A green, environmentally friendly, heat-resistant photovoltaic cable

By using annealed soft fine copper tow stranded and crosslinked polyolefin insulating materials in photovoltaic cables, combined with irradiated crosslinked polyolefin anti-corrosion protective sleeves, the problem of insufficient performance of existing cables in the cosmic and space environment is solved, and the problem of insufficient performance of existing cables in the universe and space environment is achieved. It has high environmentally friendly heat resistance and corrosion resistance, and meets the multiple needs of modern photovoltaic power generation and aerospace technology.

CN118609899BActive Publication Date: 2024-12-03广东坚宝电缆有限公司
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411082432.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-12-03
Estimated Expiration
2044-08-08

AI Technical Summary

Technical Problem

The existing cables for photovoltaic power generation cannot meet the special needs of modern photovoltaic power generation and aerospace technology, such as flame retardant, temperature resistance, oil resistance, waterproof, acid and alkali resistance, salt spray resistance, scratch resistance, and torsion resistance, especially in the space environment of the universe. Inadequate when used.

Method used

A stranded soft conductor formed by annealed soft and fine copper wire tow strands, combined with crosslinked polyolefin insulating material and irradiated crosslinked polyolefin anti-corrosion protective cover layer, forming a green and environmentally friendly with good flame retardant, heat resistance and corrosion resistance. Heat-resistant photovoltaic cable.

Benefits of technology

It realizes a high environmentally friendly protective layer of the cable, improves the mechanical properties and thermal oxygen aging resistance of the cable, meets the multiple needs of modern photovoltaic power generation and aerospace technology, and has broad market prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118609899B_ABST
    Figure CN118609899B_ABST
Patent Text Reader

Abstract

The invention provides a green, environment-friendly, heat-resistant photovoltaic cable, comprising a twisted soft conductor, a red heat-resistant insulating layer, a black heat-resistant insulating layer and an anti-corrosion protective sheath; the twisted soft conductor is formed by twisting annealed soft fine copper wires; the red heat-resistant insulating layer and the black heat-resistant insulating layer are cross-linked polyolefin insulating materials; the anti-corrosion protective sheath is an irradiable cross-linked polyolefin anti-corrosion protective sheath material; the thickness of the red heat-resistant insulating layer is 1-1.15 times the diameter of the twisted soft conductor; the thickness of the black heat-resistant insulating layer is 4-5 times the diameter of the twisted soft conductor; the photovoltaic cable has good flame retardancy, heat resistance, aging resistance and other properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of cable preparation, and specifically relates to a green, environment-friendly, heat-resistant photovoltaic cable. Background Art

[0002] Solar photovoltaic power generation, as a natural resource for sustainable development of green energy, has received more and more attention and importance from the international community. All countries have invested a lot of money in solar photovoltaic power generation and developed and researched comprehensive supporting social applications of photovoltaic power generation. According to industry experts, by 2030, the comprehensive utilization rate of photovoltaic new energy power generation in my country will reach more than 20%, and by 2040, solar power generation in my country will account for more than 50%. The above figures fully demonstrate the development prospects of the solar photovoltaic power generation industry and its important strategic position in the energy field.

[0003] Existing photovoltaic power generation cable products can no longer meet the needs of modern photovoltaic power generation and modern aerospace technology because traditional materials are affected by the research and development of domestic new materials technology and the international trade war. The flame retardancy, temperature resistance, oil resistance, waterproofness, acid and alkali resistance, salt spray resistance, scratch resistance, and torsion resistance required for photovoltaic power generation are many special effects. As we all know, the electric energy used by my country's space station comes from photovoltaic power generation technology; due to the vast universe, photovoltaic panels can continuously receive the light energy emitted by the sun, complete energy conversion, and meet the electricity needs of the space station.

[0004] Therefore, it is of practical significance to develop green, environmentally friendly and heat-resistant photovoltaic cables. In addition to being green and environmentally friendly, this cable can also meet the many special functions required for photovoltaic power generation, such as flame retardancy, temperature resistance, oil resistance, and corrosion resistance. It is a must-have for modern photovoltaic power generation and has broad market prospects. Summary of the invention

[0005] The purpose of the present invention is to provide a green, environmentally friendly, heat-resistant photovoltaic cable, which is composed of a stranded soft conductor 1 formed by stranding annealed soft fine copper wires, a red heat-resistant insulating layer 2 and a black heat-resistant insulating layer 3 made of cross-linked polyolefin insulating material, and an anti-corrosion protective sheath 4 made of irradiable cross-linked polyolefin, to achieve a photovoltaic cable with good flame retardant, heat-resistant and corrosion-resistant properties.

