Semiconductor device and manufacturing method and device of hafnium oxide film layer

During the production process of the hafnium oxide film layer, the hafnium source and oxygen are alternately passed to one side of the substrate to form a hafnium oxide film layer including the first hafnium oxide layer and the second hafnium oxide layer, and the problem of poor film layer quality is solved. , high step coverage, continuity and refractive index uniformity of the film layer are achieved.

CN118910546APending Publication Date: 2024-11-08GUANGCHI SEMICON TECH (SHANGHAI) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410967599.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing hafnium oxide film layer production methods have problems with poor film quality, including difficulty in controlling thickness uniformity and uneven refractive index.

Method used

By passing hafnium source and first oxygen source to one side of the substrate, a first hafnium oxide layer is formed, and then passing hafnium source and oxygen to the side of the first hafnium oxide layer away from the substrate, forming a second hafnium oxide layer, forming a second hafnium oxide layer, including A hafnium oxide film layer of the hafnium monoxide layer and the second hafnium oxide layer.

Benefits of technology

The film quality of the hafnium oxide film layer is improved, the step coverage is high, the film layer continuity is good, the film layer thickness is uniform, the refractive index is close to the actual refractive index of hafnium oxide, and the hafnium oxide in the hafnium oxide film layer is high.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910546A_ABST
    Figure CN118910546A_ABST
Patent Text Reader

Abstract

The invention discloses a semiconductor device and a manufacturing method and device of a hafnium oxide film layer. The manufacturing method of the hafnium oxide film layer comprises the following steps: providing a substrate; introducing a hafnium source and a first oxygen source into one side of the substrate to form a first hafnium oxide layer; the hafnium source and a second oxygen source are introduced into the side, away from the substrate, of the first hafnium oxide layer to form a second hafnium oxide layer, the hafnium oxide film layer comprises the first hafnium oxide layer and the second hafnium oxide layer, and the second oxygen source comprises oxygen. The invention provides a semiconductor device and a manufacturing method and device of a hafnium oxide film layer, which can improve the film layer quality of the hafnium oxide film layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of atomic layer deposition, and in particular to a method and device for manufacturing a semiconductor device and a hafnium oxide film layer. Background Art

[0002] Hafnium oxide has the characteristics of high dielectric constant, high refractive index and high melting point, and has broad application prospects in the semiconductor and optical fields.

[0003] However, the hafnium oxide film produced by the existing hafnium oxide film production method has the problem of poor film quality, which is specifically manifested in that the thickness uniformity of the hafnium oxide film is difficult to control and the refractive index is uneven in the region. Summary of the invention

[0004] The present invention provides a semiconductor device, a method and a device for manufacturing a hafnium oxide film layer, which can improve the film quality of the hafnium oxide film layer.

[0005] According to one aspect of the present invention, a method for manufacturing a hafnium oxide film layer is provided, the manufacturing method comprising:

[0006] providing a substrate;

[0007] introducing a hafnium source and a first oxygen source into one side of the substrate to form a first hafnium oxide layer;

[0008] The hafnium source and the second oxygen source are introduced into a side of the first hafnium oxide layer away from the substrate to form a second hafnium oxide layer, wherein the hafnium oxide film layer includes the first hafnium oxide layer and the second hafnium oxide layer, and the second oxygen source includes oxygen.

[0009] Optionally, the first oxygen source includes at least one of ozone and water vapor; and the hafnium source includes dimethylamine.

[0010] Optionally, the step of introducing a hafnium source and a first oxygen source into one side of the substrate to form the first hafnium oxide layer specifically includes:

[0011] The hafnium source and the first oxygen source are alternately introduced into one side of the substrate for a first set number of times to form the first hafnium oxide layer.

[0012] Optionally, the alternately introducing the hafnium source and the first oxygen source a first set number of times to form the first hafnium oxide layer specifically includes:

[0013] Open the first purge valve and introduce purge gas;

[0014] When the purge gas of the first set time is introduced, the hafnium source valve is opened and the hafnium source is introduced;

[0015] When the hafnium source is introduced for a second set time, closing the hafnium source valve;

[0016] When the hafnium source valve is closed for a third set time, closing the first purge valve;

[0017] When the first purge valve is closed for a fourth set time, the second purge valve is opened to allow purge gas to pass;

[0018] When the second purge valve is opened for a fifth set time, the first oxygen source valve is opened to introduce the first oxygen source;

[0019] When the first oxygen source is introduced for a sixth set time, closing the first oxygen source valve;

[0020] When the first oxygen source valve is closed for a seventh set time, closing the second purge valve;

[0021] When the second purge valve is closed for an eighth set time, determining whether the number of times the hafnium source is introduced is less than the first set number of times;

[0022] If yes, the process returns to the step of opening the first purge valve and introducing the purge gas; if no, it indicates that the first hafnium oxide film layer is formed.

