Underwater construction curing coating as well as preparation method and application thereof

By using epoxy modified amine resins and polyetheramine toughening resins in underwater construction, the problems of slow curing speed and poor adhesion of underwater coatings are solved, and rapid curing and high adhesion are achieved. Protection and emergency repair of underwater projects.

CN118931322APending Publication Date: 2024-11-12MARINE CHEM RES INST CO LTD

Patent Information

Application Number
CN202411068700.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing underwater coatings have slow curing speed, poor adhesion and poor flexibility underwater, and cannot effectively protect underwater engineering equipment and facilities, resulting in short service life and safety hazards.

Method used

Epoxy modified amine resin is used as a curing agent, combined with amine accelerator and polyetheramine toughening resin, and mixing components A and components B to form a rapid curing, high adhesion and high flexibility underwater Construction of cured coatings.

Benefits of technology

It achieves rapid curing, high adhesion and excellent anticorrosion performance underwater, is suitable for underwater protection and emergency repair, and extends the service life of engineering equipment and facilities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004980164650000021
    Figure BDA0004980164650000021
  • Figure BDA0004980164650000031
    Figure BDA0004980164650000031
  • Figure BDA0004980164650000061
    Figure BDA0004980164650000061
Patent Text Reader

Abstract

The invention discloses an underwater construction curing coating as well as a preparation method and application thereof, and belongs to the technical field of underwater protective coatings. The curing coating for underwater construction comprises a component A and a component B, the component A comprises epoxy resin (I), an epoxy diluent, a pigment filler and an auxiliary agent, and the component B comprises epoxy modified amine resin, an alcohol diluent and an accelerant; wherein the epoxy modified amine resin is a reaction product of epoxy resin (II), an amine curing agent and toughened resin. The underwater construction curing coating provided by the invention has the advantages of fast curing, high adhesive force and excellent corrosion resistance, can be effectively brushed and cured underwater, and can be applied to the fields of underwater protection and underwater repair of various engineering equipment and facilities.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of underwater protective coatings, and in particular relates to an underwater construction curing coating and a preparation method and application thereof. Background Art

[0002] Engineering equipment and various facilities that have been in underwater environment for a long time are affected by water immersion and other harsh conditions, resulting in their service life being far less than the designed life, which creates certain safety hazards. Since a large number of underwater engineering structures are immovable, how to improve the durability of such engineering equipment and facilities is an important issue.

[0003] Underwater curing coating refers to a coating that can be cured underwater, and its base resin mainly includes vinyl resin, epoxy resin, etc. However, the vinyl resin system needs to add solvent, and it is not completely cured in water, and it pollutes the environment. Therefore, most of the existing underwater coatings use epoxy resin as the base resin. At present, researchers have developed some underwater epoxy coatings that can be cured underwater, but these underwater epoxy coatings still have the following problems: after underwater coating, the curing time required for the coating is long and the curing is not complete, the water between the coating and the substrate surface cannot be removed, the environmental adaptability is poor, the formed coating has poor toughness, is easy to bubble, and has poor adhesion to the substrate surface. Therefore, it is of great significance to develop a fast-curing, high-adhesion and environmentally adaptable underwater construction curing coating for underwater protection of various engineering equipment and facilities and underwater emergency repair. Summary of the invention

[0004] In order to overcome the shortcomings of existing anti-corrosion coatings, such as slow underwater curing speed, poor coating adhesion, and poor flexibility, the present invention provides an underwater construction curing coating. The underwater construction curing coating provided by the present invention has the characteristics of rapid curing, high adhesion, and heavy anti-corrosion.

[0005] One of the purposes of the present invention is to provide an underwater construction curing coating, comprising component A and component B, wherein the component A comprises epoxy resin (I), epoxy diluent, pigments and fillers, and additives, and the component B comprises epoxy-modified amine resin, alcohol diluent, and accelerator; wherein the epoxy-modified amine resin is the reaction product of epoxy resin (II), amine curing agent, and toughening resin.