[0006] In order to achieve the above object, the present invention provides the following technical solutions:

[0007] A green, environment-friendly, heat-resistant photovoltaic cable comprises a twisted soft conductor 1, a red heat-resistant insulating layer 2, a black heat-resistant insulating layer 3 and an anti-corrosion protective sheath 4; the twisted soft conductor 1 is formed by twisting annealed soft fine copper wires; the red heat-resistant insulating layer 2 is coated on the outside of the twisted soft conductor 1 to form a red heat-resistant assembly; the black heat-resistant insulating layer 3 is coated on the outside of the twisted soft conductor 1 to form a black heat-resistant assembly; the red heat-resistant assembly and the black heat-resistant assembly are arranged in parallel, and are coated with an anti-corrosion protective sheath 4 on the outside.

[0008] Furthermore, the red heat-resistant insulating layer 2 and the black heat-resistant insulating layer 3 are cross-linked polyolefin insulating materials; the thickness of the red heat-resistant insulating layer 2 and the black heat-resistant insulating layer 3 is 1-1.15 times the diameter of the bundled soft conductor 1.

[0009] Furthermore, the anti-corrosion protective sheath layer 4 is made of a radiation cross-linkable polyolefin anti-corrosion protective sheath material, and the thickness of the anti-corrosion protective sheath layer 4 is 4-5 times the diameter of the bundled soft conductor 1.

[0010] Furthermore, the preparation process of the cross-linked polyolefin insulation material is as follows: by weight, 40-80 parts of linear low-density polyethylene, 12-18 parts of nonylphenol dichloride disulfide copolymer, 3-6 parts of organic montmorillonite, 1-3 parts of zinc borate and 1.5-3.5 parts of 2,2'-methylenebis(4-tert-octyl-6-benzotriazolephenol) are mixed, and reacted at a temperature of 160-200°C for 4-6h; then 2-5 parts of tert-butyl isopropyl peroxide and 3-6 parts of silane coupling agent KH570 are added thereto, and the mixture is reacted at a temperature of 100-120°C for 2-4h to obtain a cross-linked polyolefin insulation material.

[0011] Furthermore, the preparation process of the cross-linked polyolefin insulation material is optimized as follows: in parts by weight, 60 parts of linear low-density polyethylene, 15 parts of nonylphenol dichloride disulfide copolymer, 5 parts of organic montmorillonite, 2 parts of zinc borate and 2 parts of 2,2'-methylenebis(4-tert-octyl-6-benzotriazolephenol) are mixed, and reacted at a temperature of 180°C for 5.5 hours; then 4 parts of tert-butyl isopropyl peroxide and 5 parts of silane coupling agent KH570 are added thereto, and the mixture is reacted at a temperature of 110°C for 3 hours to obtain a cross-linked polyolefin insulation material.

[0012] Furthermore, the preparation process of the radiation cross-linkable polyolefin anticorrosive protective sleeve material is as follows: by weight, 30-50 parts of ethylene-octene copolymer, 20-40 parts of ethylene vinyl acetate resin, 3-8 parts of triallyl isocyanate, 1-3 parts of triphenyl triazine, 2-5 parts of sodium dehydroacetate and 1-4 parts of potassium sorbate are mixed, and mixed in a closed mixer at a temperature of 175-195° C. for 12-18 minutes; then, the mixture is put into a twin-screw extruder with four temperature sections for granulation to obtain an anticorrosive protective sleeve layer.

[0013] Furthermore, the preparation process of the radiation cross-linkable polyolefin anti-corrosion protective sleeve material is optimized as follows: 45 parts of ethylene-octene copolymer, 35 parts of ethylene vinyl acetate resin, 6 parts of triallyl isocyanate, 2 parts of triphenyl triazine, 4 parts of sodium dehydroacetate and 3 parts of potassium sorbate are mixed by weight, and mixed in a closed mixer at a temperature of 190°C for 15 minutes; then put into a twin-screw extruder with four temperature sections for extrusion to obtain an anti-corrosion protective sleeve layer.

