Preparation method of CuS / polydopamine heating leather

Through the preparation of CuS/polydopamine leather, combined with the dual heating functions of electric and light and heat, the problem of insufficient warming performance of traditional leather is solved, and effective heating effect is achieved in a variety of scenarios, suitable for changing environments in winter.

CN118910339APending Publication Date: 2024-11-08SHAANXI UNIV OF SCI & TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411210501.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The warming performance of traditional leather is insufficient and cannot be effectively used in low-temperature outdoor environments, which limits its application in variable winter scenarios. The existing heating function of heating leather is single, which cannot meet the needs of multiple scenarios.

Method used

CuS/polydopamine heating leather is prepared by forming a polydopamine self-polymerization layer on the surface of the leather as the CuS growth site to construct CuS/polydopamine leather, combining the dual heating functions of electric and photothermal. Specific steps include preparing a polydopamine solution, immersing the leather, treating it in CuSO4 and Na2S2O3 solutions, adding citric acid to adjust the pH, washing and drying after shaking, forming CuS/polydopamine leather with electric, thermal, photothermal properties.

Benefits of technology

The electric and thermal performance of CuS/polydopamine leather is achieved, with an average resistance of 13.1Ω, a driving voltage of 3V can reach 82℃, a high solar spectrum absorption rate of 84%, and can heat up to 77℃ under standard sunlight, suitable for a variety of Heating the scene.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a CuS / polydopamine heating leather preparation method, which specifically comprises: 1, preparing a polydopamine solution, immersing leather in the polydopamine solution, standing, taking out, completely washing with deionized water, and airing to obtain polydopamine leather; step 2, preparing a CuSO4 solution and a Na2S2O3 solution with the same concentration; 3, the polydopamine leather obtained in the step 1 is placed in a CuSO4 solution, then a Na2S2O3 solution is poured, then a citric acid solution is added to adjust the pH to 4-4.5, oscillation is conducted, after oscillation is finished, deionized water is used for sufficient washing till a washing solution is completely clarified, natural airing is conducted, and the CuS / polydopamine leather is obtained. According to the CuS / polydopamine heating leather prepared by the preparation method of the CuS / polydopamine heating leather provided by the invention, polydopamine is self-polymerized on the surface of the leather to form an adhesion layer which is used as a secondary reaction platform to provide a growth site for CuS, and then CuS is introduced to construct the CuS / polydopamine heating leather, so that the CuS / polydopamine heating leather has the characteristic of electrothermal and photo-thermal heating.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of functional leather preparation, and relates to a method for preparing CuS / polydopamine heated leather. Background Art

[0002] The leather industry is an important part of my country's light industry. However, with the improvement of consumption level, consumers' demand for high-performance leather has gradually expanded, prompting the traditional leather industry to develop towards functionalization and intelligence. Traditional leather has poor thermal insulation performance and cannot be used in low-temperature outdoor environments, which limits the application of leather products in the winter cold-resistant market. Therefore, it is necessary to develop leather with heating properties to meet people's needs for cold protection and warmth, thereby achieving high-value development of leather, which is also in line with the development plan of the leather industry.

[0003] At present, the main idea of ​​preparing heating leather is to introduce materials with excellent conductivity such as AgNW or materials with light-to-heat conversion performance such as carbon nanotubes into leather through coating or vacuum filtration. Under the action of external power supply or sunlight, the temperature of the leather is increased through the conversion of electrical energy, light energy and thermal energy, thereby reducing the temperature difference between the human body and the external environment, thereby reducing the total amount of heat dissipated by the human body and achieving leather warmth for the human body. However, the heating function of the above-mentioned heating leather is relatively single, which hinders its further application in the changing scenes in winter. Therefore, it is very important to develop heating leather with multiple integrated heating functions. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing CuS / polydopamine heating leather, which solves the problem that traditional leather cannot be heated.

[0005] The technical solution adopted by the present invention is a method for preparing CuS / polydopamine heated leather, which specifically comprises the following steps:

[0006] Step 1: prepare a polydopamine solution, immerse the leather in the polydopamine solution and let it stand, then take it out and wash it thoroughly with deionized water, and finally dry it to obtain polydopamine leather;

[0007] Step 2: Prepare CuSO4 solution and Na2S2O3 solution of the same concentration;

[0008] Step 3: Place the polydopamine leather obtained in step 1 in a CuSO4 solution, then pour in a Na2S2O3 solution, and then add a citric acid solution to adjust the pH to 4-4.5, and shake. After the shaking, wash it thoroughly with deionized water until the washing liquid is completely clear, and dry it naturally to obtain CuS / polydopamine leather.