[0023] Optionally, the step of introducing the hafnium source and the second oxygen source into a side of the first hafnium oxide layer away from the substrate to form the second hafnium oxide layer specifically includes:

[0024] The second hafnium oxide layer is formed by alternately introducing the hafnium source and the second oxygen source for a second set number of times toward a side of the first hafnium oxide layer away from the substrate.

[0025] Optionally, the alternately introducing the hafnium source and the second oxygen source a second set number of times to form the second hafnium oxide layer specifically includes:

[0026] Open the first purge valve and introduce purge gas;

[0027] When the purge gas of the first set time is introduced, the hafnium source valve is opened and the hafnium source is introduced;

[0028] When the hafnium source is introduced for a second set time, closing the hafnium source valve;

[0029] When the hafnium source valve is closed for a third set time, closing the first purge valve;

[0030] When the first purge valve is closed for a fourth set time, the third purge valve is opened to allow the purge gas to pass;

[0031] When the third purge valve is opened for a ninth set time, the second oxygen source valve is opened and the second oxygen source is introduced;

[0032] When the second oxygen source is introduced for a tenth set time, closing the second oxygen source valve;

[0033] When the second oxygen source valve is closed for an eleventh set time, closing the third purge valve;

[0034] When the third purge valve is closed for a twelfth set time, determining whether the number of times the hafnium source is introduced is less than a second set number of times;

[0035] If yes, the process returns to the step of opening the first purge valve and introducing the purge gas; if no, it indicates that the second hafnium oxide film layer is formed.

[0036] Optionally, the first set time length ranges from 0.1s to 1.5s; the second set time length ranges from 0.3s to 1.7s; the third set time length ranges from 7s to 15s; the fourth set time length ranges from 2s to 7s; the ninth set time length ranges from 0.1s to 1.5; the tenth set time length ranges from 0.1s to 1s; the eleventh set time length ranges from 0.5s to 6s; the twelfth set time length ranges from 5s to 14s.

[0037] Optionally, the second set number of times is greater than the first set number of times.

[0038] According to another aspect of the present invention, there is provided a semiconductor device, the semiconductor device comprising a hafnium oxide film layer;

[0039] The hafnium oxide film layer is manufactured by the method for manufacturing a hafnium oxide film layer provided by any embodiment of the present invention.

[0040] According to another aspect of the present invention, a manufacturing device for a hafnium oxide film layer is provided, the manufacturing device comprising a substrate providing module, a first hafnium oxide layer forming module and a second hafnium oxide layer forming module;

[0041] The substrate providing module is used to provide a substrate;

[0042] The first hafnium oxide layer forming module is used to introduce a hafnium source and a first oxygen source into one side of the substrate to form a first hafnium oxide layer;

[0043] The second hafnium oxide layer forming module is used to introduce the hafnium source and the second oxygen source into the side of the first hafnium oxide layer away from the substrate to form a second hafnium oxide layer, wherein the hafnium oxide film layer includes the first hafnium oxide layer and the second hafnium oxide layer, and the second oxygen source includes oxygen.

[0044] The present embodiment provides a method for manufacturing a hafnium oxide film layer, the manufacturing method comprising: first providing a substrate, then introducing a hafnium source and a first oxygen source into one side of the substrate to form a first hafnium oxide layer, and then introducing a hafnium source and oxygen into the side of the first hafnium oxide layer away from the substrate to form a second hafnium oxide layer, thereby finally forming a hafnium oxide film layer including the first hafnium oxide layer and the second hafnium oxide layer. In the present embodiment, oxygen is added during the manufacturing of the hafnium oxide film layer, so that the step coverage of the manufactured hafnium oxide film layer is high, the film layer continuity is good, the film layer thickness is uniform, and the refractive index of the manufactured hafnium oxide film layer is close to the actual refractive index of hafnium oxide, and the purity of hafnium oxide in the hafnium oxide film layer is high. In summary, the manufacturing method of the hafnium oxide film layer provided in the present embodiment can improve the film quality of the hafnium oxide film layer.