[0006] In the underwater construction curing coating provided by the present invention:

[0007] The A component includes the following components in parts by weight:

[0008]

[0009] The B component includes the following components in parts by weight:

[0010] 40-80 parts of epoxy-modified amine resin, preferably 55-65 parts;

[0011] 20 to 50 parts of alcohol diluent, preferably 35 to 45 parts;

[0012] The amount of accelerator is 1 to 10 parts, preferably 2 to 5 parts.

[0013] In the underwater construction curing coating provided by the present invention:

[0014] The epoxy resin (I) is at least one selected from bisphenol A epoxy resin (bisphenol A epoxy resin E-12, bisphenol A epoxy resin E-20, bisphenol A epoxy resin E-51, bisphenol A epoxy resin E-44, etc.), novolac epoxy resin (novolac epoxy resin F-51, novolac epoxy resin F-44, novolac epoxy resin F-48, etc.), bisphenol F epoxy resin (NPEF-170 resin), and hyperbranched epoxy resin;

[0015] The epoxy diluent is selected from at least one of glycidyl ether compounds, preferably at least one of C12-14 alkyl glycidyl ether, phenyl glycidyl ether, 1,4-cyclohexanedimethanol diglycidyl ether, trimethylolpropane triglycidyl ether, neopentyl glycol diglycidyl ether, and o-cresyl glycidyl ether;

[0016] The pigment filler is at least one of magnesium carbonate, talc, mica powder, precipitated barium sulfate, wollastonite, silicon carbide, silicon micropowder, light calcium carbonate, titanium dioxide, red iron oxide, aluminum oxide, zinc oxide, and calcium oxide;

[0017] The auxiliary agent is selected from at least one of a wetting and dispersing agent, a leveling agent, a thixotropic agent, a defoaming agent, and a toughening agent; the auxiliary agent can be an auxiliary agent component commonly used in the art, for example, at least one of the wetting and dispersing agents BYK-P2710, BYK-P104S, BYK-9076, and MOK-5012, the leveling agent is selected from at least one of BYK-361N, BYK-342, and Deqian 837, the thixotropic agent is selected from at least one of polyamide wax, fumed silica, and organic bentonite, the defoaming agent is selected from at least one of BYK-085 and BYK-066N, and the toughening agent is selected from at least one of polyetheramine A450 and D-230;

[0018] The alcohol diluent is selected from at least one of monohydric alcohol and polyhydric alcohol, preferably at least one of glycerol, benzyl alcohol, methanol, ethanol and ethylene glycol;

[0019] The accelerator is selected from at least one of amino compound accelerators, preferably at least one of 2,4,6-tris(dimethylaminomethyl)phenol (K54, DMP-30), N,N-dimethylaniline, triethylamine, 4-methylimidazole, and 2-methyl-4-ethylimidazole.

[0020] According to the present invention, the epoxy-modified amine resin is prepared by the following method: adding an amine curing agent to a solvent to dissolve, adding epoxy resin (II) to react, and then adding a toughening resin to react to obtain the epoxy-modified amine resin. The reaction mechanism of the amino hydrogen and epoxy groups of the amine curing agent is as follows:

[0021]

[0022] The amine curing agent is selected from at least one of 4,4',4",4"'-methanetetrayltetraphenylamine, 4,4,4"-triaminotriphenylmethane, meta-phenylenediamine, 4,4'-diaminodiphenylmethane, 4,4'-diaminodicyclohexylmethane, oleylamine, polyamide (polyamide 650, polyamide 651), phenolic amine (phenolic amine 810, phenolic amine 910, phenolic amine T31, phenolic amine T33 and phenolic amine T316), ethylenediamine, polyethylene polyamine (diethylenetriamine, triethylenetetramine, tetraethylenepentamine), hexamethylenediamine, amine compounds containing alicyclic rings (for example, cyclohexyl, heterocyclic oxygen, nitrogen atom hexacyclic ring, etc.), meta-phenylenediamine, meta-phenylenediamine, and 4,4'-diaminodiphenyl sulfone (DDS), preferably at least one of 4,4,4"-triaminotriphenylmethane and 4,4'-diaminodiphenylmethane;

