Anti-PID EVA packaging adhesive film

By using a reactive deacidifying agent system of carbodiimide or carbodiimide compounds and amino-containing silane coupling agents in EVA encapsulation films, the problems of reduced light transmittance and PID in EVA films in humid and hot environments were solved, achieving better interfacial adhesion and anti-PID effects.

CN118909554APending Publication Date: 2024-11-08SHAOXING HUAYUAN NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411247455.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

EVA encapsulation film will hydrolyze and release acetic acid or acidic substances in humid and hot environments, leading to power degradation of photovoltaic modules. Furthermore, existing inorganic deacidifying agents affect light transmittance and cause appearance problems.

Method used

A reactive deacidifying agent system is adopted, including carbodiimide or carbodiimide compounds and amino-containing silane coupling agents. Through deacidification condensation reaction, the interfacial adhesion performance is maintained in a humid and hot environment, thereby enhancing the anti-PID effect.

Benefits of technology

Maintaining the light transmittance of the film in a humid and hot environment enhances interfacial adhesion, achieves better anti-PID effect, and prevents power degradation of photovoltaic modules.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005031220210000091
    Figure BDA0005031220210000091
  • Figure BDA0005031220210000101
    Figure BDA0005031220210000101
Patent Text Reader

Abstract

The invention discloses an anti-PID (Potential Induced Degradation) EVA (Ethylene Vinyl Acetate) packaging adhesive film. The EVA packaging adhesive film comprises 0.01-1% of a deacidification agent A, 0.01-1% of a deacidification agent B and 0.1-5% of a catalyst relative to the sum of the weight of the deacidification agent A and the weight of the deacidification agent B, the acid removal agent A is carbodiimide or a carbodiimide compound; the deacidification agent B is a silane coupling agent with amino groups. The EVA packaging adhesive film provided by the invention adopts a reaction type acid remover system, so that the EVA packaging adhesive film not only can be better applied to a humid and hot environment to realize a better anti-PID effect, but also does not affect the light transmittance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of photovoltaic module packaging films, and in particular to an anti-PID EVA packaging film. Background Art

[0002] As the global demand for renewable energy continues to rise, photovoltaic power generation has received widespread attention as a clean and sustainable form of energy. The common photovoltaic module has a front cover plate, a front encapsulation film, a cell layer, a back encapsulation film and a backplane from the front to the back. Among them, the encapsulation film is the key material for the encapsulation of photovoltaic modules, and is generally divided into EVA, POE and other encapsulation films. EVA is a copolymer of ethylene-vinyl acetate. Due to its superiority in adhesion, durability, optical properties, etc., it is increasingly widely used in various optical products. However, in a humid and hot environment, the EVA film will gradually hydrolyze and release acetic acid or acidic substances, causing the photovoltaic module to attenuate power; therefore, the EVA encapsulation film on the market usually adds alkaline oxides or peroxides such as magnesium hydroxide and aluminum hydroxide as acid scavengers. However, the addition of these substances will affect the transmittance, and these small-molecule inorganic substances will slowly migrate out of the film surface during use, causing appearance problems. Summary of the invention

[0003] To solve the above technical problems, the purpose of the present invention is to provide an anti-PID EVA encapsulation film, which adopts a reactive acid scavenger system, which can not only be better applied in a humid and hot environment to achieve a better anti-PID effect, but also will not affect the light transmittance.

[0004] In order to achieve the above technical objectives and the above technical effects, the present invention is implemented through the following technical solutions:

[0005] A PID-resistant EVA packaging film comprises EVA resin, 0.01-1% of an acid scavenger A, 0.01-1% of an acid scavenger B, and 0.1-5% of a catalyst relative to the sum of the weights of the acid scavenger A and the acid scavenger B; the acid scavenger A is carbodiimide or a carbodiimide compound; and the acid scavenger B is a silane coupling agent with an amino group.

[0006] Preferably, the carbodiimide or carbodiimide compound is selected from one or a combination of two or more of dicyclohexylcarbodiimide, diisopropylcarbodiimide, 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide, and 1-ethyl-(3-dimethylaminopropyl)carbodiimide.

[0007] Preferably, the silane coupling agent with an amino group is selected from one or a combination of two or more of γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane, N-β-(aminoethyl)-γ-aminopropylmethyldiethoxysilane, phenylaminomethyltriethoxysilane and phenylaminomethyltrimethoxysilane.