[0009] The present invention is also characterized in that:

[0010] In step 1, the specific steps of preparing the polydopamine solution are:

[0011] 2 mg / mL dopamine hydrochloride was dissolved in 10 mM Tris buffer solution, followed by the addition of 5 mM copper sulfate and 19.6 mM hydrogen peroxide.

[0012] In step 1, the specific steps of leather immersion and washing are:

[0013] The leather is quickly immersed in the polydopamine solution, left to stand at 25-35° C. for 0.5-1 hour, then taken out, and the leather is fully washed with deionized water until the washing solution is completely clarified, and finally dried to obtain the polydopamine leather.

[0014] In step 2, the specific steps of preparing the CuSO4 solution and the Na2S2O3 solution are as follows:

[0015] Dissolve CuSO4 and Na2S2O3 in deionized water to obtain CuSO4 solution and Na2S2O3 solution respectively, and the concentration of the CuSO4 solution is 50-350 mM.

[0016] In step S3, the concentration of the citric acid solution is 10%.

[0017] In step S3, the process parameters of oscillation are oscillation at 65° C. for 1-2 hours.

[0018] The beneficial effects of the present invention are:

[0019] The present invention provides a method for preparing CuS / polydopamine heating leather. In the present invention, polydopamine is self-polymerized on the leather surface to form an adhesion layer, which serves as a secondary reaction platform to provide a growth site for CuS. CuS is then introduced to construct the CuS / polydopamine heating leather, so that the leather has the characteristics of electric and light heating. DETAILED DESCRIPTION

[0020] The present invention is described in detail below in conjunction with specific implementation modes.

[0021] The preparation method of CuS / polydopamine heated leather specifically comprises the following steps:

[0022] Step 1: prepare a polydopamine solution, dissolve 2 mg / mL dopamine hydrochloride in 10 mM tris buffer solution, then add 5 mM copper sulfate and 19.6 mM hydrogen peroxide to obtain a polydopamine solution; quickly immerse the leather in the polydopamine solution, let it stand for 0.5 to 1 hour at 25 to 35° C., then take it out, wash the leather with deionized water until the washing solution is completely clear, and finally dry it to obtain polydopamine leather;

[0023] Step 2: Prepare a CuSO4 solution and a Na2S2O3 solution of the same concentration, dissolve the CuSO4 and Na2S2O3 in deionized water to obtain a CuSO4 solution and a Na2S2O3 solution, respectively, wherein the concentration of the CuSO4 solution is 50-350 mM;

[0024] Step 3: Place the polydopamine leather obtained in step 1 in a CuSO4 solution, then pour in a Na2S2O3 solution, and then add a 10% citric acid solution to adjust the pH to 4-4.5, oscillate at 65°C for 1-2 hours, and after the oscillation, wash thoroughly with deionized water until the washing liquid is completely clear, and dry naturally to obtain CuS / polydopamine leather.

[0025] The two poles of the multimeter were respectively connected to the CuS / polydopamine leather with a distance of 1 cm between the two poles, and the resistance at different positions was measured; the average resistance of the CuS / polydopamine leather was measured to be 13.1Ω, and the electric heating temperature could reach 82°C when the driving voltage was 3V. The CuS / polydopamine leather had a high solar spectrum absorptivity of 84%, and could be heated to 77°C in 240s under a standard solar light density, indicating that it has excellent electrothermal / photothermal properties.

[0026] Example 1

[0027] The preparation method of CuS / polydopamine heated leather specifically comprises the following steps:

[0028] Step 1: prepare a polydopamine solution, dissolve 2 mg / mL dopamine hydrochloride in 10 mM tris buffer solution, then add 5 mM copper sulfate and 19.6 mM hydrogen peroxide to obtain a polydopamine solution; quickly immerse the leather in the polydopamine solution, let it stand for 0.5 h at 25° C., then take it out, wash the leather thoroughly with deionized water until the washing solution is completely clear, and finally dry it to obtain polydopamine leather;

[0029] Step 2: Prepare a CuSO4 solution and a Na2S2O3 solution of the same concentration, dissolve the CuSO4 and Na2S2O3 in deionized water to obtain a CuSO4 solution and a Na2S2O4 solution, respectively, wherein the concentration of the CuSO4 solution is 50 mM;

[0030] Step 3: Place the polydopamine leather obtained in step 1 in a CuSO4 solution, then pour in a Na2S2O3 solution, and then add a 10% citric acid solution to adjust the pH to 4, oscillate at 65°C for 1 hour, and after the oscillation, wash thoroughly with deionized water until the washing liquid is completely clear, and dry naturally to obtain CuS / polydopamine leather.

