Non-magnetic self-lubricating fitting material and preparation method thereof
By using non-magnetic self-lubricating metal materials in iron metal tools, and using spherical graphite and austenite + Mo and V carbide tissues, the hysteresis loss, wear resistance and corrosion resistance of iron metal tools are solved, and the problem of hysteresis loss, wear resistance and corrosion resistance of iron metal tools is achieved. Higher wear and corrosion resistance, reducing power loss and environmental pollution.
Patent Information
- Application Number
- CN202411331603.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-24
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-09-24
AI Technical Summary
The existing iron metal tools have large hysteresis losses due to strong magnetism, resulting in high power loss and electricity bill losses, and are not wear-resistant and corrosion-resistant.
Using magnetically-free self-lubricating metal materials, through specific proportions of element composition and process processing, a spherical graphite self-lubricating film and austenite + Mo and V carbide tissue are formed to reduce magnetic properties, improve wear resistance and corrosion resistance, and through Martensite phase transformation improves hardness.
It significantly reduces hysteresis loss, improves the wear and corrosion resistance of the metal, extends the service life, and reduces environmental pollution.
Smart Images

Figure CN118910496A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of hardware materials, and in particular relates to a non-magnetic self-lubricating hardware material. The invention also relates to a preparation method of the non-magnetic self-lubricating hardware material. Background Art
[0002] Hardware plays a very important role in power transmission and transformation projects. Its quality stability and reliability directly determine the safe operation of the power grid system. In recent years, with the rapid development of my country's power industry, accompanied by the characteristics of large transmission capacity, long distance, and the need to pass through a variety of complex climate and geomorphic regions, the power system has put forward higher requirements for the electrical performance, mechanical performance, reliability, durability, energy saving, and economy of power hardware for overhead transmission lines. At present, the commonly used materials for power transmission line hardware are mainly malleable cast iron, weathering steel, aluminum and aluminum alloy. Malleable cast iron and steel hardware have excellent mechanical properties, but there are pain points such as inconvenient installation, corrosion resistance, hysteresis and eddy current loss. Aluminum hardware solves the above problems very well, but the price of aluminum hardware is relatively high, and the strength of aluminum and aluminum alloy is relatively low, which is difficult to meet the requirements of the power industry. It can only be used in environments where mechanical properties are not demanding.
[0003] Iron fittings account for the largest share, but they face three major pain points: 1. Not corrosion-resistant; 2. Not wear-resistant; 3. Large power loss. The loss of iron fittings during operation accounts for about 0.01-0.03% of the transmission capacitor. According to statistics, at an operating current of 400A, the hysteresis eddy current power loss of iron suspension clamps reaches 39W. The total power loss caused by iron suspension clamps in high-voltage lines across the country exceeds 340 million kW·h / year, and the total electricity bill loss reaches 130 million yuan / year. Summary of the invention
[0004] The purpose of the present invention is to provide a non-magnetic self-lubricating hardware material, which solves the problem of large hysteresis loss of existing iron hardware materials due to strong magnetism.
[0005] Another object of the present invention is to provide a method for preparing a non-magnetic self-lubricating hardware material.
[0006] The technical solution adopted by the present invention is that the non-magnetic self-lubricating hardware material is composed of the following raw materials in terms of mass percentage: C 3.3%-3.8%, Si 2.0%-2.6%, Ni 10%-14%, Mo 0.5%-1.0%, V 0.5%-1.0%, Mn 0.1%-0.2%, P≤0.1%, S≤0.015%, and the balance is Fe, and the sum of the contents of the above components is 100%.
[0007] Another technical solution adopted by the present invention is a method for preparing a non-magnetic self-lubricating hardware material, which is specifically implemented according to the following steps:
[0008] Step 1, according to the following material mass percentages: C3.3%-3.8%, Si2.0%-2.6%, Ni10%-14%, Mo0.5%-1.0%, V0.5%-1.0%, Mn0.1%-0.2%, P≤0.1%, S≤0.015%, the balance is Fe, the sum of the contents of the above components is 100%, weigh bread iron, ferrosilicon, nickel plate, ferrochrome, ferromolybdenum, ferrovanadium, and carburizer;
[0009] Step 2, placing the raw materials weighed in step 1 in a medium frequency furnace to melt at high temperature to obtain a first liquid;
[0010] Step 3, pouring the first liquid into a holding furnace, and adding a silicon-barium inoculant and a rare earth magnesium spheroidizer into the holding furnace and stirring thoroughly to obtain a second liquid;
[0011] Step 4, pouring the second liquid into the preheated horizontal continuous casting furnace, and obtaining the first metal part by a horizontal continuous casting method;
[0012] Step 5, placing the first metal piece in a vacuum furnace, introducing argon gas, keeping the temperature, and then cooling the first metal piece to room temperature with water to obtain a second metal piece;
[0013] Step 6, placing the second metal part in a muffle furnace for low temperature tempering to obtain a third metal part;
[0014] Step 7: Machine the third metal part into a metal fitting shape.