[0008] Preferably, the catalyst is selected from one or a combination of two or more of 4-N,N-dimethylpyridine, 1-hydroxybenzotriazole, 4-pyrrolidinylpyridine, 1-hydroxy-7-azabenzotriazole, N-hydroxyphthalimide, and pentafluorophenol.

[0009] Furthermore, the EVA encapsulation film also includes EVA resin, a cross-linking agent, a co-cross-linking agent and a light stabilizer.

[0010] Furthermore, the EVA packaging film includes 94.5-98.5% of EVA resin, 0.5-1.5% of a cross-linking agent, 0.5-1.5% of an auxiliary cross-linking agent, and 0.1-0.5% of a light stabilizer.

[0011] Preferably, the crosslinking agent is an organic peroxide crosslinking agent, and the organic peroxide crosslinking agent is selected from one or a combination of two or more of diisopropylbenzene peroxide, tert-butyl peroxy-2-ethylhexyl carbonate, 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, tert-amyl peroxy-2-ethylhexyl carbonate, di(2-ethyl)hexyl peroxydicarbonate, tert-amyl peroxy-2-ethylhexyl carbonate, benzoyl peroxide, and tert-butyl peroxy-2-ethylhexanoate.

[0012] Preferably, the auxiliary cross-linking agent is selected from one or a combination of two or more of triallyl isocyanurate, 3-(trimethoxysilyl)propyl methacrylate, 3-vinylphenol, triallyl cyanurate, trimethylolpropane triacrylate and trimethylolpropane trimethacrylate.

[0013] Preferably, the light stabilizer is selected from light stabilizer 770, light stabilizer 292, light stabilizer 944, or a combination of two or more thereof.

[0014] Furthermore, the EVA packaging film also includes one or more of an antioxidant, an ultraviolet absorber, a silane coupling agent, and a filler.

[0015] Preferably, the antioxidant is selected from one or more of antioxidant 1010, antioxidant 1076, and antioxidant 168.

[0016] Preferably, the silane coupling agent is selected from one or more of vinyl triethoxysilane, vinyl trimethoxysilane, vinyl triperoxide tert-butyl silane, vinyl triacetoxysilane, vinyl tri(β-methoxyethoxy)silane, and γ-(methacryloyloxy)propyltrimethoxysilane.

[0017] Preferably, the filler is selected from one or more of titanium dioxide, calcium carbonate, barium sulfate, silicon dioxide, silicon micropowder, calcium sulfate, bismuth oxychloride, magnesium hydroxide, and zinc oxide.

[0018] The ultraviolet absorber is selected from one or more of UV531, UV234, UV312, benzophenone, 2-ethylhexyl salicylate, and isooctyl p-methoxycinnamate.

[0019] The beneficial effects of the present invention are:

[0020] The EVA adhesive film of the present invention is added with an acid scavenger system in which two acid scavengers are combined, one of which is a carbodiimide or a carbodiimide compound, and the other is a silane coupling agent with an amino group. The acid scavenger system is a reactive acid scavenger system. In a hot and humid environment, the carbodiimide or the carbodiimide compound can react with the generated acetic acid or an acidic substance to a certain extent, and the silane coupling agent with the amino group and the generated acetic acid or an acidic substance can undergo an acid removal condensation reaction. The carbodiimide or the carbodiimide compound acts as a dehydrating agent, which can promote the acid removal condensation reaction and improve the acid removal effect.

[0021] The present invention uses two acid scavengers to work together to maintain the adhesive properties of the interface through acid removal condensation reaction in a hot and humid environment, and can enhance the interface adhesion, especially the interface adhesion after hot and humid aging;

[0022] The present invention uses two acid scavengers in synergy to achieve better anti-PID effect;

[0023] The EVA film of the present invention adopts a reactive acid scavenger system, which not only has a better application effect in a hot and humid environment, but also ensures that the peel strength of the EVA film does not decrease in a hot and humid environment, and the anti-PID effect of the film is better, and compared with the inorganic acid scavenging system, it does not affect the light transmittance. DETAILED DESCRIPTION

[0024] The technical solutions in the present invention will be described clearly and completely below in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] The invention provides an anti-PID EVA packaging adhesive film. The raw materials for preparing the film include EVA resin, 0.01-1% of an acid scavenger A, 0.01-1% of an acid scavenger B, and 0.1-5% of a catalyst relative to the sum of the weights of the acid scavenger A and the acid scavenger B; the acid scavenger A is carbodiimide or a carbodiimide compound; and the acid scavenger B is a silane coupling agent with an amino group.

