Water-based electrogalvanizing chromium-free fingerprint-resistant agent
Through the combined use of water-based electrogalvanized chromium-free fingerprint-resistant fingerprint-resistant agent, the shortcomings of electrogalvanized chromium-free fingerprint-resistant fingerprint-resistant agent in the prior art have been solved, better coating performance and resistance are achieved, and electrogalvanized galvanized The surface treatment effect of steel plate.
Patent Information
- Application Number
- CN202410954844.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-08
AI Technical Summary
The existing electrogalvanized chromium-free fingerprint-resistant fingerprint agents have shortcomings in coating performance, alkali resistance, degreasing resistance, stamping bending performance, solvent resistance, and black transformation resistance.
Use water-based electrogalvanized galvanized chromium-free fingerprint-resistant fingerprint agent, including aqueous ethylene methyl acrylate copolymer, aqueous polyurethane acrylic copolymer, oxidized polyethylene wax, etc., silane hydrolysate, emulsifier, pH adjuster, silicon sol, titanate coupler The combination of these components forms a paint film with excellent hardness and flexibility, improving coating performance and resistance.
It significantly improves the coating performance, alkali resistance, degreasing agent resistance, stamping bending performance, solvent resistance and black deformation resistance, ensuring the surface treatment effect of electro-plating galvanized steel plate.
Smart Images

Figure CN118909528A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a chromium-free anti-fingerprint agent, in particular to a water-based electro-galvanizing chromium-free anti-fingerprint agent and a preparation method thereof. Background Art
[0002] With the development of society, people's requirements for environmental protection are becoming more and more stringent. In the past, chromate surface treatment was mostly applied to parts for home appliances, building materials, and automobiles. However, in recent years, chromium-free anti-fingerprint agents have been gradually used to treat the surface of steel sheets, especially for home appliances. The pre-coated electro-galvanized anti-fingerprint sheet is not only beautiful, but also has good processability and corrosion resistance, because it is coated with a chromium-free anti-fingerprint agent on its surface.
[0003] There are two main directions for chromium-free surface treatment agents for electrogalvanized steel sheets in the prior art. One direction is the anionic system, which is mainly based on resin. The chromium-free surface treatment agent under this system has excellent stamping performance and moisture and heat resistance, but has deviations in salt spray resistance, edge salt spray performance, and ultrasonic cleaning performance. The other direction is the cationic system, which is mainly based on silane, and then corrosion inhibitors and resins are added. The chromium-free surface treatment agent under this system has excellent salt spray resistance, edge salt spray performance, and ultrasonic cleaning performance, but has deviations in stamping performance and moisture and heat resistance.
[0004] However, the existing electro-galvanized chromium-free anti-fingerprint agent has deficiencies in coating performance, alkali resistance, degreasing agent resistance, stamping and bending performance, solvent resistance, blackening resistance, and artificial sweat resistance. Summary of the invention
[0005] One advantage of the present invention is that it provides a water-based electrogalvanizing chromium-free anti-fingerprint agent, wherein the water-based electrogalvanizing chromium-free anti-fingerprint agent has good coating performance, alkali resistance, degreasing agent resistance, stamping and bending performance, solvent resistance, blackening resistance, and artificial welding resistance.
[0006] In order to achieve at least one of the above advantages of the present invention, the present invention provides a water-based electro-galvanizing chromium-free anti-fingerprint agent, which comprises the following components in parts by weight:
[0007]
[0008] Water-based ethylene methyl acrylate copolymer 2% to 6%
[0009] Waterborne polyurethane acrylic copolymer 8%~15%
[0010] Oxidized polyethylene wax 0.5%~1.5%
[0011] The balance was deionized water.
[0012] According to an embodiment of the present invention, the silane hydrolyzate is a mixture of epoxy silane, amino silane, alkyl silane and vinyl silane.
