, and the dispersion or sand milling is performed at 1000 to 2000 rpm (e.g., 1500 rpm) for 30 minutes to 1 hour; The method further comprises the following steps in step (2): cooling the dispersed system to 40° C. and stirring evenly.
[0033] In a third aspect, the present invention provides a metal corrosion protection method, comprising the following steps: Component A and component B of the above-mentioned anti-corrosion coating for rapid curing in high humidity environment are mixed evenly, and coated on the metal surface for curing.
[0034] In some embodiments of the present invention, the curing is performed in a high humidity environment with a humidity ≥ 80% RH, such as 80% RH.
[0035] The present invention is further described in detail below in conjunction with specific embodiments, and the examples provided are only for illustrating the present invention, rather than for limiting the scope of the present invention. The examples provided below can be used as a guide for further improvements by those of ordinary skill in the art, and do not constitute a limitation of the present invention in any way.
[0036] The methods used in the following examples, unless otherwise specified, are all conventional methods, carried out according to the techniques or conditions described in the literature in the art or according to the product instructions. The materials, reagents, etc. used in the following examples, unless otherwise specified, can all be obtained from commercial sources.
[0037] The epoxy resin in the following examples is Hansen 828, Hansen; liquid epoxy resin, the viscosity (mpa·s) at 5°C is 12000-14000, and the epoxy equivalent is 184-190 g / ep.; The curing agent LS-D107 in Comparative Example 1 is from Hubei Green Home Material Technology Co., Ltd.; type: modified aromatic amine; viscosity: 4000-7000 mpa.s; amine value: 140-180 mgKOH / g; active hydrogen equivalent: 190; The curing agent in the embodiment is Hansen 3115A, Hansen; type: polyamide; viscosity: 55,000-70,000 mPa.s; amine value: 232-243 mgKOH / g active hydrogen equivalent 156.
[0038] The dispersant BYK-110, the leveling agent BYK-306 and the defoaming agent BYK-141 in the examples are all products of BYK of Germany.
[0039] Example 1 1. Formula The anticorrosive coating of this embodiment for rapid curing in a high humidity environment is composed of the following components in parts by weight: Epoxy resin [Hansen 828] 25 parts; Solvent [xylene and n-butanol in a mass ratio of 3:1] 18.3 parts; Anti-rust pigment [zinc phosphate] 15 parts; Pigment [Titanium dioxide (Chemours R706)] 10 parts Filler [talc 1250 mesh] 20 parts; Filler [barium sulfate 1250 mesh] 10 parts; Dispersant [BYK-110] 1 part; Leveling agent [BYK-306] 0.5 parts; Defoaming agent [BYK-141] 0.5 parts.
[0040] Component B: Curing agent [modified amine curing agent Hansen 3115A] 10 parts; 2. Preparation method The preparation method of component A comprises the following steps: Step 1: Add epoxy resin and solvent into the reaction kettle, stir evenly, control the temperature to ≤50°C, and disperse at high speed at 1500 rpm for 30 minutes; Step 2: Add anti-rust pigment, filler and additive to the mixed system obtained in step 1, stir evenly, continue to control the temperature ≤ 50°C, disperse at high speed at 1500 rpm for 1 hour, cool to 40°C, stir evenly, and obtain component A.
[0041] The preparation method of component B comprises the following steps: Take the curing agent to obtain component B.
[0042] Example 2 The anticorrosive coating of this embodiment for rapid curing in a high humidity environment is composed of the following components in parts by weight: Epoxy resin [Hansen 828] 20 parts; Solvent [xylene and n-butanol in a mass ratio of 3:1] 18.3 parts; Anti-rust pigment [zinc phosphate] 15 parts; Pigment [titanium dioxide (Chemours R706)] 10 parts; Filler [talc 1250 mesh] 20 parts; Filler [barium sulfate 1250 mesh] 15 parts; Dispersant [BYK-110] 1 part; Leveling agent [BYK-306] 0.3 parts; Defoaming agent [BYK-141] 0.4 parts.
[0043] Component B: Curing agent [modified amine curing agent Hansen 3115A] 8 parts; The preparation method is the same as that of Example 1.