[0015] Another technical solution of the present invention is also characterized in that:
[0016] In step 3, the amount of silicon-barium inoculant added is 1.0% to 1.5% of the mass of the first liquid, and the amount of rare earth magnesium spheroidizer added is 1.0% to 2.0% of the mass of the first liquid.
[0017] In step 5, the vacuum pressure in the vacuum furnace is not greater than -0.1 MPa, and the interval time for taking the first metal out of the vacuum furnace for water quenching is not greater than 30 seconds.
[0018] In step 5, the temperature of the vacuum furnace is 1050° C. to 1150° C., and the insulation time is 4 h to 8 h.
[0019] In step 6, the insulation temperature of the muffle furnace is 100° C. to 200° C., and the insulation time is 1 h to 4 h.
[0020] The matrix structures of the second metal part and the third metal part are both austenite + Mo, V carbides.
[0021] The beneficial effects of the present invention are:
[0022] 1) The non-magnetic self-lubricating hardware material contains no less than 10% volume fraction of spherical graphite, which can form a self-lubricating film during service to improve the wear resistance of the hardware;
[0023] 2) The matrix structure of non-magnetic self-lubricating hardware is austenite, which has low magnetism and can greatly reduce electromagnetic loss;
[0024] 3) The austenite in the matrix of the non-magnetic self-lubricating hardware provides high plasticity and toughness, and the Mo and V carbides provide high strength, ensuring the excellent mechanical properties of the material;
[0025] 4) The austenite in the matrix of non-magnetic self-lubricating hardware has high corrosion resistance, which avoids the process of using hot-dip galvanizing on the surface of traditional iron hardware to improve corrosion resistance and reduces environmental pollution;
[0026] 5) During the service of non-magnetic self-lubricating hardware, such as sandstorm impact, the austenite in it can induce martensitic phase transformation through strain to increase the hardness of the material and further improve its wear resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 is a microstructure photograph of the distribution state of spheroidal graphite in the cast iron material prepared in Example 1 of the present invention;
[0028] Figure 2 is a scanning microstructure image of the cast iron material prepared in Example 2 of the present invention;
[0029] Figure 3 This is a scanning microstructure image of the XRD image of the material after heat treatment in Example 3 of the present invention;
[0030] Figure 4 is a scanning microstructure image of the material after heat treatment in Example 4 of the present invention;
[0031] Figure 5 This is an EDS image of the material after heat treatment in Example 4 of the present invention. DETAILED DESCRIPTION
[0032] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0033] The non-magnetic self-lubricating hardware material is composed of the following raw materials in terms of mass percentage: C 3.3%-3.8%, Si 2.0%-2.6%, Ni 10%-14%, Mo 0.5%-1.0%, V 0.5%-1.0%, Mn 0.1%-0.2%, P≤0.1%, S≤0.015%, and the balance is Fe, and the sum of the contents of the above components is 100%.