[0013] According to one embodiment of the present invention, the epoxy silane is selected from one or more of γ-glycidyl ether propyl trimethoxysilane, γ-glycidyl ether propyl triethoxysilane, β-(3,4-epoxycyclohexyl)ethyl trimethoxysilane, β-(3,4-epoxycyclohexyl)ethyl triethoxysilane, and 3-glycidyloxypropyl methyl diethoxysilane; the aminosilane (A2) is selected from one or more of γ-aminopropyl triethoxysilane, γ-aminopropyl trimethoxysilane, N-(2-aminoethyl)aminopropyl trimethoxysilane, N-(2-aminoethyl)aminopropyl triethoxysilane, N-(2-aminoethyl)aminopropyl dimethoxysilane, and N-(2-aminoethyl)aminopropyl diethoxysilane. The alkylsilane (A3) is selected from one or more of octyltrimethoxysilane, octyltriethoxysilane, methyltriethoxysilane, hexadecyltrimethoxysilane, 1,2-bis(trimethylsilane)ethane, and 1,2-bis(triethylsilane)ethane. The vinylsilane is selected from one or more of vinyltriethoxysilane, vinyltrimethoxysilane, and vinyltri(2-methoxyethoxy)silane.
[0014] According to an embodiment of the present invention, the emulsifier is a non-ionic emulsifier.
[0015] According to an embodiment of the present invention, the pH adjuster is bio-based glucosamine.
[0016] According to an embodiment of the present invention, the silica sol is aluminum-modified silica sol.
[0017] According to an embodiment of the present invention, the particle size of the silica sol is less than 3 nm, and the pH value is selected in the range of 8.5 to 10.5.
[0018] According to one embodiment of the present invention, the lithium compound is SiO 2 The content is 18% to 22%, Li 2 The O content is between 1.8% and 2.5%.
[0019] According to an embodiment of the present invention, the waterborne polyurethane resin is selected as waterborne anionic polyurethane, and its 100% modulus is in the range of 3000-7000 psi, its elongation at break is in the range of 150-300%, and its pH value is in the range of 7.0-9.
[0020] According to one embodiment of the present invention, the water-based ethylene methyl acrylate copolymer (H) is a water-based ethylene methyl acrylate copolymer with a pH value in the range of 7.0 to 9.5, the water-based polyurethane acrylic copolymer is an aromatic polyurethane acrylic copolymer dispersion with a pH value in the range of 7.0 to 9, the oxidized polyethylene wax particle size is in the range of 200nm to 2um, and the melting point is in the range of 50°C to 140°C. DETAILED DESCRIPTION
[0021] The following description is used to disclose the present invention so that those skilled in the art can implement the present invention. The preferred embodiments described below are only examples, and those skilled in the art can think of other obvious variations. The basic principles of the present invention defined in the following description can be applied to other embodiments, variations, improvements, equivalents, and other technical solutions that do not deviate from the spirit and scope of the present invention.
[0022] A water-based electro-galvanizing chromium-free anti-fingerprint agent according to a preferred embodiment of the present invention will be described in detail below, wherein the water-based electro-galvanizing chromium-free anti-fingerprint agent comprises the following components in parts by weight: Silane hydrolyzate (A) 4%~15% Emulsifier (B) 0.1%~1% pH adjuster (C) 0.2%~1.5% Silica sol (D) 4%~10% Titanate coupling agent (E) 0.5%~3% Silicon lithium compound (F) 0.1%~1% Waterborne polyurethane resin (G) 20%~30% Water-based ethylene methyl acrylate copolymer (H) 2%~6% Waterborne polyurethane acrylic copolymer (I) 8%~15% Oxidized polyethylene wax (J) 0.5%~1.5% The balance was deionized water.