[0014] Furthermore, the temperatures of the twin-screw extruder in the four temperature sections are 150°C, 160°C, 175°C, and 185°C, respectively.

[0015] The preparation method of the above-mentioned green, environmentally friendly, heat-resistant photovoltaic cable is as follows: first, annealed soft and fine copper wire bundles are twisted into a twisted soft conductor 1; a red heat-resistant insulating layer 2 is coated on the outside of the twisted soft conductor 1 to form a red heat-resistant assembly; a black heat-resistant insulating layer 3 is coated on the outside of the twisted soft conductor 1 to form a black heat-resistant assembly; the red heat-resistant assembly and the black heat-resistant assembly are arranged in parallel, and are coated with an anti-corrosion protective sheath 4 on the outside, and are cross-linked by irradiation to obtain a green, environmentally friendly, heat-resistant photovoltaic cable.

[0016] Furthermore, the irradiation process parameters are: beam pressure 1-1.3 MeV, beam current 70-90 mA, dose 40-60 kGy, speed 500-600 m / min.

[0017] Compared with the prior art, the advantages and beneficial effects of the present invention are:

[0018] 1. The green, environment-friendly, heat-resistant photovoltaic cable of the present invention is made of annealed soft and fine copper wire bundles twisted into a soft bundle twisted soft copper conductor with the function of carrying large current overload and good cutting flexibility. The cross-linked polyolefin insulation material is used as the heat-resistant insulation layer, and the irradiable cross-linked polyolefin anti-corrosion protective sheath material is used as the anti-corrosion protective sheath. The molecular structure of the heat-resistant insulation layer and the anti-corrosion protective sheath is changed by irradiation cross-linking, and a mesh-like layer-by-layer reinforcement structure is formed to form a highly environmentally friendly protective layer.

[0019] 2. In the preparation of the cross-linked polyolefin insulation layer, the present invention uses low-density polyethylene, nonylphenol disulfide dichloride copolymer and other matrices, and under the joint action of organic montmorillonite, zinc borate, tert-butyl isopropyl peroxide and silane coupling agent KH570, a cross-linked polyolefin insulation material with good cross-linking degree, good mechanical properties and good heat-oxidative aging resistance is obtained.

[0020] 3. In the preparation of the anti-corrosion protective sleeve layer, the present invention uses ethylene-octene copolymer and ethylene vinyl acetate resin as the matrix, and under the action of triallyl isocyanate, triphenyl triazine, sodium dehydroacetate and potassium sorbate, a radiation-crosslinked polyolefin anti-corrosion protective sleeve material with good anti-corrosion performance and good heat resistance is obtained. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Exemplary embodiments of the present invention will now be described, by way of non-limiting example only, and with reference to the accompanying illustrative drawings.

[0022] Figure 1 It is a stereogram of the cable of the present invention.

[0023] Figure 2 It is a cross-sectional view of the cable of the present invention.

[0024] Among them, 1-twisted soft conductor, 2-red heat-resistant insulation layer, 3-black heat-resistant insulation layer, 4-anti-corrosion protective sheath. DETAILED DESCRIPTION

[0025] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] The sources of the substances in the present invention are as follows:

[0027] Linear low-density polyethylene is produced by Dongguan Jinshixiang Plastic Raw Materials Co., Ltd. with product number LLDPE; nonylphenol dichloride disulfide copolymer is produced by Hunan Jiahang Pharmaceutical Technology Co., Ltd. with product number 1635; silane coupling agent KH570 is produced by Shanghai Yuanye Biotechnology Co., Ltd. with product number S15030; ethylene-octene copolymer is produced by Dongguan Yucheng Plastic Co., Ltd. with product number 8999; ethylene vinyl acetate resin is produced by Dongguan Yucheng Plastic Co., Ltd. with product number 3185.