[0034] The preparation method of the non-magnetic self-lubricating hardware material is specifically implemented according to the following steps:
[0035] Step 1, according to the following material mass percentages: C3.3%-3.8%, Si2.0%-2.6%, Ni10%-14%, Mo0.5%-1.0%, V0.5%-1.0%, Mn0.1%-0.2%, P≤0.1%, S≤0.015%, the balance is Fe, the sum of the contents of the above components is 100%, weigh bread iron, ferrosilicon, nickel plate, ferrochrome, ferromolybdenum, ferrovanadium, and carburizer;
[0036] Step 2, placing the raw materials weighed in step 1 in a medium frequency furnace to melt at high temperature to obtain a first liquid;
[0037] Step 3, pouring the first liquid into a holding furnace, and adding a silicon-barium inoculant and a rare earth magnesium spheroidizer into the holding furnace and stirring thoroughly to obtain a second liquid;
[0038] In step 3, the amount of silicon-barium inoculant added is 1.0% to 1.5% of the mass of the first liquid, the amount of rare earth magnesium spheroidizer added is 1.0% to 2.0% of the mass of the first liquid, and the residual magnesium content in the final material is controlled to be 0.02% to 0.05% of the mass of the first liquid, and the rare earth element content is 0.02% to 0.05% of the mass of the first liquid;
[0039] The addition of spheroidizer and inoculant is to promote graphitization, improve the graphite morphology and distribution, and obtain evenly distributed spherical graphite;
[0040] Step 4, pouring the second liquid into the preheated horizontal continuous casting furnace, and obtaining the first metal part by a horizontal continuous casting method;
[0041] Step 5, placing the first metal piece in a vacuum furnace, introducing argon gas, keeping the temperature, and then cooling the first metal piece to room temperature with water to obtain a second metal piece;
[0042] In step 5, the vacuum pressure in the vacuum furnace is not greater than -0.1 MPa, and the interval time between taking the first metal out of the vacuum furnace and water quenching is not greater than 30 seconds, in order to prevent the precipitation of carbon dissolved in the γ phase;
[0043] In step 5, the temperature of the vacuum furnace is 1050° C. to 1150° C., and the holding time is 4 h to 8 h;
[0044] Ni is an austenite stabilizing element. 1050℃~1150℃ can make the Ni element more evenly distributed to obtain a fully austenite structure and a non-magnetic, corrosion-resistant matrix; Mo and V elements can form dispersed carbides to improve material strength;
[0045] Step 6, placing the second metal part in a muffle furnace for low-temperature tempering, the purpose of tempering is to eliminate stress, and obtaining a third metal part;
[0046] In step 6, the holding temperature of the muffle furnace is 100° C. to 200° C., and the holding time is 1 h to 4 h;
[0047] The matrix structures of the second metal part and the third metal part are austenite + Mo and V carbides;
[0048] Step 7: Machine the third metal part into a metal fitting shape.
[0049] Example 1
[0050] The preparation method of the non-magnetic self-lubricating hardware material is specifically implemented according to the following steps:
[0051] Step 1, weigh the raw materials according to the material mass percentage: C3.4%, Si2.0%, Ni11%, Mo0.6%, V0.6%, Mn0.15%, P 0.03%, S0.01%, the balance is Fe, and the raw materials are bread iron, ferrosilicon, nickel plate, ferrochrome, ferromolybdenum, ferrovanadium, and carburizer;
[0052] Step 2, melting the weighed raw materials in a medium frequency furnace at high temperature to obtain a first liquid;
[0053] Step 3, pouring the first liquid into a holding furnace, adding 1.3% of the mass of the first liquid silicon barium inoculant and 1.8% of the mass of the first liquid rare earth magnesium spheroidizer thereto and stirring thoroughly to obtain a second liquid;
[0054] Step 4, pouring the second liquid into the preheated horizontal continuous casting furnace, and obtaining a casting, namely the first metal, by a horizontal continuous casting method;
[0055] Step 5, placing the first metal piece in a vacuum furnace at 1100°C with a vacuum pressure of -0.2MPa, introducing argon gas, keeping the temperature for 6 hours, and then cooling the furnace to room temperature with water to obtain a second metal piece;
[0056] Step 6, placing the second metal piece in a muffle furnace at 200° C. for 2 hours and then air-cooling to room temperature to obtain a third metal piece;
[0057] Step 7: The third metal part is machined into a metal fitting shape.