[0023]
[0024] It is worth mentioning that the component A can provide the salt spray performance of the chrome-free anti-fingerprint agent; component B can make component A and subsequent components coexist stably; component C is used to adjust the pH value of component A; component D is used to fill the gaps in the anti-fingerprint film and improve the salt spray performance of the anti-fingerprint agent. The particle size of component D has a greater impact on the performance. Within a certain range, the smaller the particle size of component D, the better the performance; component E can improve the adhesion of the anti-fingerprint film, and can improve the salt spray performance when combined with component A; component F can assist in improving the overall salt spray performance of the anti-fingerprint film, and it can suppress the occurrence of fine pitting in the salt spray of the anti-fingerprint film; component G, component H, and component I can provide the overall paint film skeleton, and the combination of three types of resins of component G, component H, and component I makes the formed electroplated zinc-free chrome-free anti-fingerprint film have excellent hardness and flexibility; component J can improve the subsequent processing performance of the electroplated zinc-free chrome-free anti-fingerprint agent, but the amount used should not be too much to prevent overcoating and abnormal performance.
[0025] Preferably, the silane hydrolyzate (A) is a mixture of epoxy silane, amino silane, alkyl silane and vinyl silane. The epoxy silane (A1) is selected from one or more of γ-glycidyl ether propyl trimethoxy silane, γ-glycidyl ether propyl triethoxy silane, β-(3,4-epoxycyclohexyl)ethyl trimethoxy silane, β-(3,4-epoxycyclohexyl)ethyl triethoxy silane and 3-glycidyloxypropyl methyl diethoxy silane; the amino silane (A2) is selected from one or more of γ-aminopropyl triethoxy silane, γ-aminopropyl trimethoxy silane, N-(2-aminoethyl)aminopropyl trimethoxy silane, N-(2-aminoethyl)aminopropyl triethoxy silane, N-(2-aminoethyl)aminopropyl dimethoxy silane and N-(2-aminoethyl)aminopropyl diethoxy silane. The alkylsilane (A3) is selected from one or more of octyltrimethoxysilane, octyltriethoxysilane, methyltriethoxysilane, hexadecyltrimethoxysilane, 1,2-bis(trimethylsilane)ethane, and 1,2-bis(triethylsilane)ethane. The vinylsilane (A4) is selected from one or more of vinyltriethoxysilane, vinyltrimethoxysilane, and vinyltri(2-methoxyethoxy)silane.
[0026] Preferably, the emulsifier (B) is a nonionic emulsifier.
[0027] Preferably, the pH regulator (C) is bio-based glucosamine. Using this as a pH regulator, the silane hydrolyzate can exist stably under alkaline conditions.
[0028] Preferably, the silica sol (D) is aluminum-modified silica sol. Preferably, the silica sol particle size is less than 3 nm, and the pH value is selected in the range of 8.5 to 10.5.
[0029] Preferably, the titanate coupling agent (E) is a chelated titanate coupling agent, which has very good hydrolysis stability and can stably exist in an aqueous polymer system. Its usage is 0.5-3%. When the usage is small, the salt spray resistance is poor. When the usage is large, the electrogalvanized fingerprint-resistant sample has a large color difference in high temperature resistance.
[0030] Preferably, the silicon-lithium compound (F) is selected from SiO 2 The content is 18% to 22%, Li 2 The O content is between 1.8% and 2.5%. SiO 2 :Li 2 The content ratio of O needs to be within the corresponding content range, and its content ratio cannot be too high or too low. Too high or too low content ratios will affect the stability of the final configured silicon-lithium compound. The silicon-lithium content ratio selected by the silicon-lithium compound in this patent is easy to configure and the configured silicon-lithium compound has good stability. Add an equal amount of silicon-lithium compound to the water-based electroplating zinc chromium-free anti-fingerprint agent described in this patent. 2 The O content is too low, which is not enough to suppress the salt spray of the fingerprint-resistant film and cause fine pitting. 2 The O content is too high, and its salt spray resistance is excellent, but it will cause the board surface to turn black after salt spray resistance.
[0031] Preferably, the waterborne polyurethane resin (G) is selected as waterborne anionic polyurethane, with a 100% modulus in the range of 3000-7000 psi, a breaking elongation in the range of 150-300%, and a pH value in the range of 7.0-9.
[0032] Preferably, the aqueous ethylene methyl acrylate copolymer (H) is an aqueous ethylene methyl acrylate copolymer having a pH value in the range of 7.0 to 9.5.