[0045] It should be understood that the contents described in this section are not intended to identify the key or important features of the embodiments of the present invention, nor are they intended to limit the scope of the present invention. Other features of the present invention will become easily understood through the following description. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0047] Figure 1 is a schematic flow chart of a method for manufacturing a hafnium oxide film layer provided according to an embodiment of the present invention;

[0048] Figure 2 is a schematic structural diagram of a hafnium oxide film layer manufactured according to the method for manufacturing a hafnium oxide film layer provided in an embodiment of the present invention;

[0049] Figure 3 is a schematic structural diagram of a hafnium oxide film layer provided according to an embodiment of the present invention;

[0050] Figure 4 is a schematic diagram of thicknesses corresponding to different regions of a hafnium oxide film layer provided in an embodiment of the present invention;

[0051] Figure 5 is a schematic diagram of the refractive index corresponding to different regions of a hafnium oxide film layer provided according to an embodiment of the present invention;

[0052] Figure 6 Schematic diagram of the structure of a device for manufacturing a hafnium oxide film layer provided according to an embodiment of the present invention. DETAILED DESCRIPTION

[0053] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0054] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.

[0055] Figure 1 is a schematic diagram of a process for manufacturing a hafnium oxide film layer according to an embodiment of the present invention, with reference to Figure 1 The method for manufacturing the hafnium oxide film provided in this embodiment comprises the following steps:

[0056] S110, providing a substrate.

[0057] Specifically, the material of the substrate may be glass or silicon. The substrate may be located in an atomic layer deposition chamber.

[0058] S120, introducing a hafnium source and a first oxygen source into one side of the substrate to form a first hafnium oxide layer.

[0059] Specifically, the first hafnium oxide layer can be formed by atomic layer deposition. The first oxygen source can be ozone or water vapor. The hafnium source can be CpHf(NMe2)3. The temperature range of the hafnium source introduced into the atomic layer deposition chamber can be 140°C to 150°C. The hafnium source and the first oxygen source can be introduced alternately during the formation of the first hafnium oxide layer. Before executing step S120, the substrate can be heated to a first set temperature. Heating the substrate to the first set temperature is conducive to the formation of the hafnium oxide film layer. The first set temperature can be 200°C or greater than 200°C.

[0060] S130, introducing a hafnium source and a second oxygen source into a side of the first hafnium oxide layer away from the substrate to form a second hafnium oxide layer, wherein the hafnium oxide film layer includes the first hafnium oxide layer and the second hafnium oxide layer, and the second oxygen source includes oxygen.

[0061] Specifically, the second hafnium oxide layer is located on a side of the first hafnium oxide layer away from the substrate. The second hafnium oxide layer can be formed by atomic layer deposition. During the formation of the second hafnium oxide layer, a hafnium source and a second oxygen source can be alternately introduced. The temperature of the oxygen introduced can be room temperature, and the pressure of the oxygen introduced can be 0.2 MPa.

[0062] In this embodiment, a hafnium source and a first oxygen source are first introduced to form a first hafnium oxide layer, and then a hafnium source and oxygen are introduced to form a second hafnium oxide layer, and finally a hafnium oxide film layer including a first hafnium oxide layer and a second hafnium oxide layer is formed. The hafnium oxide film layer provided in this embodiment has good film quality, a step coverage rate of more than 83%, and an 8-inch area uniformity of ±0.42%. The calculation method of the area uniformity is: (T max -T min ) / (2*T ave ), where T max is the maximum thickness of the hafnium oxide film in the region, T min is the minimum thickness of the hafnium oxide film in the region, T ave is the average thickness of the hafnium oxide film in the region.