[0028] Example 1

[0029] like Figure 1 and Figure 2As shown, this embodiment provides a green, environmentally friendly, heat-resistant photovoltaic cable, including a bundled twisted soft conductor 1, a red heat-resistant insulating layer 2, a black heat-resistant insulating layer 3 and an anti-corrosion protective sheath 4; the bundled twisted soft conductor 1 is formed by twisting annealed soft fine copper wires; the red heat-resistant insulating layer 2 is coated on the outside of the bundled twisted soft conductor 1 with an adhesive to form a red heat-resistant assembly; the black heat-resistant insulating layer 3 is coated on the outside of the bundled twisted soft conductor 1 with an adhesive to form a black heat-resistant assembly; the red heat-resistant insulating layer 2 and the black heat-resistant insulating layer 3 are cross-linked polyolefin insulating materials; the diameter of the bundled twisted soft conductor 1 is 1 cm; the thickness of the red heat-resistant insulating layer 2 and the black heat-resistant insulating layer 3 is 1 cm. The red heat-resistant assembly and the black heat-resistant assembly are arranged in parallel, and are coated with an anti-corrosion protective sheath 4 on the outside; the anti-corrosion protective sheath 4 is a irradiable cross-linked polyolefin anti-corrosion protective sheath material; the thickness of the anti-corrosion protective sheath 4 is 4 cm.

[0030] The preparation method of the cable comprises the following steps: firstly, annealing soft fine copper wire bundles are twisted into a twisted soft conductor 1; a red heat-resistant insulating layer 2 is coated on the outside of the twisted soft conductor 1 to form a red heat-resistant assembly; a black heat-resistant insulating layer 3 is coated on the outside of the twisted soft conductor 1 to form a black heat-resistant assembly; the red heat-resistant assembly and the black heat-resistant assembly are arranged in parallel, and are coated with an anti-corrosion protective sheath 4 on the outside, and are cross-linked by irradiation, and the irradiation process parameters are: beam voltage 1MeV, beam current 70mA, dose 40kGy, speed 500m / min; thus, a green, environmentally friendly, heat-resistant photovoltaic cable is obtained.

[0031] The preparation process of the cross-linked polyolefin insulation material is as follows: 40g of linear low-density polyethylene, 12g of nonylphenol dichloride disulfide copolymer, 3g of organic montmorillonite, 1g of zinc borate and 1.5g of 2,2'-methylenebis(4-tert-octyl-6-benzotriazolephenol) are mixed, and reacted at a temperature of 160°C for 4h; then 2g of tert-butyl isopropyl peroxide and 3g of silane coupling agent KH570 are added thereto, and the mixture is reacted at a temperature of 100°C for 2h to obtain the cross-linked polyolefin insulation material.

[0032] The preparation process of the anti-corrosion protective sleeve layer, which is a radiation cross-linkable polyolefin anti-corrosion protective sleeve material, is as follows: 30g of ethylene-octene copolymer, 20g of ethylene vinyl acetate resin, 3g of triallyl isocyanate, 1g of triphenyl triazine, 2g of sodium dehydroacetate and 1g of potassium sorbate are mixed, and mixed in a closed mixer at a temperature of 175°C for 12 minutes; then, the mixture is put into a twin-screw extruder with four temperature sections for granulation to obtain the anti-corrosion protective sleeve layer; the temperatures of the twin-screw extruder in the four temperature sections are 150°C, 160°C, 175°C and 185°C respectively.

[0033] Example 2

[0034] like Figure 1 and Figure 2As shown, this embodiment provides a green, environmentally friendly, heat-resistant photovoltaic cable, including a bundled twisted soft conductor 1, a red heat-resistant insulating layer 2, a black heat-resistant insulating layer 3 and an anti-corrosion protective sheath 4; the bundled twisted soft conductor 1 is formed by twisting annealed soft fine copper wires; the red heat-resistant insulating layer 2 is coated on the outside of the bundled twisted soft conductor 1 with an adhesive to form a red heat-resistant assembly; the black heat-resistant insulating layer 3 is coated on the outside of the bundled twisted soft conductor 1 with an adhesive to form a black heat-resistant assembly; the red heat-resistant insulating layer 2 and the black heat-resistant insulating layer 3 are cross-linked polyolefin insulation materials; the diameter of the bundled twisted soft conductor 1 is 1 cm; the thickness of the red heat-resistant insulating layer 2 and the black heat-resistant insulating layer 3 is 1.15 cm. The red heat-resistant assembly and the black heat-resistant assembly are arranged in parallel, and are coated with an anti-corrosion protective sheath 4 on the outside; the anti-corrosion protective sheath 4 is a irradiable cross-linked polyolefin anti-corrosion protective sheath material; the thickness of the anti-corrosion protective sheath 4 is 5 cm.