[0058] Example 2
[0059] The preparation method of the non-magnetic self-lubricating hardware material is specifically implemented according to the following steps:
[0060] Step 1, weigh the raw materials according to the material mass percentage: C3.6%, Si2.2%, Ni10%, Mo0.6%, V0.6%, Mn0.12%, P 0.02%, S0.01%, the balance is Fe, and the raw materials are bread iron, ferrosilicon, nickel plate, ferrochrome, ferromolybdenum, ferrovanadium, and carburizer;
[0061] Step 2, melting the weighed raw materials in a medium frequency furnace at high temperature to obtain a first liquid;
[0062] Step 3, pouring the first liquid into a holding furnace, adding 1.0% of the mass of the first liquid silicon barium inoculant and 1.0% of the mass of the first liquid rare earth magnesium spheroidizer thereto and stirring thoroughly to obtain a second liquid;
[0063] Step 4, pouring the second liquid into the preheated horizontal continuous casting furnace, and obtaining a casting, namely the first metal, by a horizontal continuous casting method;
[0064] Step 5, placing the first metal piece in a vacuum furnace at 1050° C. with a vacuum pressure of -0.2 MPa, introducing argon gas, keeping the temperature for 8 hours, and then cooling the furnace to room temperature with water to obtain a second metal piece;
[0065] Step 6, placing the second metal piece in a muffle furnace at 200° C. for 4 hours and then air-cooling to room temperature to obtain a third metal piece;
[0066] Step 7: The third metal part is machined into a metal fitting shape.
[0067] Example 3
[0068] The preparation method of the non-magnetic self-lubricating hardware material is specifically implemented according to the following steps:
[0069] Step 1, weigh the raw materials according to the material mass percentage: C3.5%, Si2.6%, Ni12%, Mo0.7%, V0.5%, Mn0.1%, P0.02%, S0.01%, the balance is Fe, and the raw materials are bread iron, ferrosilicon, nickel plate, ferrochrome, ferromolybdenum, ferrovanadium, and carburizer;
[0070] Step 2, melting the weighed raw materials in a medium frequency furnace at high temperature to obtain a first liquid;
[0071] Step 3, pouring the first liquid into a holding furnace, adding 1.5% of the mass of the first liquid silicon barium inoculant and 2.0% of the mass of the first liquid rare earth magnesium spheroidizer thereto and stirring thoroughly to obtain a second liquid;
[0072] Step 4, pouring the second liquid into the preheated horizontal continuous casting furnace, and obtaining a casting, namely the first metal, by a horizontal continuous casting method;
[0073] Step 5, placing the first metal piece in a vacuum furnace at 1120° C. with a vacuum pressure of -0.2 MPa, introducing argon gas, keeping the temperature for 5 hours, and then cooling the furnace to room temperature with water to obtain a second metal piece;
[0074] Step 6, placing the second metal piece in a muffle furnace at 150° C. for 3 hours and then air-cooling to room temperature to obtain a third metal piece;
[0075] Step 7: The third metal part is machined into a metal fitting shape.
[0076] Example 4
[0077] The preparation method of the non-magnetic self-lubricating hardware material is specifically implemented according to the following steps:
[0078] Step 1, weigh the raw materials according to the material mass percentage: C3.5%, Si2.5%, Ni13%, Mo0.5%, V0.8%, Mn0.13%, P 0.03%, S0.01%, the balance is Fe, and the raw materials are bread iron, ferrosilicon, nickel plate, ferrochrome, ferromolybdenum, ferrovanadium, and carburizer;
[0079] Step 2, melting the weighed raw materials in a medium frequency furnace at high temperature to obtain a first liquid;
[0080] Step 3, pouring the first liquid into a holding furnace, adding 1.4% of the mass of the first liquid silicon barium inoculant and 1.7% of the mass of the first liquid rare earth magnesium spheroidizer thereto and stirring thoroughly to obtain a second liquid;
[0081] Step 4, pouring the second liquid into the preheated horizontal continuous casting furnace, and obtaining a casting, namely the first metal, by a horizontal continuous casting method;
[0082] Step 5, placing the first metal piece in a vacuum furnace at 1080°C with a vacuum pressure of -0.2MPa, introducing argon gas, keeping the temperature for 6 hours, and then cooling the furnace to room temperature with water to obtain a second metal piece;
[0083] Step 6, placing the second metal piece in a muffle furnace at 180° C. for 3 hours and then air-cooling to room temperature to obtain a third metal piece;
[0084] Step 7: The third metal part is machined into a metal fitting shape.