[0063] The following table shows the step coverage of different regions in the hafnium oxide film layer manufactured by the method for manufacturing the hafnium oxide film layer provided by the embodiment of the present invention:

[0064]

[0065] Part 1, Part 2, Part 3, and Part 4 refer to four different regions in the manufactured hafnium oxide film layer. Figure 2 Schematic diagram of the structure of a hafnium oxide film layer made by the method for making a hafnium oxide film layer provided in an embodiment of the present invention, with reference to Figure 2 , Figure 2 The substrate includes a protruding pillar 100, and the hafnium oxide film 110 manufactured on the surface of the substrate having the pillar 100 by using the manufacturing method provided by the embodiment of the present invention has the advantages of good step coverage, no film breakage and good thickness uniformity. Figure 3 is a schematic diagram of the structure of a hafnium oxide film layer provided according to an embodiment of the present invention, with reference to Figure 3, in the above table, Sidewall step Coverage=a / b*100%,Bottom step Coverage=d / b*100%,Conformality=a / c*100%. Wherein, a may be the minimum thickness of one of the sidewalls in the hafnium oxide film layer 110, c may be the maximum thickness of one of the sidewalls in the hafnium oxide film layer 110, b may be the maximum thickness of the top of one of the pillars 110 in the hafnium oxide film layer 110, and d may be the maximum thickness of the hafnium oxide film layer 110 located between two pillars 110 in the hafnium oxide film layer 110.

[0066] Figure 4 is a schematic diagram of thicknesses corresponding to different regions of a hafnium oxide film layer provided according to an embodiment of the present invention, with reference to Figure 4 , Figure 4 The abscissa in represents the length of the hafnium oxide film layer in the first direction. Figure 4 The ordinate in represents the length of the hafnium oxide film layer in the second direction. Figure 4 The colored bar on the right side of the graph represents the thickness of the hafnium oxide film layer, where the first direction is perpendicular to the second direction. Figure 4 It can be seen that the thickness of the hafnium oxide film layer in each region is within the range of 15.272nm to 15.466nm, and the thickness difference of the hafnium oxide film layer in different regions is small. It can be seen that the thickness uniformity of the hafnium oxide film layer manufactured by the manufacturing method provided in this embodiment is good. Figure 5 is a schematic diagram of the refractive index corresponding to different regions of a hafnium oxide film layer provided according to an embodiment of the present invention, with reference to Figure 5 , Figure 5 The abscissa in represents the length of the hafnium oxide film layer in the first direction. Figure 5 The ordinate in represents the length of the hafnium oxide film layer in the second direction. Figure 5 The colored bar on the right side of the graph represents the refractive index of the hafnium oxide film. Figure 5 It can be seen that the refractive index of the hafnium oxide film layer in each region is within the range of 1.9683 to 1.9987. In practice, the refractive index of hafnium oxide is about 2. It can be seen that the refractive index of the hafnium oxide film layer prepared by the manufacturing method provided in this embodiment is consistent with the refractive index of hafnium oxide, the purity of hafnium oxide in the prepared hafnium oxide film layer is high, and the refractive index has good uniformity in different regions.

[0067] The present embodiment provides a method for manufacturing a hafnium oxide film layer, the manufacturing method comprising: first providing a substrate, then introducing a hafnium source and a first oxygen source into one side of the substrate to form a first hafnium oxide layer, and then introducing a hafnium source and oxygen into the side of the first hafnium oxide layer away from the substrate to form a second hafnium oxide layer, thereby finally forming a hafnium oxide film layer including the first hafnium oxide layer and the second hafnium oxide layer. In the present embodiment, oxygen is added during the manufacturing of the hafnium oxide film layer, so that the step coverage of the manufactured hafnium oxide film layer is high, the film layer continuity is good, the film layer thickness is uniform, and the refractive index of the manufactured hafnium oxide film layer is close to the actual refractive index of hafnium oxide, and the purity of hafnium oxide in the hafnium oxide film layer is high. In summary, the manufacturing method of the hafnium oxide film layer provided in the present embodiment can improve the film quality of the hafnium oxide film layer.

[0068] Optionally, the first oxygen source includes at least one of ozone and water vapor; and the hafnium source includes dimethylamine.

[0069] Specifically, firstly setting ozone and / or water vapor to react with dimethylamine groups can facilitate the reaction of oxygen with dimethylamine groups to form a second hafnium oxide layer, thereby ultimately facilitating improving the film quality of the hafnium oxide film layer.

[0070] Optionally, introducing a hafnium source and a first oxygen source into one side of the substrate to form the first hafnium oxide layer specifically includes: alternately introducing a hafnium source and a first oxygen source a first set number of times into one side of the substrate to form the first hafnium oxide layer.