[0033] Preferably, the aqueous polyurethane acrylic copolymer (I) is an aromatic polyurethane acrylic copolymer dispersion with a pH value in the range of 7.0 to 9.
[0034] Preferably, the particle size of the oxidized polyethylene wax (J) is 200nm-2um, and the melting point is 50°C-140°C. The particle size of the wax has a great influence on the performance. If the particle size is too fine, the stamping resistance is poor and the stamping film is prone to blackening. If the particle size is too coarse, it is easy to cause floating wax, agglomeration and the like, and the salt spray resistance is poor.
[0035] Example 1
[0036] At room temperature, add deionized water into the reactor, add silane hydrolyzate while stirring, and stir for 15 minutes; then add emulsifier while stirring, and stir for 15 minutes; then add pH adjuster while stirring, and stir for 20 minutes; then add silica sol while stirring, and stir for 13 minutes; slowly add titanate coupling agent while stirring, and stir for 40 minutes; slowly add silicon lithium compound while stirring, and stir for 30 minutes; add waterborne polyurethane resin, waterborne ethylene acrylic acid copolymer, and waterborne acrylic resin in order while stirring, and stir for 30 minutes;
[0037] Aqueous oxidized polyethylene wax was added and stirred for 30 minutes to obtain the anti-fingerprint agent for the electro-galvanized steel sheet.
[0038] Example 2
[0039] At room temperature, add deionized water into the reactor, add silane hydrolyzate while stirring, and stir for 15 minutes; then add emulsifier while stirring, and stir for 15 minutes; then add pH adjuster while stirring, and stir for 20 minutes; then add silica sol while stirring, and stir for 10 minutes; slowly add titanate coupling agent while stirring, and stir for 30 minutes; slowly add silicon lithium compound while stirring, and stir for 25 minutes; add waterborne polyurethane resin, waterborne ethylene acrylic acid copolymer, and waterborne acrylic resin in order while stirring, and stir for 30 minutes;
[0040] Aqueous oxidized polyethylene wax was added and stirred for 25 minutes to obtain the anti-fingerprint agent for the electro-galvanized steel sheet.
[0041] Example 3
[0042] At room temperature, add deionized water into the reactor, add silane hydrolyzate while stirring, and stir for 15 minutes; then add emulsifier while stirring, and stir for 15 minutes; then add pH adjuster while stirring, and stir for 20 minutes; then add silica sol while stirring, and stir for 15 minutes; slowly add titanate coupling agent while stirring, and stir for 50 minutes; slowly add silicon lithium compound while stirring, and stir for 25 minutes; add waterborne polyurethane resin, waterborne ethylene acrylic acid copolymer, and waterborne acrylic resin in order while stirring, and stir for 20 minutes;
[0043] Aqueous oxidized polyethylene wax was added and stirred for 15 minutes to obtain the anti-fingerprint agent for the electro-galvanized steel sheet.
[0044] Example 4
[0045] At room temperature, add deionized water into the reactor, add silane hydrolyzate while stirring, and stir for 15 minutes; then add emulsifier while stirring, and stir for 15 minutes; then add pH adjuster while stirring, and stir for 20 minutes; then add silica sol while stirring, and stir for 13 minutes; slowly add titanate coupling agent while stirring, and stir for 40 minutes; slowly add silicon lithium compound while stirring, and stir for 15 minutes; add waterborne polyurethane resin, waterborne ethylene acrylic acid copolymer, and waterborne acrylic resin in order while stirring, and stir for 40 minutes;
[0046] Aqueous oxidized polyethylene wax was added and stirred for 25 minutes to obtain the anti-fingerprint agent for the electro-galvanized steel sheet.