[0026] Specifically, the EVA encapsulation film also includes EVA resin. In addition, the EVA encapsulation film may also include a cross-linking agent, a co-cross-linking agent and a light stabilizer.

[0027] More specifically, in addition to the above-mentioned 0.01-1% of acid scavenger A, 0.01-1% of acid scavenger B and 0.1-5% of catalyst relative to the sum of the weights of acid scavenger A and acid scavenger B, the raw materials for preparing the EVA encapsulation film also include 94.5-98.5% EVA resin, 0.5-1.5% cross-linking agent, 0.5-1.5% auxiliary cross-linking agent, and 0.1-0.5% light stabilizer.

[0028] The carbodiimide or carbodiimide compound is selected from one or a combination of two or more of dicyclohexylcarbodiimide, diisopropylcarbodiimide, 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide, and 1-ethyl-(3-dimethylaminopropyl)carbodiimide.

[0029] The silane coupling agent with amino group is selected from one or a combination of two or more of γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane, N-β-(aminoethyl)-γ-aminopropylmethyldiethoxysilane, anilinomethyltriethoxysilane and anilinomethyltrimethoxysilane.

[0030] The catalyst is selected from one or a combination of two or more of 4-N,N-dimethylpyridine, 1-hydroxybenzotriazole, 4-pyrrolidinylpyridine, 1-hydroxy-7-azabenzotriazole, N-hydroxyphthalimide and pentafluorophenol.

[0031] The crosslinking agent is an organic peroxide crosslinking agent, and the organic peroxide crosslinking agent is selected from one or a combination of two or more of diisopropylbenzene peroxide, tert-butyl peroxy-2-ethylhexyl carbonate, 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, tert-amyl peroxy-2-ethylhexyl carbonate, di(2-ethyl)hexyl peroxydicarbonate, tert-amyl peroxy-2-ethylhexyl carbonate, benzoyl peroxide, and tert-butyl peroxy-2-ethylhexanoate.

[0032] The auxiliary cross-linking agent is selected from one or a combination of two or more of triallyl isocyanurate, 3-(trimethoxysilyl)propyl methacrylate, 3-vinylphenol, triallyl cyanurate, trimethylolpropane triacrylate and trimethylolpropane trimethacrylate.

[0033] The light stabilizer is selected from the group consisting of light stabilizer 770, light stabilizer 292, and light stabilizer 944, or a combination of two or more thereof.

[0034] In addition to the above components, the EVA packaging film may also be added with one or more of an antioxidant, an ultraviolet absorber, a silane coupling agent, and a filler as required.

[0035] Among them, the antioxidant is selected from one or more of antioxidant 1010, antioxidant 1076, and antioxidant 168.

[0036] The silane coupling agent is selected from one or more of vinyl triethoxysilane, vinyl trimethoxysilane, vinyl triperoxide tert-butyl silane, vinyl triacetoxysilane, vinyl tri(β-methoxyethoxy)silane, and γ-(methacryloyloxy)propyl trimethoxysilane.

[0037] The filler is selected from one or more of titanium dioxide, calcium carbonate, barium sulfate, silicon dioxide, silicon micropowder, calcium sulfate, bismuth oxychloride, magnesium hydroxide and zinc oxide.

[0038] The ultraviolet absorber is selected from one or more of UV531, UV234, UV312, benzophenone, 2-ethylhexyl salicylate, and isooctyl p-methoxycinnamate.

[0039] Example 1

[0040] Based on 100 parts by total weight, the raw materials for preparing the EVA encapsulation film include:

[0041] 96.15 parts of EVA resin, 1 part of acid scavenger A: dicyclohexylcarbodiimide, 0.05 parts of catalyst 4-N,N-dimethylpyridine, 1 part of acid scavenger B: γ-aminopropyltrimethoxysilane, 0.3 parts of cross-linking agent peroxy-2-ethylhexyl carbonate tert-butyl ester, 0.3 parts of cross-linking agent peroxy-2-ethylhexyl carbonate tert-amyl ester, 0.5 parts of auxiliary cross-linking agent triallyl isocyanurate, 0.2 parts of auxiliary cross-linking agent trimethylolpropane trimethacrylate, 0.3 parts of silane coupling agent KH570, 0.1 parts of antioxidant 1076, and 0.1 parts of light stabilizer 292.