[0071] Specifically, alternately introducing the hafnium source and the first oxygen source is conducive to the formation of the first hafnium oxide layer, and the first set number of times can be 5 or 10, and the range of the first set number of times can be 5 to 20. The number of times the hafnium source and the first oxygen source are introduced is the first set number of times, and the hafnium source and the first oxygen source are introduced alternately. Exemplarily, when the first set number of times is 5, the steps of forming the first hafnium oxide layer can be: introducing the hafnium source once, introducing the first oxygen source once, introducing the hafnium source once, introducing the first oxygen source once, introducing the hafnium source once, introducing the first oxygen source once, introducing the hafnium source once, introducing the first oxygen source once, introducing the hafnium source once, introducing the first oxygen source once, introducing the hafnium source once, introducing the first oxygen source once, introducing the hafnium source once, introducing the first oxygen source once, introducing the hafnium source once, introducing the first oxygen source once, introducing the hafnium source once, introducing the first oxygen source once, introducing the hafnium source once, and introducing the first oxygen source once.

[0072] Optionally, alternately introducing a hafnium source and a first oxygen source for a first set number of times to form the first hafnium oxide layer specifically includes the following steps:

[0073] S121. Open the first purge valve and introduce purge gas.

[0074] Specifically, after the first purge valve is opened, the purge gas enters the atomic layer deposition chamber through the first purge valve. The purge gas may be nitrogen.

[0075] S122, when the purge gas of the first set time is introduced, the hafnium source valve is opened and the hafnium source is introduced.

[0076] Specifically, the first set time length may be 0.1s, and the range of the first set time length may be 0.1s to 1.5s. After the hafnium source valve is opened, the hafnium source enters the atomic layer deposition chamber through the hafnium source valve. The hafnium source is introduced when the purge gas of the first set time length is introduced, and the purge gas is still introduced while the hafnium source is introduced. The purge gas can push the hafnium source to quickly enter the atomic layer deposition chamber.

[0077] S123, when the hafnium source is introduced for a second set time, closing the hafnium source valve.

[0078] Specifically, the second set time length may be 0.9s, and the range of the second set time length may be 0.3s to 1.7s. Exemplarily, when the hafnium source is introduced for 0.9s, the hafnium source valve is closed. After the hafnium source valve is closed, the hafnium source cannot pass through the hafnium source valve into the atomic layer deposition chamber, and the purge gas still passes through the first purge valve into the atomic layer deposition chamber.

[0079] S124, when the hafnium source valve is closed for a third set time, closing the first purge valve.

[0080] Specifically, the third set time may be 9s, and the range of the third set time may be 7s to 15s. The first purge valve is closed later than the hafnium source valve, so that the purge gas passing through the first purge valve can push the hafnium source in the pipeline into the atomic layer deposition chamber.

[0081] S125, when the first purge valve is closed for a fourth set time, the second purge valve is opened to allow the purge gas to pass through.

[0082] Specifically, the fourth set time length may be 3s, and the range of the fourth set time length may be 2s to 7s. After the first purge valve is closed, waiting for the fourth set time length before introducing the purge gas may facilitate the hafnium source in the pipeline to fully enter the atomic layer deposition chamber. The purge gas here enters the atomic layer deposition chamber through the second purge valve.

[0083] S126. When the second purge valve is opened for a fifth set time, the first oxygen source valve is opened and the first oxygen source is introduced.

[0084] Specifically, the fifth set time length can be 0.1s, and the range of the fifth set time length can be 0.1s to 1.5s. After the first oxygen source valve is opened, the first oxygen source enters the atomic layer deposition chamber through the first oxygen source valve. When the purge gas of the fifth set time length is introduced, the first oxygen source is introduced, and the purge gas is still introduced while the first oxygen source is introduced. The purge gas can push the first oxygen source to quickly enter the atomic layer deposition chamber.

[0085] S127. When the first oxygen source is introduced for the sixth set time, the first oxygen source valve is closed.

[0086] Specifically, the sixth set time length may be 3s, and the range of the sixth set time length may be 2s to 7s. Exemplarily, when the first oxygen source is passed through for 3s, the first oxygen source valve is closed. After the first oxygen source valve is closed, the first oxygen source is no longer passed through, and the purge gas still enters the atomic layer deposition chamber through the second purge valve.

[0087] S128. When the first oxygen source valve is closed for the seventh set time, close the second purge valve.

[0088] Specifically, the seventh set time length may be 2s, and the range of the seventh set time length may be 0.5s to 6s. The second purge valve is closed later than the first oxygen source valve, so that the purge gas passing through the second purge valve can push the first oxygen source in the pipeline into the atomic layer deposition chamber.