[0031] Example 2

[0032] The preparation method of CuS / polydopamine heated leather specifically comprises the following steps:

[0033] Step 1: prepare a polydopamine solution, dissolve 2 mg / mL dopamine hydrochloride in 10 mM tris buffer solution, then add 5 mM copper sulfate and 19.6 mM hydrogen peroxide to obtain a polydopamine solution; quickly immerse the leather in the polydopamine solution, let it stand at 35° C. for 1 hour, then take it out, wash the leather thoroughly with deionized water until the washing solution is completely clear, and finally dry it to obtain polydopamine leather;

[0034] Step 2: Prepare a CuSO4 solution and a Na2S2O3 solution of the same concentration, dissolve the CuSO4 and Na2S2O3 in deionized water to obtain a CuSO4 solution and a Na2S2O3 solution, respectively, wherein the concentration of the CuSO4 solution is 350 mM;

[0035] Step 3: Place the polydopamine leather obtained in step 1 in a CuSO4 solution, then pour in a Na2S2O3 solution, and then add a 10% citric acid solution to adjust the pH to 4.5, oscillate at 65°C for 2 hours, and after the oscillation, wash thoroughly with deionized water until the washing liquid is completely clear, and dry naturally to obtain CuS / polydopamine leather.

[0036] Example 3

[0037] The preparation method of CuS / polydopamine heated leather specifically comprises the following steps:

[0038] Step 1: prepare a polydopamine solution, dissolve 2 mg / mL dopamine hydrochloride in 10 mM tris buffer solution, then add 5 mM copper sulfate and 19.6 mM hydrogen peroxide to obtain a polydopamine solution; quickly immerse the leather in the polydopamine solution, let it stand at 30° C. for 0.8 h, then take it out, wash the leather thoroughly with deionized water until the washing solution is completely clear, and finally dry it to obtain polydopamine leather;

[0039] Step 2: Prepare a CuSO4 solution and a Na2S2O3 solution of the same concentration, dissolve the CuSO4 and Na2S2O3 in deionized water to obtain a CuSO4 solution and a Na2S2O3 solution, respectively, wherein the concentration of the CuSO4 solution is 200 mM;

[0040] Step 3: Place the polydopamine leather obtained in step 1 in a CuSO4 solution, then pour in a Na2S2O3 solution, and then add a 10% citric acid solution to adjust the pH to 4.3, oscillate at 65°C for 1.5 hours, and after the oscillation, wash thoroughly with deionized water until the washing liquid is completely clear, and dry naturally to obtain CuS / polydopamine leather.

Claims

1. A method for preparing CuS / polydopamine heated leather, characterized in that: The specific steps include: Step 1: prepare a polydopamine solution, immerse the leather in the polydopamine solution and let it stand, then take it out and wash it thoroughly with deionized water, and finally dry it to obtain polydopamine leather; Step 2: Prepare CuSO4 solution and Na2S2O3 solution of the same concentration; Step 3: Place the polydopamine leather obtained in step 1 in a CuSO4 solution, then pour in a Na2S2O3 solution, and then add a citric acid solution to adjust the pH to 4-4.5, and shake. After the shaking, wash it thoroughly with deionized water until the washing liquid is completely clear, and dry it naturally to obtain CuS / polydopamine leather.

2. The method for preparing CuS / polydopamine heated leather according to claim 1, characterized in that: In step 1, the specific steps of preparing the polydopamine solution are: 2 mg / mL dopamine hydrochloride was dissolved in 10 mM Tris buffer solution, followed by the addition of 5 mM copper sulfate and 19.6 mM hydrogen peroxide.

3. The method for preparing CuS / polydopamine heated leather according to claim 2, characterized in that: In step 1, the specific steps of leather immersion and washing are: The leather is quickly immersed in the polydopamine solution, left to stand at 25-35° C. for 0.5-1 hour, then taken out, and the leather is fully washed with deionized water until the washing solution is completely clarified, and finally dried to obtain the polydopamine leather.

4. The method for preparing CuS / polydopamine heated leather according to claim 3, characterized in that: In step 2, the specific steps of preparing the CuSO4 solution and the Na2S2O3 solution are: CuSO4 and Na2S2O3 are dissolved in deionized water to obtain CuSO4 solution and Na2S2O3 solution respectively, and the concentration of the CuSO4 solution is 50-350 mM.

5. The method for preparing CuS / polydopamine heated leather according to claim 4, characterized in that: In step S3, the concentration of the citric acid solution is 10%.

6. The method for preparing CuS / polydopamine heated leather according to claim 5, characterized in that: In step S3, the process parameters of oscillation are oscillation at 65° C. for 1-2 hours.

Citation Information

Patent Citations

  • Preparation method of double-mode heating cotton fabric with photothermal conversion and Joule heating performance

    CN117265881A

  • Multifunctional wearable fabric heater and preparation method thereof

    CN117449091A