[0042] The above raw materials were stirred evenly in a conical stirring kettle, placed at 35°C for 12 hours, and then put into a film casting machine to prepare a film with a gram weight of 380g / m 2 Anti-PID EVA encapsulation film.

[0043] Example 2

[0044] Based on 100 parts by total weight, the raw materials for preparing the EVA encapsulation film include:

[0045] 97.17 parts of EVA resin, 0.5 parts of acid scavenger A: diisopropylcarbodiimide, 0.03 parts of catalyst 4-N,N-dimethylpyridine, 0.5 parts of acid scavenger B: γ-aminopropyltriethoxysilane, 0.3 parts of cross-linking agent peroxy-2-ethylhexyl carbonate tert-butyl ester, 0.3 parts of cross-linking agent peroxy-2-ethylhexyl carbonate tert-amyl ester, 0.5 parts of auxiliary cross-linking agent triallyl isocyanurate, 0.2 parts of auxiliary cross-linking agent trimethylolpropane trimethacrylate, 0.3 parts of silane coupling agent KH570, 0.1 parts of antioxidant 1076, and 0.1 parts of light stabilizer 292.

[0046] The above raw materials were stirred evenly in a conical stirring kettle, placed at 35°C for 12 hours, and then put into a film casting machine to prepare a film with a gram weight of 380g / m 2 Anti-PID EVA encapsulation film.

[0047] Example 3

[0048] Based on 100 parts by total weight, the raw materials for preparing the EVA encapsulation film include:

[0049] 97.99 parts of EVA resin, 0.1 parts of acid scavenger A: diisopropylcarbodiimide, 0.01 parts of catalyst 4-N,N-dimethylpyridine, 0.1 parts of acid scavenger B: γ-aminopropyltriethoxysilane, 0.3 parts of cross-linking agent peroxy-2-ethylhexyl carbonate tert-butyl ester, 0.3 parts of cross-linking agent peroxy-2-ethylhexyl carbonate tert-amyl ester, 0.5 parts of auxiliary cross-linking agent triallyl isocyanurate, 0.2 parts of auxiliary cross-linking agent trimethylolpropane trimethacrylate, 0.3 parts of silane coupling agent KH570, 0.1 parts of antioxidant 1076, and 0.1 parts of light stabilizer 292.

[0050] The above raw materials were stirred evenly in a conical stirring kettle, placed at 35°C for 12 hours, and then put into a film casting machine to prepare a film with a gram weight of 380g / m 2 Anti-PID EVA encapsulation film.

[0051] Comparative Example 1

[0052] Based on 100 parts by weight, the raw materials for preparation include:

[0053] 98.2 parts of EVA resin, 0.3 parts of cross-linking agent peroxy-2-ethylhexyl tert-butyl carbonate, 0.3 parts of cross-linking agent peroxy-2-ethylhexyl tert-amyl carbonate, 0.5 parts of auxiliary cross-linking agent triallyl isocyanurate, 0.2 parts of auxiliary cross-linking agent trimethylolpropane trimethacrylate, 0.3 parts of silane coupling agent KH570, 0.1 parts of antioxidant 1076, and 0.1 parts of light stabilizer 292.

[0054] The above raw materials were stirred evenly in a conical stirring kettle, placed at 35°C for 12 hours, and then put into a film casting machine to prepare a film with a gram weight of 380g / m 2 Anti-PID EVA encapsulation film.

[0055] Comparative Example 2

[0056] Based on 100 parts by weight, the raw materials for preparation include:

[0057] 97.7 parts of EVA resin, 0.5 parts of magnesium hydroxide with a particle size of 0.5 μm, 0.3 parts of cross-linking agent tert-butyl peroxide-2-ethylhexyl carbonate, 0.3 parts of cross-linking agent tert-amyl peroxide-2-ethylhexyl carbonate, 0.5 parts of auxiliary cross-linking agent triallyl isocyanurate, 0.2 parts of auxiliary cross-linking agent trimethylolpropane trimethacrylate, 0.3 parts of silane coupling agent KH570, 0.1 parts of antioxidant 1076, and 0.1 parts of light stabilizer 292.