[0089] S129: When the second purge valve is closed for an eighth set time, determine whether the number of times the hafnium source is introduced is less than the first set number of times.

[0090] If not, a first hafnium oxide layer is formed; if so, the process returns to step S121.

[0091] Specifically, the eighth set time length can be 8s, and the range of the eighth set time length can be 5s to 14s. During the eighth set time length when the second purge valve is closed, the first oxygen source in the pipeline can fully enter the atomic layer deposition chamber, so that the first oxygen source and the hafnium source can fully react to form a first hafnium oxide layer with good film quality. When the number of times the hafnium source is introduced does not reach the first set number of times, the hafnium source and the first oxygen source continue to be alternately input. When the number of times the hafnium source is introduced is not less than the first set number of times, it indicates that the first hafnium oxide layer has been formed.

[0092] It should be noted that the number of times the hafnium source is input between the opening of the hafnium source valve and the closing of the hafnium source valve is one. The number of times the first oxygen source is input between the opening of the first oxygen source valve and the closing of the first oxygen source valve is one.

[0093] Optionally, introducing a hafnium source and a second oxygen source into a side of the first hafnium oxide layer away from the substrate to form the second hafnium oxide layer specifically includes: alternately introducing a second set number of hafnium sources and a second oxygen source into a side of the first hafnium oxide layer away from the substrate to form the second hafnium oxide layer.

[0094] Specifically, alternately introducing the hafnium source and the second oxygen source is conducive to the formation of the second hafnium oxide layer, the second set number of times may be 495, and the sum of the first set number of times and the second set number of times may be 500. The number of times the hafnium source and the second oxygen source are introduced is the second set number of times, and the hafnium source and the second oxygen source are introduced alternately.

[0095] Optionally, alternately introducing the hafnium source and the second oxygen source for a second set number of times to form the second hafnium oxide layer specifically includes the following steps:

[0096] S131, open the first purge valve and introduce purge gas.

[0097] Specifically, the content of step S131 is the same as that of step S121. For the description of step S131, please refer to the description of step S121, which will not be repeated here.

[0098] S132, when the purge gas of the first set time is introduced, the hafnium source valve is opened and the hafnium source is introduced.

[0099] Specifically, the content of step S132 is the same as that of step S122. For the description of step S132, please refer to the description of step S122, which will not be repeated here.

[0100] S133, when the hafnium source is introduced for a second set time, closing the hafnium source valve.

[0101] Specifically, the content of step S133 is the same as that of step S123. For the description of step S133, please refer to the description of step S123, which will not be repeated here.

[0102] S134, when the hafnium source valve is closed for the third set time, closing the first purge valve.

[0103] Specifically, the content of step S134 is the same as that of step S124. For the description of step S134, please refer to the description of step S124, which will not be repeated here.

[0104] S135, when the first purge valve is closed for a fourth set time, the third purge valve is opened to allow the purge gas to pass through.

[0105] Specifically, the purge gas here enters the atomic layer deposition chamber through the third purge valve. The third purge valve can be the same valve as the second purge valve, or the third purge valve can be different from the second purge valve.

[0106] S136. When the third purge valve is opened for the ninth set time, the second oxygen source valve is opened and the second oxygen source is introduced.

[0107] Specifically, the ninth set time length can be 0.1s, and the range of the ninth set time length can be 0.1s to 1.5s. After the second oxygen source valve is opened, the second oxygen source enters the atomic layer deposition chamber through the second oxygen source valve. When the purge gas of the ninth set time length is introduced, the second oxygen source is introduced, and the purge gas is still introduced while the second oxygen source is introduced. The purge gas can push the second oxygen source to quickly enter the atomic layer deposition chamber.

[0108] S137. When the second oxygen source is introduced for the tenth set time, the second oxygen source valve is closed.

[0109] Specifically, the tenth set time length can be 0.3s. The tenth set time length can range from 0.1s to 1s. Exemplarily, when the second oxygen source is introduced for 0.3s, the second oxygen source valve is closed. After the second oxygen source valve is closed, the second oxygen source is no longer introduced, and the purge gas still enters the atomic layer deposition chamber through the third purge valve.

[0110] S138. When the second oxygen source valve is closed for the eleventh set time, close the third purge valve.