[0035] The preparation method of the cable comprises the following steps: firstly, annealing soft fine copper wire bundles are twisted into a twisted soft conductor 1; a red heat-resistant insulating layer 2 is coated on the outside of the twisted soft conductor 1 to form a red heat-resistant assembly; a black heat-resistant insulating layer 3 is coated on the outside of the twisted soft conductor 1 to form a black heat-resistant assembly; the red heat-resistant assembly and the black heat-resistant assembly are arranged in parallel, and are coated with an anti-corrosion protective sheath on the outside, and are cross-linked by irradiation, and the irradiation process parameters are: beam voltage 1.3 MeV, beam current 90 mA, dose 60 kGy, and speed 600 m / min; thus, a green, environmentally friendly, heat-resistant photovoltaic cable is obtained.

[0036] The preparation process of the cross-linked polyolefin insulation material is as follows: 80g of linear low-density polyethylene, 18g of nonylphenol dichloride disulfide copolymer, 6g of organic montmorillonite, 3g of zinc borate and 3.5g of 2,2'-methylenebis(4-tert-octyl-6-benzotriazolephenol) are mixed, and the mixture is reacted at a temperature of 200°C for 6h; then 5g of tert-butyl isopropyl peroxide and 6g of silane coupling agent KH570 are added thereto, and the mixture is reacted at a temperature of 120°C for 4h to obtain the cross-linked polyolefin insulation material.

[0037] The preparation process of the anti-corrosion protective sleeve layer, which is a radiation-crosslinkable polyolefin anti-corrosion protective sleeve material, is as follows: 50g of ethylene-octene copolymer, 40g of ethylene vinyl acetate resin, 8g of triallyl isocyanate, 3g of triphenyl triazine, 5g of sodium dehydroacetate and 4g of potassium sorbate are mixed, and mixed in a closed mixer at a temperature of 195°C for 18 minutes; then, the mixture is put into a twin-screw extruder with four temperature sections for granulation to obtain the anti-corrosion protective sleeve layer; the temperatures of the twin-screw extruder in the four temperature sections are 150°C, 160°C, 175°C and 185°C, respectively.

[0038] Example 3

[0039] like Figure 1 and Figure 2As shown, this embodiment provides a green, environmentally friendly, heat-resistant photovoltaic cable, including a bundled soft conductor 1, a red heat-resistant insulating layer 2, a black heat-resistant insulating layer 3 and an anti-corrosion protective sheath 4; the bundled soft conductor 1 is formed by bundle twisting annealed soft fine copper wires; the red heat-resistant insulating layer 2 is coated on the outside of the bundled soft conductor 1 with an adhesive to form a red heat-resistant assembly; the black heat-resistant insulating layer 3 is coated on the outside of the bundled soft conductor 1 with an adhesive to form a black heat-resistant assembly; the red heat-resistant insulating layer 2 and the black heat-resistant insulating layer 3 are cross-linked polyolefin insulation materials; the diameter of the bundled soft conductor 1 is 1 cm; the thickness of the red heat-resistant insulating layer 2 and the black heat-resistant insulating layer 3 is 1.12 cm. The red heat-resistant assembly and the black heat-resistant assembly are arranged in parallel, and are coated with an anti-corrosion protective sheath 4 on the outside; the anti-corrosion protective sheath 4 is an irradiable cross-linked polyolefin anti-corrosion protective sheath material; the thickness of the anti-corrosion protective sheath 4 is 4.5 cm.

[0040] The preparation method of the cable comprises the following steps: firstly, annealing soft fine copper wire bundles are twisted into a twisted soft conductor 1; a red heat-resistant insulating layer 2 is coated on the outside of the twisted soft conductor 1 to form a red heat-resistant assembly; a black heat-resistant insulating layer 3 is coated on the outside of the twisted soft conductor 1 to form a black heat-resistant assembly; the red heat-resistant assembly and the black heat-resistant assembly are arranged in parallel, and are coated with an anti-corrosion protective sheath on the outside, and are cross-linked by irradiation, and the irradiation process parameters are: beam voltage 1.15 MeV, beam current 85 mA, dose 50 kGy, and speed 550 m / min; thus, a green, environmentally friendly, heat-resistant photovoltaic cable is obtained.