[0058] The above raw materials were stirred evenly in a conical stirring kettle, placed at 35°C for 12 hours, and then put into a film casting machine to prepare a film with a gram weight of 380g / m 2 Anti-PID EVA encapsulation film.

[0059] Comparative Example 3

[0060] Based on 100 parts by weight, the raw materials for preparation include:

[0061] 95.15 parts of EVA resin, 1.5 parts of acid scavenger A: diisopropylcarbodiimide, 0.05 parts of catalyst 4-N,N-dimethylpyridine, 1.5 parts of acid scavenger B: γ-aminopropyltriethoxysilane, 0.3 parts of cross-linking agent peroxy-2-ethylhexyl carbonate tert-butyl ester, 0.3 parts of cross-linking agent peroxy-2-ethylhexyl carbonate tert-amyl ester, 0.5 parts of auxiliary cross-linking agent triallyl isocyanurate, 0.2 parts of auxiliary cross-linking agent trimethylolpropane trimethacrylate, 0.3 parts of silane coupling agent KH570, 0.1 parts of antioxidant 1076, and 0.1 parts of light stabilizer 292.

[0062] The above raw materials were stirred evenly in a conical stirring kettle, placed at 35°C for 12 hours, and then put into a film casting machine to prepare a film with a gram weight of 380g / m 2 Anti-PID EVA encapsulation film.

[0063] Comparative Example 4

[0064] Based on 100 parts by weight, the raw materials for preparation include:

[0065] 97.67 parts of EVA resin, 0.03 parts of catalyst 4-N,N-dimethylpyridine, 0.5 parts of acid scavenger B: γ-aminopropyl triethoxysilane, 0.3 parts of cross-linking agent peroxy-2-ethylhexyl carbonate tert-butyl ester, 0.3 parts of cross-linking agent peroxy-2-ethylhexyl carbonate tert-amyl ester, 0.5 parts of auxiliary cross-linking agent triallyl isocyanurate, 0.2 parts of auxiliary cross-linking agent trimethylolpropane trimethacrylate, 0.3 parts of silane coupling agent KH570, 0.1 parts of antioxidant 1076, and 0.1 parts of light stabilizer 292.

[0066] The above raw materials were stirred in a conical stirring kettle, placed at 35°C for 12 hours, and then put into a film casting machine to prepare a film with a gram weight of 380 g / m 2 Anti-PID EVA encapsulation film.

[0067] Performance Testing

[0068] The light transmittance test of the encapsulation film samples of Examples 1-3 and Comparative Examples 1-4 was performed with reference to IEC62788-1-2;

[0069] The encapsulation film samples of Examples 1-3 and Comparative Examples 1-4 were prepared into photovoltaic modules, the power of the photovoltaic modules was tested, and the power attenuation of the photovoltaic modules after PID192h and PID384h was tested;

[0070] The packaging film samples of Examples 1-3 and Comparative Examples 1-4 were laminated at 145° C. according to the backplane / EVA packaging film / glass stacking method, and the peeling strength with EVA and the peeling strength with EVA after PCT 48h and DH 2000h were tested.

[0071] The test results are shown in Table 1.

[0072] Table 1

[0073]

[0074]

[0075] From the data in Table 1, we can see that:

[0076] The light transmittance of Examples 1-3 is almost unchanged compared with that of Comparative Example 1 without adding an acid scavenger, indicating that the acid scavenger of the present invention does not affect the light transmittance at a certain ratio. After adding magnesium hydroxide acid scavenger to Comparative Example 2, the light transmittance is significantly reduced. The light transmittance of Comparative Example 3 is also reduced, indicating that the amount of the acid scavenger of the present invention will affect the transmittance after exceeding a certain range.

[0077] Contrast each embodiment and comparative example with EVA peel strength, initial value is not much different, all about 90N / cm.After PCT48h and DH2000, the peel strength numerical value of comparative example 1 and comparative example 2 is reduced to near 50N / cm, and obvious reduction has occurred.And the peel strength numerical value of embodiment 1-3 is also more than 70N / cm, this is because acid scavenger of the present invention is reactive acid scavenger, by deacidification condensation reaction in a hot and humid environment, keeps the adhesive property of interface.Comparative example 4 only adds acid scavenger B, and the interface adhesive property after PCT48h and DH2000, obviously reduces, illustrates that two kinds of acid scavengers of the present invention can realize strengthening interface bonding, particularly interface bonding after hot and humid aging in synergy.