[0111] Specifically, the eleventh set time length may be 2s, and the range of the eleventh set time length may be 0.5s to 6s. The third purge valve is closed later than the second oxygen source valve, so that the purge gas passing through the third purge valve can push the second oxygen source in the pipeline into the atomic layer deposition chamber.

[0112] S139: When the third purge valve is closed for a twelfth set time, determine whether the number of times the hafnium source is introduced is less than a second set number of times.

[0113] If not, a first hafnium oxide layer is formed; if so, the process returns to step S131 .

[0114] Specifically, the twelfth set time length can be 8s, and the range of the twelfth set time length can be 5s to 14s. During the twelfth set time length when the third purge valve is closed, the second oxygen source in the pipeline can fully enter the atomic layer deposition chamber, so that the second oxygen source and the hafnium source can fully react to form a second hafnium oxide layer with good film quality. When the number of times the hafnium source is introduced does not reach the second set number, the hafnium source and the second oxygen source continue to be alternately input. When the number of times the hafnium source is introduced is not less than the second set number, it indicates that the second hafnium oxide layer has been formed.

[0115] It should be noted that the number of times the second oxygen source is input between the opening of the second oxygen source valve and the closing of the second oxygen source valve is once.

[0116] Optionally, the range of the first set time length is 0.1s to 1.5s; the range of the second set time length is 0.3s to 1.7s; the range of the third set time length is 7s to 15s; the range of the fourth set time length is 2s to 7s; the range of the ninth set time length is 0.1s to 1.5; the range of the tenth set time length is 0.1s to 1s; the range of the eleventh set time length is 0.5s to 6s; the range of the twelfth set time length is 5s to 14s. This setting can further improve the film quality of the manufactured hafnium oxide film layer.

[0117] Optionally, the second set number of times is greater than the first set number of times. This setting can make the film quality of the manufactured hafnium oxide film better.

[0118] This embodiment further provides a semiconductor device, which includes a hafnium oxide film layer; the hafnium oxide film layer is manufactured by the method for manufacturing the hafnium oxide film layer provided by any embodiment of the present invention.

[0119] Specifically, the hafnium oxide film layer provided in this embodiment has excellent quality and can improve the quality of semiconductor devices.

[0120] Figure 6 is a schematic diagram of a structure of a hafnium oxide film manufacturing device provided according to an embodiment of the present invention, referring to Figure 6 The manufacturing device of the hafnium oxide film provided in this embodiment includes a substrate providing module 210, a first hafnium oxide layer forming module 220 and a second hafnium oxide layer forming module 230; the substrate providing module 210 is used to provide a substrate; the first hafnium oxide layer forming module 220 is used to introduce a hafnium source and a first oxygen source into one side of the substrate to form a first hafnium oxide layer; the second hafnium oxide layer forming module 230 is used to introduce a hafnium source and a second oxygen source into a side of the first hafnium oxide layer away from the substrate to form a second hafnium oxide layer, wherein the hafnium oxide film includes a first hafnium oxide layer and a second hafnium oxide layer, and the second oxygen source includes oxygen.

[0121] The hafnium oxide film manufacturing device provided in this embodiment has corresponding beneficial effects as the hafnium oxide film manufacturing method provided in any embodiment of the present invention. For technical details not detailed in this embodiment, please refer to the hafnium oxide film manufacturing method provided in any embodiment of the present invention.

[0122] It should be understood that the various forms of processes shown above can be used to reorder, add or delete steps. For example, the steps described in the present invention can be executed in parallel, sequentially or in different orders, as long as the desired results of the technical solution of the present invention can be achieved, and this document does not limit this.

[0123] The above specific implementations do not constitute a limitation on the protection scope of the present invention. It should be understood by those skilled in the art that various modifications, combinations, sub-combinations and substitutions can be made according to design requirements and other factors. Any modification, equivalent substitution and improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for manufacturing a hafnium oxide film, characterized in that: include: providing a substrate; introducing a hafnium source and a first oxygen source into one side of the substrate to form a first hafnium oxide layer; The hafnium source and the second oxygen source are introduced into a side of the first hafnium oxide layer away from the substrate to form a second hafnium oxide layer, wherein the hafnium oxide film layer includes the first hafnium oxide layer and the second hafnium oxide layer, and the second oxygen source includes oxygen.

2. The method for manufacturing a hafnium oxide film according to claim 1, characterized in that: The first oxygen source includes at least one of ozone and water vapor; and the hafnium source includes dimethylamine.