[0023] The solvent is selected from alcohol solvents, preferably at least one selected from glycerol, benzyl alcohol, methanol, ethanol, and ethylene glycol;

[0024] The epoxy resin (II) is selected from at least one of bisphenol A epoxy resin (bisphenol A epoxy resin E-12, bisphenol A epoxy resin E-20, bisphenol A epoxy resin E-51, bisphenol A epoxy resin E-44), novolac epoxy resin (novolac epoxy resin F-51, novolac epoxy resin F-44, novolac epoxy resin F-48), bisphenol F epoxy resin (NPEF-170 resin), and hyperbranched epoxy resin;

[0025] The toughening resin is a polyetheramine (one or more of Huntsman's RP-400, RP-2000, RT-1000, and RP3-5000);

[0026] The mass ratio of the amine curing agent to the epoxy resin (II) is (1-10):1, preferably (2-6):1;

[0027] The mass ratio of the amine curing agent to the solvent is (0.5-2):1, preferably (0.6-1.5):1;

[0028] The mass ratio of the amine curing agent to the toughening resin is (1-20):1, preferably (5-10):1;

[0029] The dissolution can be carried out under appropriate heating conditions, for example, the dissolution temperature is 55-65°C;

[0030] The reaction conditions are 55-110° C. for 2-6 hours.

[0031] The second object of the present invention is to provide a method for preparing the underwater construction curing coating according to the first object of the present invention, comprising:

[0032] (1) mixing epoxy resin (I), epoxy diluent, pigment, filler and additive to obtain component A;

[0033] (2) mixing epoxy-modified amine resin, alcohol diluent, and accelerator to obtain component B;

[0034] (3) Mix component A and component B to obtain the underwater construction curing coating.

[0035] According to the present invention, in the method for preparing the underwater construction curing coating, the mass ratio of the component A to the component B is 100:(15-35), preferably 100:(20-30).

[0036] The third object of the present invention is to provide the underwater construction curing coating described in the first object of the present invention or the underwater construction curing coating obtained by the preparation method described in the second object of the present invention, and its application in underwater protection and emergency repair.

[0037] The present invention adopts epoxy-modified amine resin as a curing agent, utilizes the characteristics of amine curing agent being easy to cure in humid, underwater and other environments, introduces amine accelerator to accelerate the crosslinking between epoxy resin and curing agent by catalyzing the epoxy group of epoxy resin, and finally introduces polyetheramine toughening resin to increase the flexibility of paint film and reduce the difficulty of underwater construction of coating. Therefore, the underwater construction curing coating provided by the present invention has fast curing, high adhesion and excellent anti-corrosion performance, can be effectively brushed and cured underwater, and can be applied to the underwater protection and underwater emergency repair fields of various engineering equipment and facilities. DETAILED DESCRIPTION

[0038] The present invention is described in detail below in conjunction with specific embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the contents of the present invention still fall within the scope of protection of the present invention.

[0039] The test instruments and test conditions used in the examples are as follows:

[0040] Adhesion: Tested according to GB / T 5210-2006 paint and varnish pull-off adhesion test;

[0041] Flexibility: Tested according to GB / T 1731-1993 paint film flexibility determination method.

[0042] Water resistance: tested according to GB / T 1733-1993 method for determining water resistance of paint films.

[0043] The raw materials used in the examples and comparative examples, unless otherwise specified, are disclosed in the prior art, for example, they can be directly purchased or prepared according to the preparation methods disclosed in the prior art.

[0044] The present invention is further described in detail below in conjunction with the examples, but the embodiments of the present invention are not limited thereto. The raw material parts in the following examples are all parts by weight.