[0078] Comparing the PID power attenuation, the components of Examples 1-3 are all within 2% after PID192h and PID384h, and have obvious anti-PID attenuation effect. Comparative Example 1 does not add an acid scavenger, and its power attenuation after PID192h and PID384h can reach 4.32% and 6.41% respectively. Comparative Example 2 adds magnesium hydroxide acid scavenger to have a certain anti-PID effect, but the effect is not as good as the embodiments of the present invention. Comparative Example 4 only adds acid scavenger B, and the anti-PID attenuation ability is reduced, and the attenuation after PID is larger, which shows that the two acid scavengers of the present invention can achieve better anti-PID effect in synergy.

[0079] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.

[0080] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A PID-resistant EVA encapsulation film, characterized in that: The EVA packaging film comprises EVA resin, 0.01-1% of an acid scavenger A, 0.01-1% of an acid scavenger B and 0.1-5% of a catalyst relative to the sum of the weights of the acid scavenger A and the acid scavenger B; the acid scavenger A is carbodiimide or a carbodiimide compound; and the acid scavenger B is a silane coupling agent with an amino group.

2. The PID-resistant EVA packaging film according to claim 1, characterized in that: The carbodiimide or carbodiimide compound is selected from one or a combination of two or more of dicyclohexylcarbodiimide, diisopropylcarbodiimide, 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide, and 1-ethyl-(3-dimethylaminopropyl)carbodiimide.

3. The PID-resistant EVA packaging film according to claim 1, characterized in that: The silane coupling agent with amino group is selected from one or a combination of two or more of γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane, N-β-(aminoethyl)-γ-aminopropylmethyldiethoxysilane, anilinomethyltriethoxysilane and anilinomethyltrimethoxysilane.

4. The PID-resistant EVA packaging film according to claim 1, characterized in that: The catalyst is selected from one or a combination of two or more of 4-N,N-dimethylpyridine, 1-hydroxybenzotriazole, 4-pyrrolidinylpyridine, 1-hydroxy-7-azabenzotriazole, N-hydroxyphthalimide and pentafluorophenol.

5. The PID-resistant EVA packaging film according to claim 1, characterized in that: The EVA encapsulation film also includes a cross-linking agent, a co-cross-linking agent and a light stabilizer.

6. The PID-resistant EVA packaging film according to claim 5, characterized in that: The EVA packaging film comprises 94.5-98.5% of EVA resin, 0.5-1.5% of a cross-linking agent, 0.5-1.5% of an auxiliary cross-linking agent, and 0.1-0.5% of a light stabilizer.

7. The PID-resistant EVA packaging film according to claim 5, characterized in that: The crosslinking agent is an organic peroxide crosslinking agent, and the organic peroxide crosslinking agent is selected from one or a combination of two or more of diisopropylbenzene peroxide, tert-butyl peroxy-2-ethylhexyl carbonate, 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, tert-amyl peroxy-2-ethylhexyl carbonate, di(2-ethyl)hexyl peroxydicarbonate, tert-amyl peroxy-2-ethylhexyl carbonate, benzoyl peroxide, and tert-butyl peroxy-2-ethylhexanoate.

8. The PID-resistant EVA packaging film according to claim 5, characterized in that: The auxiliary cross-linking agent is selected from one or a combination of two or more of triallyl isocyanurate, 3-(trimethoxysilyl)propyl methacrylate, 3-vinylphenol, triallyl cyanurate, trimethylolpropane triacrylate and trimethylolpropane trimethacrylate.

9. The PID-resistant EVA packaging film according to claim 5, characterized in that: The light stabilizer is selected from the group consisting of light stabilizer 770, light stabilizer 292, and light stabilizer 944, or a combination of two or more thereof.

10. The PID-resistant EVA packaging film according to claim 1 or 5, characterized in that: The EVA packaging film also includes one or more of an antioxidant, an ultraviolet absorber, a silane coupling agent, and a filler.