3. The method for manufacturing a hafnium oxide film according to claim 1, characterized in that: The step of introducing a hafnium source and a first oxygen source into one side of the substrate to form a first hafnium oxide layer specifically includes: The hafnium source and the first oxygen source are alternately introduced into one side of the substrate for a first set number of times to form the first hafnium oxide layer.

4. The method for manufacturing a hafnium oxide film according to claim 3, characterized in that: The step of alternately introducing the hafnium source and the first oxygen source for a first set number of times to form the first hafnium oxide layer specifically includes: Open the first purge valve and introduce purge gas; When the purge gas of the first set time is introduced, the hafnium source valve is opened and the hafnium source is introduced; When the hafnium source is introduced for a second set time, closing the hafnium source valve; When the hafnium source valve is closed for a third set time, closing the first purge valve; When the first purge valve is closed for a fourth set time, the second purge valve is opened to allow purge gas to pass; When the second purge valve is opened for a fifth set time, the first oxygen source valve is opened to introduce the first oxygen source; When the first oxygen source is introduced for a sixth set time, closing the first oxygen source valve; When the first oxygen source valve is closed for a seventh set time, closing the second purge valve; When the second purge valve is closed for an eighth set time, determining whether the number of times the hafnium source is introduced is less than the first set number of times; If yes, the process returns to the step of opening the first purge valve and introducing the purge gas; if no, it indicates that the first hafnium oxide film layer is formed.

5. The method for manufacturing a hafnium oxide film according to claim 3, characterized in that: The step of introducing the hafnium source and the second oxygen source into a side of the first hafnium oxide layer away from the substrate to form the second hafnium oxide layer specifically includes: The second hafnium oxide layer is formed by alternately introducing the hafnium source and the second oxygen source for a second set number of times toward a side of the first hafnium oxide layer away from the substrate.

6. The method for manufacturing a hafnium oxide film according to claim 5, characterized in that: The step of alternately introducing the hafnium source and the second oxygen source a second set number of times to form the second hafnium oxide layer specifically includes: Open the first purge valve and introduce purge gas; When the purge gas of the first set time is introduced, the hafnium source valve is opened and the hafnium source is introduced; When the hafnium source is introduced for a second set time, closing the hafnium source valve; When the hafnium source valve is closed for a third set time, closing the first purge valve; When the first purge valve is closed for a fourth set time, the third purge valve is opened to allow the purge gas to pass; When the third purge valve is opened for a ninth set time, the second oxygen source valve is opened and the second oxygen source is introduced; When the second oxygen source is introduced for a tenth set time, closing the second oxygen source valve; When the second oxygen source valve is closed for an eleventh set time, closing the third purge valve; When the third purge valve is closed for a twelfth set time, determining whether the number of times the hafnium source is introduced is less than a second set number of times; If yes, the process returns to the step of opening the first purge valve and introducing the purge gas; if no, it indicates that the second hafnium oxide film layer is formed.

7. The method for manufacturing a hafnium oxide film according to claim 6, characterized in that: The first set time length ranges from 0.1s to 1.5s; the second set time length ranges from 0.3s to 1.7s; the third set time length ranges from 7s to 15s; the fourth set time length ranges from 2s to 7s; the ninth set time length ranges from 0.1s to 1.5; the tenth set time length ranges from 0.1s to 1s; the eleventh set time length ranges from 0.5s to 6s; the twelfth set time length ranges from 5s to 14s.

8. The method for manufacturing a hafnium oxide film according to claim 5, characterized in that: The second set number of times is greater than the first set number of times.

9. A semiconductor device, characterized in that: including a hafnium oxide film layer; The hafnium oxide film layer is manufactured by the method for manufacturing a hafnium oxide film layer according to any one of claims 1 to 8.

10. A device for manufacturing a hafnium oxide film, characterized in that: It includes a substrate providing module, a first hafnium oxide layer forming module and a second hafnium oxide layer forming module; The substrate providing module is used to provide a substrate; The first hafnium oxide layer forming module is used to introduce a hafnium source and a first oxygen source into one side of the substrate to form a first hafnium oxide layer; The second hafnium oxide layer forming module is used to introduce the hafnium source and the second oxygen source into the side of the first hafnium oxide layer away from the substrate to form a second hafnium oxide layer, wherein the hafnium oxide film layer includes the first hafnium oxide layer and the second hafnium oxide layer, and the second oxygen source includes oxygen.