[0044] Example 3 Epoxy resin [Hansen 828] 30 parts; Solvent [xylene and n-butanol in a mass ratio of 3:1] 18.3 parts; Anti-rust pigment [zinc phosphate] 15 parts; Pigment [titanium dioxide (Chemours R706)] 10 parts; Filler [talc 1250 mesh] 15 parts; Filler [barium sulfate 1250 mesh] 10 parts; Dispersant [BYK-110] 1 part; Leveling agent [BYK-306] 0.3 parts; Defoaming agent [BYK-141] 0.4 parts.
[0045] Component B: Curing agent [modified amine curing agent Hansen 3115A] 12 parts; The preparation method is the same as that of Example 1.
[0046] Comparative Example 1 A traditional domestic aromatic amine curing agent LS-D107 was used, and other components and preparation methods were the same as those in Example 1.
[0047] Comparative Example 2 No anti-rust pigment was added, and other components and preparation methods were the same as in Example 1.
[0048] Comparative Example 3 The anti-rust pigment was replaced with aluminum zinc phosphate, and the other components and preparation method were the same as in Example 1.
[0049] Comparative Example 4 The anti-rust pigment was replaced by modified zinc phosphate, and the other components and preparation method were the same as in Example 1.
[0050] Comparative Example 5 The 1250 mesh barium sulfate in the filler was replaced with 1250 mesh calcium carbonate, and the other components and preparation method were the same as in Example 1.
[0051] Comparative Example 6 The 1250 mesh talc in the filler was replaced with 1250 mesh calcium carbonate, and the other components and preparation method were the same as in Example 1.
[0052] Comparative Example 7 No auxiliary agent was added, and other components and preparation methods were the same as in Example 1.
[0053] Test Case The performance of the anti-corrosion coating prepared in the above examples was tested, and the results are shown in Table 1.
[0054] Component A and component B in the above Examples 1-3 and Comparative Examples 1-7 were mixed in proportion and tested. The curing and testing were carried out at room temperature (25°C) and a humidity of 80% RH. The testing method was as follows: Adhesion: GB / T 5210; Salt spray resistance: GB / T 1771; Flexibility: GB / T 1731; Impact resistance: GB / T 1732; Water resistance: GB / T 1733; Fineness: GB / T 1724; Leveling: JB / T3998; Surface drying time: GB / T 1728; Drying time: GB / T 1728; Bubbles: visual inspection.
[0055] Table 1 Test results of fast curing anticorrosive coatings in high humidity environment
[0056] Table 2 Test results of fast curing anticorrosive coatings in high humidity environment
[0057] It can be seen from Examples 1-3 that the anticorrosive coating for rapid curing in a high humidity environment of the present invention has a fineness of 60 μm, a surface drying time of less than 1.5 h, a solid drying time of less than 24 h, a leveling property ≥ 8, no bubbles, an adhesion ≥ 10 MPA, a salt spray resistance ≥ 1000 h, an impact resistance of 50 cm, a flexibility of 1 mm, and a water resistance ≥ 720 h, and all performance indicators meet the relevant requirements. It can be seen that the anticorrosive coating of the present invention has a short curing time in a high humidity environment, strong adhesion, a long salt spray resistance time, and good anticorrosion performance.
[0058] It can be seen from Example 1 and Comparative Example 1 that the type of curing agent not only affects the actual drying time, but also affects bubbles, adhesion and salt spray resistance. The present invention preferably uses the modified amine curing agent Hansen 3115A.
[0059] It can be seen from Example 1 and Comparative Examples 2-4 that the addition of the anti-rust pigment and the type of the anti-rust pigment in the present invention will affect the actual drying time, leveling, adhesion and salt spray resistance of the anti-corrosion coating. The anti-rust pigment of the present invention is preferably zinc phosphate.
[0060] It can be seen from Example 1 and Comparative Examples 5-6 that the type of filler in the present invention will affect the surface drying time, actual drying time, leveling, adhesion and salt spray resistance of the anti-corrosion coating. The filler in the present invention is preferably a combination of talc and barium sulfate.