[0047] Example 5
[0048] At room temperature, add deionized water into the reactor, add silane hydrolyzate while stirring, and stir for 30 minutes; then add emulsifier while stirring, and stir for 15 minutes; then add pH adjuster while stirring, and stir for 20 minutes; then add silica sol while stirring, and stir for 13 minutes; slowly add titanate coupling agent while stirring, and stir for 30 minutes; slowly add silicon lithium compound while stirring, and stir for 25 minutes; add waterborne polyurethane resin, waterborne ethylene acrylic acid copolymer, and waterborne acrylic resin in order while stirring, and stir for 30 minutes;
[0049] Aqueous oxidized polyethylene wax was added and stirred for 30 minutes to obtain the anti-fingerprint agent for the electro-galvanized steel sheet.
[0050] Example 6
[0051] At room temperature, add deionized water into the reactor, add silane hydrolyzate while stirring, and stir for 15 minutes; then add emulsifier while stirring, and stir for 20 minutes; then add pH adjuster while stirring, and stir for 40 minutes; then add silica sol while stirring, and stir for 13 minutes; slowly add titanate coupling agent while stirring, and stir for 50 minutes; slowly add silicon lithium compound while stirring, and stir for 25 minutes; add waterborne polyurethane resin, waterborne ethylene acrylic acid copolymer, and waterborne acrylic resin in order while stirring, and stir for 30 minutes;
[0052] Aqueous oxidized polyethylene wax was added and stirred for 30 minutes to obtain the anti-fingerprint agent for the electro-galvanized steel sheet.
[0053] Example 7
[0054] At room temperature, add deionized water into the reactor, add silane hydrolyzate while stirring, and stir for 15 minutes; then add emulsifier while stirring, and stir for 40 minutes; then add pH adjuster while stirring, and stir for 20 minutes; then add silica sol while stirring, and stir for 10 minutes; slowly add titanate coupling agent while stirring, and stir for 30 minutes; slowly add silicon lithium compound while stirring, and stir for 15 minutes; add waterborne polyurethane resin, waterborne ethylene acrylic acid copolymer, and waterborne acrylic resin in order while stirring, and stir for 30 minutes;
[0055] Aqueous oxidized polyethylene wax was added and stirred for 15 minutes to obtain the anti-fingerprint agent for the electro-galvanized steel sheet.
[0056] Example 8
[0057] At room temperature, add deionized water into the reactor, add silane hydrolyzate while stirring, and stir for 15 minutes; then add emulsifier while stirring, and stir for 30 minutes; then add pH adjuster while stirring, and stir for 20 minutes; then add silica sol while stirring, and stir for 15 minutes; slowly add titanate coupling agent while stirring, and stir for 30 minutes; slowly add silicon lithium compound while stirring, and stir for 30 minutes; add waterborne polyurethane resin, waterborne ethylene acrylic acid copolymer, and waterborne acrylic resin in order while stirring, and stir for 30 minutes;
[0058] Aqueous oxidized polyethylene wax was added and stirred for 30 minutes to obtain the anti-fingerprint agent for the electro-galvanized steel sheet.
[0059] Table 1 shows the components (parts by mass) of the aqueous surface treatment agents in Examples 1 to 8.
[0060]
[0061]
[0062] The water-based chromium-free anti-fingerprint agent prepared in Examples 1 to 8 was coated on a 0.5 mm thick electro-galvanized steel plate using a wire rod roller and baked in an oven at 300°C for 15 seconds. The metal plate temperature PMT was 110 to 130°C to obtain a film weight of 1.0 g / m 2 After the water-based chrome-free anti-fingerprint dry film was placed at room temperature for 24 hours, the performance of the steel plate coated with the water-based surface treatment agent was tested. The test results are shown in Table 2.
[0063] Table 2 shows the performance test results of the steel plate coated with chrome-free anti-fingerprint agent
[0064]
[0065]
[0066] Table 2 shows that when the chromium-free anti-fingerprint agent is applied on the electro-galvanized substrate, all performances reach the target.
[0067] The above-mentioned chromium-free anti-fingerprint agent embodiment of the present invention is only an example for clearly explaining the present invention, and is not intended to limit the implementation methods of the present invention. Those skilled in the art should understand that other different forms of changes can be made based on the above description, and it is impossible to give detailed examples of all implementation methods here. All obvious changes derived from the technical solution of the present invention are still within the scope of protection of the present invention.