[0045] Example 1

[0046] A method for preparing an underwater construction curing coating comprises the following steps:

[0047] (1) Add 35 parts of benzyl alcohol to 50 parts of 4,4'-diaminodiphenylmethane (DDM), heat to 60°C, add 10 parts of epoxy resin E51 after DDM is dissolved, reduce the purity of the amine curing agent, and thus reduce its crystallization probability. After the epoxy resin reacts completely, keep it at 110°C for 4 hours, and finally add 5 parts of toughening resin (polyetheramine A-450) to react for 20 minutes to obtain epoxy-modified amine resin. The reaction mechanism of DDM and epoxy group is as follows;

[0048]

[0049] (2) 50 parts by weight of bisphenol A epoxy resin E-51, 7 parts by weight of phenyl glycidyl ether, 35 parts by weight of silica powder, 6 parts by weight of titanium dioxide, 1.8 parts by weight of thixotropic agent SD-2, and 0.2 parts by weight of BYK-066N were mixed to obtain component A;

[0050] (3) 60 parts by weight of epoxy-modified amine resin, 38 parts by weight of benzyl alcohol and 2 parts by weight of 2,4,6-tris(dimethylaminomethyl)phenol were uniformly mixed to obtain component B;

[0051] (4) When in use, component A and component B are stirred and mixed in a weight ratio of 100:25 to obtain an underwater construction curing coating.

[0052] Example 2

[0053] (1) Benzyl alcohol and methanol are mixed in a ratio of 2:1, 35 parts of the benzyl alcohol / methanol mixed solvent are added to 50 parts of 4,4'-diaminodiphenylmethane, the temperature is raised to 60°C, and after the 4,4'-diaminodiphenylmethane is dissolved, 10 parts of bisphenol F epoxy resin EF-170 are added. After the epoxy resin reacts completely, the temperature is kept at 110°C for 4 hours, and finally 5 parts of toughening resin (polyetheramine A-450) are added to obtain epoxy-modified amine resin;

[0054] (2) 50 parts by weight of bisphenol A epoxy resin E-44, 5 parts by weight of phenyl glycidyl ether, 35 parts by weight of silicon powder, 7.8 parts by weight of titanium dioxide, 2 parts by weight of thixotropic agent SD-2, and 0.2 parts by weight of BYK-066N were mixed uniformly to obtain component A;

[0055] (3) 60 parts by weight of epoxy-modified amine resin, 38 parts by weight of a mixture of benzyl alcohol and methanol (the mass ratio of benzyl alcohol to methanol is 1:1), and 2 parts by weight of 2,4,6-tris(dimethylaminomethyl)phenol were uniformly mixed to obtain component B;

[0056] (4) When in use, component A and component B are stirred and mixed in a weight ratio of 100:20 to obtain an underwater construction curing coating.

[0057] Example 3

[0058] (1) Add 35 parts of benzyl alcohol solvent to 25 parts of 4,4'-diaminodiphenylmethane and 25 parts of 4,4'-diaminodicyclohexylmethane, raise the temperature to 60°C, and add 10 parts of bisphenol A epoxy resin E51 after 4,4'-diaminodiphenylmethane and 4,4'-diaminodicyclohexylmethane are dissolved. After the reaction of E51 is complete, keep the temperature at 110°C for 4 hours, and finally add 5 parts of toughening resin (polyetheramine A-450) to obtain epoxy modified amine resin;

[0059] (2) 25 parts by weight of bisphenol A epoxy resin E-44, 25 parts by weight of bisphenol A epoxy resin E-51, 5 parts by weight of phenyl glycidyl ether, 35 parts by weight of silica powder, 6 parts by weight of titanium dioxide, 2 parts by weight of thixotropic agent SD-2, and 2 parts by weight of BYK-066N were mixed uniformly to obtain component A;

[0060] (3) 60 parts by weight of epoxy-modified amine resin, 38 parts by weight of benzyl alcohol and 2 parts by weight of 2,4,6-tris(dimethylaminomethyl)phenol were uniformly mixed to obtain component B;

[0061] (4) When in use, component A and component B are stirred and mixed in a weight ratio of 100:30 to obtain an underwater construction curing coating.