[0061] It can be seen from Example 1 and Comparative Example 7 that the addition of the auxiliary agent in the present invention is more conducive to shortening the surface drying time and the actual drying time, improving the leveling property, eliminating bubbles, and improving the adhesion and salt spray resistance.
[0062] The present invention has been described in detail above. For those skilled in the art, without departing from the purpose and scope of the present invention, can implement the present invention in a wider range under equivalent parameters, concentrations and conditions. Although the present invention provides specific embodiments, it should be understood that the present invention can be further improved. In a word, according to the principle of the present invention, the application is intended to include any changes, uses or improvements to the present invention, including departing from the disclosed scope in the application and the changes made with conventional techniques known in the art.
Claims
1. An anticorrosive coating for rapid curing in a high humidity environment, characterized in that: Including independently packaged component A and component B, the composition of each component is as follows in parts by weight: Component A: 20-40 parts of bisphenol A epoxy resin; 10-20 parts of solvent; 10-20 parts of anti-rust pigment; Pigment 5-10 parts; Filler 10-40 parts; 1 to 5 parts of additives; Component B: Polyamide curing agent 8 to 12 parts.
2. The anticorrosive coating for rapid curing in high humidity environment according to claim 1, characterized in that: The bisphenol A epoxy resin is Hexion 828.
3. The anticorrosive coating for rapid curing in high humidity environment according to any one of claims 1-2, characterized in that: The solvent is a mixture of xylene and n-butanol, preferably a mixture of xylene and n-butanol in a mass ratio of 3:1; The anti-rust pigment is zinc phosphate; The pigment is titanium dioxide; The filler is talc and barium sulfate, preferably talc and barium sulfate in a weight ratio of 15: (10-20); The particle size of the filler is 1000-2500 meshes.
4. The anticorrosive coating for rapid curing in high humidity environment according to any one of claims 1 to 3, characterized in that: In parts by weight, the 1 to 5 parts of auxiliary agents include the following components: Dispersant 0.3-1.5 parts; 0.3-1.5 parts of leveling agent; 0.4 to 2 parts of defoaming agent.
5. The anticorrosive coating for rapid curing in high humidity environment according to claim 4, characterized in that: The dispersant is BYK-110 or BYK-163; The leveling agent is BYK-306 or BYK-333; The defoamer is BYK-141 or BYK-052.
6. The anticorrosive coating for rapid curing in high humidity environment according to any one of claims 1 to 5, characterized in that: The polyamide curing agent is Hansen 3115A.
7. The method for preparing the anticorrosive coating for rapid curing in high humidity environment according to any one of claims 1 to 6, comprising: The preparation method of component A comprises the following steps: (1) mixing the bisphenol A epoxy resin and the solvent to disperse them; (2) adding the anti-rust pigment, the pigment, the filler and the auxiliary agent to the system obtained in step 1) and dispersing them to obtain the component A; The preparation method of component B comprises the following steps: The polyamide curing agent is taken to obtain the component B.
8. The method for preparing the anticorrosive coating for rapid curing in high humidity environment according to claim 7, characterized in that: In step (1), in the dispersion step, the temperature is maintained at ≤50°C, and the dispersion is carried out at 1000-2000 rpm for 30 minutes; In step (2), in the dispersion step, the temperature is maintained at ≤50°C, and the mixture is stirred or sand-milled at 1000-2000 rpm for 30 minutes to 1 hour; The method further comprises the following steps in step (2): cooling the dispersed system to 40° C. and stirring evenly.
9. A metal anticorrosion method, characterized in that: The steps include: Component A and component B in the anti-corrosion coating for rapid curing in high humidity environment according to any one of claims 1 to 6 are mixed evenly, and applied on a metal surface for curing.
10. The metal anticorrosion method according to claim 9, characterized in that: The curing is carried out in a high humidity environment with a humidity of ≥80%RH.
Citation Information
Patent Citations
Low surface treatment type solventless coating, preparation method and applications thereof
CN102766393A
Low surface treatment epoxy paint and preparation method thereof
CN109321082A
Low solvent coating composition
CN114761499A
Cited By
Metal anticorrosive paint based on modified graphene and preparation method thereof
CN120349700A