[0085] The non-magnetic self-lubricating hardware material prepared by the present invention has a large number of fine and evenly distributed spherical graphites embedded in the material structure, such as Figure 1 As shown in the figure, it can form a graphite film on the surface of the hardware during service, reduce the friction coefficient of the hardware during service, improve the wear resistance, and achieve self-lubricating properties. Figure 2 As shown in the figure, the structure is bainite + martensite. The XRD test results of the metal casting after heat treatment are as follows Figure 3 As shown in the figure, the structure is full austenite. In addition, Mo and V carbides are also dispersed in the matrix structure, such as Figure 4 As shown, the EDS spectrum of carbide is as follows Figure 5As shown. Supersaturated austenite and Mo, V carbides provide high strength, and austenite provides high plastic toughness, thereby ensuring good mechanical properties of the material. Austenite has excellent corrosion resistance, which can effectively avoid the current situation of traditional iron hardware using surface hot-dip galvanizing for corrosion protection, which can reduce costs and reduce environmental pollution. On the other hand, the non-magnetic characteristics of austenite can greatly reduce hysteresis losses and save energy. In summary, the non-magnetic self-lubricating hardware of the present invention can solve the problems faced by existing iron hardware: (1) not wear-resistant; (2) not corrosion-resistant; (3) large power loss and other problems, and effectively improve its service life.
Claims
1. Non-magnetic self-lubricating hardware materials, It is characterized in that It is composed of the following raw material components in mass percentage: C 3.3%-3.8%, Si 2.0%-2.6%, Ni 10%-14%, Mo 0.5%-1.0%, V 0.5%-1.0%, Mn 0.1%-0.2%, P≤0.1%, S≤0.015%, and the balance is Fe. The total content of the above components is 100%.
2. Preparation method of non-magnetic self-lubricating hardware material, It is characterized in that Follow the steps below to implement it: Step 1, according to the following material mass percentages: C3.3%-3.8%, Si2.0%-2.6%, Ni10%-14%, Mo0.5%-1.0%, V0.5%-1.0%, Mn 0.1%-0.2%, P≤0.1%, S≤0.015%, the balance is Fe, the sum of the contents of the above components is 100%, weigh bread iron, ferrosilicon, nickel plate, ferrochrome, ferromolybdenum, ferrovanadium, and carburizer; Step 2, placing the raw materials weighed in step 1 in a medium frequency furnace to melt at high temperature to obtain a first liquid; Step 3, pouring the first liquid into a holding furnace, and adding a silicon-barium inoculant and a rare earth magnesium spheroidizer into the holding furnace and stirring thoroughly to obtain a second liquid; Step 4, pouring the second liquid into the preheated horizontal continuous casting furnace, and obtaining the first metal part by a horizontal continuous casting method; Step 5, placing the first metal piece in a vacuum furnace, introducing argon gas, keeping the temperature, and then cooling the first metal piece to room temperature with water to obtain a second metal piece; Step 6, placing the second metal part in a muffle furnace for low temperature tempering to obtain a third metal part; Step 7: Machine the third metal part into a metal fitting shape.
3. The method for preparing the non-magnetic self-lubricating hardware material according to claim 2, It is characterized in that In step 3, the amount of silicon-barium inoculant added is 1.0% to 1.5% of the mass of the first liquid, and the amount of rare earth magnesium spheroidizer added is 1.0% to 2.0% of the mass of the first liquid.
4. The method for preparing the non-magnetic self-lubricating hardware material according to claim 2, It is characterized in that In the step 5, the vacuum pressure in the vacuum furnace is not greater than -0.1 MPa, and the interval time for taking the first metal out of the vacuum furnace for water quenching is not greater than 30 seconds.
5. The method for preparing the non-magnetic self-lubricating hardware material according to claim 2, It is characterized in that In step 5, the temperature of the vacuum furnace is 1050° C. to 1150° C., and the insulation time is 4 h to 8 h.
6. The method for preparing the non-magnetic self-lubricating hardware material according to claim 2, It is characterized in that In step 6, the insulation temperature of the muffle furnace is 100° C. to 200° C., and the insulation time is 1 h to 4 h.
7. The method for preparing the non-magnetic self-lubricating hardware material according to claim 2, It is characterized in that The matrix structures of the second metal part and the third metal part are both austenite+Mo and V carbides.
Citation Information
Patent Citations
Method for preparing chromium-iron-based high-temperature self-lubricating block material
CN104928584A
Non-magnetic nodular cast iron and preparation method thereof
CN109182891A
Alloy for aluminum alloy cutting saw and preparation method of alloy
CN113862554A
Manufacturing method of self-lubricating precision wire drawing die for non-ferrous metals such as copper, aluminum, stainless steel and like
CN114952209A
Self-lubricating and high-wear-resistance aluminum alloy turning blade material and preparation method thereof
CN116770164A