[0041] The preparation process of the cross-linked polyolefin insulation material is as follows: 60g of linear low-density polyethylene, 15g of nonylphenol dichloride disulfide copolymer, 5g of organic montmorillonite, 2g of zinc borate and 2g of 2,2'-methylenebis(4-tert-octyl-6-benzotriazolephenol) are mixed, and the mixture is reacted at a temperature of 180°C for 5.5h; then 4g of tert-butyl isopropyl peroxide and 5g of silane coupling agent KH570 are added thereto, and the mixture is reacted at a temperature of 110°C for 3h to obtain the cross-linked polyolefin insulation material.

[0042] The preparation process of the anti-corrosion protective sleeve layer, which is a radiation cross-linkable polyolefin anti-corrosion protective sleeve material, is as follows: 45g of ethylene-octene copolymer, 35g of ethylene vinyl acetate resin, 6g of triallyl isocyanate, 2g of triphenyl triazine, 4g of sodium dehydroacetate and 3g of potassium sorbate are mixed, and mixed in a closed mixer at a temperature of 190°C for 15 minutes; then, the mixture is put into a twin-screw extruder with four temperature sections for granulation to obtain the anti-corrosion protective sleeve layer; the temperatures of the twin-screw extruder in the four temperature sections are 150°C, 160°C, 175°C and 185°C respectively.

[0043] Comparative Example 1

[0044] The difference between this comparative example and Example 1 is that the preparation process of the cross-linked polyolefin insulation material does not add nonylphenol dichloride disulfide copolymer, and the other steps are the same.

[0045] Comparative Example 2

[0046] The difference between this comparative example and Example 1 is that the organic montmorillonite and zinc borate are not added in the preparation process of the cross-linked polyolefin insulation material, and the other steps are the same.

[0047] Comparative Example 3

[0048] The difference between this comparative example and Example 1 is that no silane coupling agent is added in the preparation process of the cross-linked polyolefin insulating material, and the other steps are the same.

[0049] Comparative Example 4

[0050] The difference between this comparative example and Example 1 is that triallyl isocyanate is not added in the preparation process of the radiation cross-linkable polyolefin anti-corrosion protective cover material, and the other steps are the same.

[0051] Comparative Example 5

[0052] The difference between this comparative example and Example 1 is that sodium dehydroacetate is not added in the preparation process of the radiation cross-linkable polyolefin anti-corrosion protective sheath material, and the other steps are the same.

[0053] Comparative Example 6

[0054] The difference between this comparative example and Example 1 is that three temperature sections are used in the preparation process of the radiation cross-linkable polyolefin anti-corrosion protective cover material, namely 155° C., 170° C., and 190° C., and the other steps are the same.

[0055] Performance Test:

[0056] Breakdown field strength: GB / T1408.1-2006; Heat aging test GB / T2951.12-2008; Tensile strength: GB / T2951; Oxygen index: ISO 4586. The test results are shown in the following table.

[0057] Table 1 Performance test results

[0058]

[0059] It can be seen from the above performance test results that Examples 1-3 have good performances such as anti-puncture, strength and aging resistance; in particular, the comprehensive performance of Example 3 is the most outstanding. However, since Comparative Examples 1-6 do not adopt the necessary technical solutions, their corresponding performance tests are significantly worse than those of the Examples. The above experimental results further prove the importance of the technical solutions defined in the present invention for its technical effects.