[0062] Example 4

[0063] (1) Add 35 parts of benzyl alcohol solvent to 50 parts of modified phenolic amine BS6305, stir thoroughly, and after the modified phenolic amine is dissolved and mixed evenly with the benzyl alcohol, add 10 parts of bisphenol A epoxy resin E51. After the reaction is complete at room temperature for 1 hour, add 5 parts of toughening resin (polyetheramine A-450) to obtain epoxy modified amine resin;

[0064] (2) 25 parts by weight of bisphenol A epoxy resin E-44, 25 parts by weight of bisphenol A epoxy resin E-51, 5 parts by weight of phenyl glycidyl ether, 36.8 parts by weight of silica powder, 6 parts by weight of titanium dioxide, 2 parts by weight of thixotropic agent SD-2, and 0.2 parts by weight of BYK-066N were mixed uniformly to obtain component A;

[0065] (3) 60 parts by weight of epoxy-modified amine resin, 38 parts by weight of a mixture of benzyl alcohol and methanol (the mass ratio of benzyl alcohol to methanol is 1:1), and 2 parts by weight of 2,4,6-tris(dimethylaminomethyl)phenol were uniformly mixed to obtain component B;

[0066] (4) When in use, component A and component B are stirred and mixed in a weight ratio of 100:23 to obtain an underwater construction curing coating.

[0067] Comparative Example 1

[0068] (1) 35 parts by weight of bisphenol A epoxy resin E-44, 15 parts by weight of bisphenol A epoxy resin E-51, 5 parts by weight of phenyl glycidyl ether, 35 parts by weight of silica powder, 6 parts by weight of titanium dioxide, 2 parts by weight of thixotropic agent SD-2, and 0.2 parts by weight of BYK-066N were mixed uniformly to obtain component A;

[0069] (2) 60 parts by weight of an amine resin and 40 parts by weight of benzyl alcohol are uniformly mixed to obtain a component B;

[0070] (3) When in use, component A and component B are stirred and mixed in a weight ratio of 100:20 to obtain an underwater construction curing coating.

[0071] Table 1 shows the coating performance test results obtained in Examples 1 to 4 and Comparative Example 5.

[0072] Table 1

[0073]

[0074] As can be seen from Table 1, the underwater construction curing coating of the present invention has good flexibility of the paint film, which can reach up to 8mm due to the addition of toughening resin (polyetheramine). By selecting a unique epoxy-modified amine resin as a curing agent, the coating can be rapidly cured underwater. Since the A and B components are highly cross-linked after mixing, the adhesion of the coating underwater can reach a minimum of 4.0MPa and a maximum of 5.6MPa, and both have excellent water resistance. The underwater construction curing coating of the present invention has the characteristic of rapid underwater curing, and a high-performance protective coating can be obtained after underwater construction curing.

[0075] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. An underwater construction curing coating, comprising component A and component B, wherein the component A comprises epoxy resin (I), epoxy diluent, pigment, filler, and additive, and the component B comprises epoxy-modified amine resin, alcohol diluent, and accelerator; wherein: The epoxy-modified amine resin is a reaction product of epoxy resin (II), amine curing agent and toughening resin.

2. The underwater construction curing coating according to claim 1, characterized in that: The A component includes the following components in parts by weight: The B component includes the following components in parts by weight: 40-80 parts of epoxy-modified amine resin, preferably 55-65 parts; 20 to 50 parts of alcohol diluent, preferably 35 to 45 parts; The amount of accelerator is 1 to 10 parts, preferably 2 to 5 parts.

3. The underwater construction curing coating according to claim 1 or 2, characterized in that: The epoxy resin (I) is at least one selected from bisphenol A epoxy resin, novolac epoxy resin, bisphenol F epoxy resin, and hyperbranched epoxy resin; and / or, The epoxy diluent is selected from at least one of glycidyl ether compounds, preferably at least one of C12-14 alkyl glycidyl ether, phenyl glycidyl ether, 1,4-cyclohexanedimethanol diglycidyl ether, trimethylolpropane triglycidyl ether, neopentyl glycol diglycidyl ether and o-cresyl glycidyl ether; and / or, The pigment filler is at least one of magnesium carbonate, talc, mica powder, precipitated barium sulfate, wollastonite, silicon carbide, silicon powder, light calcium carbonate, titanium dioxide, red iron oxide, aluminum oxide, zinc oxide, and calcium oxide; and / or, The auxiliary agent is selected from at least one of a wetting and dispersing agent, a leveling agent, a thixotropic agent, a defoaming agent, and a toughening agent; and / or, The alcohol diluent is selected from at least one of monohydric alcohol and polyhydric alcohol, preferably at least one of glycerol, benzyl alcohol, methanol, ethanol and ethylene glycol; and / or, The accelerator is selected from at least one of amino compound accelerators, preferably at least one of 2,4,6-tris(dimethylaminomethyl)phenol, N,N-dimethylaniline, triethylamine, 4-methylimidazole, and 2-methyl-4-ethylimidazole.