Claims
1. Aqueous electrogalvanizing chromium-free anti-fingerprint agent, characterized in that: It includes the following components by weight: The balance was deionized water.
2. The water-based electrogalvanizing chromium-free anti-fingerprint agent according to claim 1, characterized in that: The silane hydrolyzate is a mixture of epoxy silane, amino silane, alkyl silane and vinyl silane.
3. The water-based electrogalvanizing chromium-free anti-fingerprint agent according to claim 2, characterized in that: The epoxysilane is selected from one or more of γ-glycidyl ether propyl trimethoxysilane, γ-glycidyl ether propyl triethoxysilane, β-(3,4-epoxycyclohexyl)ethyl trimethoxysilane, β-(3,4-epoxycyclohexyl)ethyl triethoxysilane, and 3-glycidyloxypropyl methyl diethoxysilane; the aminosilane is selected from γ-aminopropyl triethoxysilane, γ-aminopropyl trimethoxysilane, N-(2-aminoethyl)aminopropyl trimethoxysilane, N-(2-aminoethyl)aminopropyl triethoxysilane, N -(2-aminoethyl)aminopropyldimethoxysilane, one or more of N-(2-aminoethyl)aminopropyldiethoxysilane, the alkylsilane is selected from octyltrimethoxysilane, octyltriethoxysilane, methyltriethoxysilane, hexadecyltrimethoxysilane, 1,2-bis(trimethylsilane)ethane, 1,2-bis(triethylsilane)ethane, and the vinylsilane is selected from vinyltriethoxysilane, vinyltrimethoxysilane, and vinyltri(2-methoxyethoxy)silane.
4. The water-based electrogalvanizing chromium-free anti-fingerprint agent according to claim 1, characterized in that: The emulsifier is a nonionic emulsifier.
5. The water-based electrogalvanizing chromium-free anti-fingerprint agent according to claim 1, characterized in that: The pH adjuster is bio-based glucosamine.
6. The water-based electrogalvanizing chromium-free anti-fingerprint agent according to claim 1, characterized in that: The silica sol is aluminum-modified silica sol.
7. The water-based electrogalvanizing chromium-free anti-fingerprint agent according to claim 6, characterized in that: The particle size of the silica sol is less than 3 nm, and the pH value is selected in the range of 8.5 to 10.
5.
8. The water-based electro-galvanizing chromium-free anti-fingerprint agent according to claim 1, characterized in that: The lithium compound is selected to have a SiO2 content of 18% to 22% and a Li2O content of 1.8% to 2.5%.
9. The water-based electrogalvanizing chromium-free anti-fingerprint agent according to claim 1, characterized in that: The waterborne polyurethane resin is selected as waterborne anionic polyurethane, the 100% modulus of which is in the range of 3000-7000 psi, the elongation at break is in the range of 150-300%, and the pH value is in the range of 7.0-9.
10. The water-based electrogalvanizing chromium-free anti-fingerprint agent according to claim 1, characterized in that: The aqueous ethylene methyl acrylate copolymer is an aqueous ethylene methyl acrylate copolymer with a pH value in the range of 7.0 to 9.5, the aqueous polyurethane acrylic copolymer is an aromatic polyurethane acrylic copolymer dispersion with a pH value in the range of 7.0 to 9, the oxidized polyethylene wax particle size is in the range of 200nm to 2um, and the melting point is in the range of 50°C to 140°C.
Citation Information
Patent Citations
Organic and inorganic mixed fingerprint-resistance coating and preparation method thereof
CN102070966A
Special chromium-free fingerprint resistant liquid for zinc-aluminum-magnesium coated steel plate and preparation method of special chromium-free fingerprint resistant liquid
CN107418328A
Chromium-free fingerprint-proof treatment solution for hot-galvanized steel plates
CN107629591A
Water-based fingerprint-resistant coating with interpenetrating network structure for galvanized steel sheet
CN114231109A