[0060] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A green, environmentally friendly, heat-resistant photovoltaic cable, characterized in that: It comprises a bundle of twisted soft conductors (1), a red heat-resistant insulating layer (2), a black heat-resistant insulating layer (3) and an anti-corrosion protective sheath (4); the bundle of twisted soft conductors (1) are formed by twisting annealed soft fine copper wires; the red heat-resistant insulating layer (2) is coated on the outside of the bundle of twisted soft conductors (1) to form a red heat-resistant assembly; the black heat-resistant insulating layer (3) is coated on the outside of the bundle of twisted soft conductors (1) to form a black heat-resistant assembly; the red heat-resistant assembly and the black heat-resistant assembly are arranged in parallel and are coated on the outside with an anti-corrosion protective sheath (4); The anti-corrosion protective sheath layer (4) is made of a radiation cross-linkable polyolefin anti-corrosion protective sheath material; the thickness of the anti-corrosion protective sheath layer (4) is 4-5 times the diameter of the bundled soft conductor (1); The red heat-resistant insulating layer (2) and the black heat-resistant insulating layer (3) are cross-linked polyolefin insulating materials; The preparation process of the cross-linked polyolefin insulation material is as follows: by weight, 40-80 parts of linear low-density polyethylene, 12-18 parts of nonylphenol dichloride disulfide copolymer, 3-6 parts of organic montmorillonite, 1-3 parts of zinc borate and 1.5-3.5 parts of 2,2'-methylenebis(4-tert-octyl-6-benzotriazolephenol) are mixed, and reacted at a temperature of 160-200°C for 4-6 hours; then 2-5 parts of tert-butyl isopropyl peroxide and 3-6 parts of silane coupling agent KH570 are added thereto, and reacted at a temperature of 100-120°C for 2-4 hours to obtain the cross-linked polyolefin insulation material; the thickness of the red heat-resistant insulation layer (2) and the black heat-resistant insulation layer (3) is 1-1.15 times the diameter of the bundled soft conductor (1).

2. A green, environmentally friendly, heat-resistant photovoltaic cable according to claim 1, characterized in that: The preparation process of the radiation cross-linkable polyolefin anticorrosion protective sleeve material is as follows: by weight, 30-50 parts of ethylene-octene copolymer, 20-40 parts of ethylene vinyl acetate resin, 3-8 parts of triallyl isocyanate, 1-3 parts of triphenyl triazine, 2-5 parts of sodium dehydroacetate and 1-4 parts of potassium sorbate are mixed, and the mixture is mixed in a closed mixer at a temperature of 175-195° C. for 12-18 minutes; Then the material is put into a twin-screw extruder with four temperature sections for granulation to obtain a radiation cross-linkable polyolefin anti-corrosion protective sheath material.

3. A green, environmentally friendly, heat-resistant photovoltaic cable according to claim 2, characterized in that: The preparation process of the radiation cross-linked polyolefin anti-corrosion protective cover material is optimized as follows: 45 parts of ethylene-octene copolymer, 35 parts of ethylene vinyl acetate resin, 6 parts of triallyl isocyanate, 2 parts of triphenyl triazine, 4 parts of sodium dehydroacetate and 3 parts of potassium sorbate are mixed by weight, and mixed in a closed mixer at a temperature of 190° C. for 15 minutes; then the mixture is put into a twin-screw extruder with four temperature sections for extrusion to obtain the radiation cross-linked polyolefin anti-corrosion protective cover material.

4. A green, environmentally friendly, heat-resistant photovoltaic cable according to claim 3, characterized in that: The temperatures of the twin-screw extruder in the four temperature sections are 150° C., 160° C., 175° C., and 185° C., respectively.

5. A method for preparing a green, environmentally friendly, heat-resistant photovoltaic cable as claimed in claim 1, characterized in that: The invention comprises the following steps: firstly, annealing soft fine copper wire bundles are twisted into a twisted soft conductor (1); a red heat-resistant insulating layer (2) is coated on the outside of the twisted soft conductor (1) to form a red heat-resistant assembly; a black heat-resistant insulating layer (3) is coated on the outside of the twisted soft conductor (1) to form a black heat-resistant assembly, wherein the thickness of the red heat-resistant insulating layer (2) and the black heat-resistant insulating layer (3) is 1-1.15 times the diameter of the twisted soft conductor (1); then, the red heat-resistant assembly and the black heat-resistant assembly are arranged in parallel and coated with an anti-corrosion protective sheath (4) on the outside, wherein the thickness of the anti-corrosion protective sheath (4) is 4-5 times the diameter of the twisted soft conductor (1); and after irradiation cross-linking, a green, environmentally friendly, heat-resistant photovoltaic cable is obtained.

6. The method for preparing a green, environmentally friendly, heat-resistant photovoltaic cable according to claim 5, characterized in that: The process parameters of the radiation cross-linking are: beam pressure 1-1.3 MeV, beam current 70-90 mA, dose 40-60 kGy, speed 500-600 m / min.

Citation Information

Cited By

  • Cross-linked polyolefin material for sea surface photovoltaic cable and preparation equipment of cross-linked polyolefin material

    CN119978585A