4. The underwater construction curing coating according to claim 1 or 2, characterized in that: The epoxy-modified amine resin is prepared by the following method: adding an amine curing agent into a solvent to dissolve it, adding epoxy resin (II) to react, and then adding a toughening resin to react to obtain the epoxy-modified amine resin.

5. The underwater construction curing coating according to claim 4, characterized in that: The amine curing agent is selected from at least one of 4,4',4",4'-methanetetrayltetraphenylamine, 4,4,4"-triaminotriphenylmethane, meta-phenylenediamine, 4,4'-diaminodiphenylmethane, 4,4'-diaminodicyclohexylmethane, oleylamine, polyamide, phenolic amine, ethylenediamine, polyethylene polyamine, hexamethylenediamine, alicyclic amine compounds, meta-phenylenediamine, meta-phenylenediamine, 4,4'-diaminodiphenyl sulfone, preferably at least one of 4,4,4"-triaminotriphenylmethane and 4,4'-diaminodiphenylmethane; and / or, The solvent is selected from alcohol solvents, preferably at least one selected from glycerol, benzyl alcohol, methanol, ethanol, and ethylene glycol; and / or, The epoxy resin (II) is at least one selected from bisphenol A epoxy resin, novolac epoxy resin, bisphenol F epoxy resin, and hyperbranched epoxy resin; and / or, The toughening resin is polyetheramine.

6. The underwater construction curing coating according to claim 4, characterized in that: The mass ratio of the amine curing agent to the epoxy resin (II) is (1-10):1, preferably (2-6):1; and / or, The mass ratio of the amine curing agent to the solvent is (0.5-2):1, preferably (0.6-1.5):1; and / or, The mass ratio of the amine curing agent to the toughening resin is (1-20):1, preferably (5-10):

1.

7. The underwater construction curing coating according to claim 4, characterized in that: The dissolving temperature is 55-65°C; and / or, The reaction conditions are: 55-110° C. for 2-6 hours.

8. A method for preparing the underwater construction curing coating according to any one of claims 1 to 7, comprising: (1) mixing epoxy resin (I), epoxy diluent, pigment, filler and additive to obtain component A; (2) mixing epoxy-modified amine resin, alcohol diluent, and accelerator to obtain component B; (3) Mix component A and component B to obtain the underwater construction curing coating.

9. The preparation method according to claim 8, characterized in that: The mass ratio of the component A to the component B is 100:(15-35), preferably 100:(20-30).

10. Use of the underwater construction curing coating according to any one of claims 1 to 7 or the underwater construction curing coating obtained by the preparation method according to any one of claims 8 to 9 in underwater protection and emergency repair.

Citation Information

Patent Citations

  • Epoxy anti-corrosive paint for underwater construction and preparation method

    CN101311233A

  • Underwater curable coating, underwater protective layer and application thereof

    CN104745046A

  • Preparation method of underwater curing agent

    CN105694002A

  • Underwater concrete flexible epoxy anticorrosion paint and preparation method thereof

    CN108676457A

  • Underwater construction curing coating as well as preparation method and application thereof

    CN115124906A

Cited By

  • Deep-sea pressure-resistant self-stratification solventless coating and preparation method thereof

    CN119899576A

  • A deep-sea pressure-resistant self-layering solvent-free coating and a preparation method thereof

    CN119899576B