Preparation method and application of 1D carbon-loaded phosphorus-doped sulfide nanotube catalyst applied to electrolyzed water
The 1D carbon-loaded phosphorus-doped sulfide nanotube catalyst prepared by coaxial electrospinning technology solves the problem of low efficiency of electrocatalysts in existing electrolytic water technology, and achieves low overpotential and efficient electrolytic water decomposition of hydrogen, promoting the development of hydrogen by promoting The development of clean energy.
Patent Information
- Application Number
- CN202411147852.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-08
AI Technical Summary
The existing electrolytic hydrogen production technology requires efficient electrocatalysts to reduce overpotentials and improve energy conversion efficiency. The morphology and structure of traditional catalysts have a great impact on the reaction process, making it difficult to achieve ideal zero carbon emissions.
Coaxial electrospinning technology was used to prepare 1D carbon-loaded phosphorus-doped sulfide nanotube catalyst with high specific surface area. MoS2/CoS2 nanosheets were grown in situ on the surface of hollow carbon nanofibers by hydrothermal method, and optimized by phosphorus doping strategy The catalyst active site forms a three-dimensional electrocatalytic conductive network.
Under alkaline conditions, the catalyst exhibits low overpotential (85mV) and low Tafel slope (68.6mV dec-1), which significantly improves the electrocatalytic activity and stability of electrolytic water and achieves more efficient water decomposition of hydrogen.
Smart Images

Figure CN118910665A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of electrocatalysis, and relates to a preparation method and application of a 1D carbon-supported phosphorus-doped sulfide nanotube catalyst for water electrolysis. The coaxial electrospinning technology is used to prepare a 1D carbon-supported phosphorus-doped sulfide nanotube catalyst with a high specific surface area for water electrolysis. Background Art
[0002] my country is a major energy consumer and carbon emitter. According to the International Energy Agency (IEA) statistical report, the total global carbon dioxide emissions in 2023 will be 37.4 billion tons, and the carbon dioxide generated by my country's energy industry will reach 12.6 billion tons. In order to actively respond to the challenges of global climate change, my country proposed at the United Nations General Assembly the goal of achieving carbon peak by 2030 and carbon neutrality by 2060. In order to achieve this goal, it is urgent to seek ideal clean energy. Due to its high energy density and cleanliness, hydrogen is considered to be the most ideal form of energy.
[0003] There are currently various ways to produce hydrogen, of which more than 96% are produced from fossil fuels. However, this process produces a large amount of carbon dioxide. Therefore, the hydrogen produced by this method is called "black hydrogen". The biggest advantage of renewable energy electrolysis of water to produce hydrogen is that it can achieve zero carbon emissions in the hydrogen production process, and the hydrogen produced is green hydrogen. However, water electrolysis technology consists of two half reactions: the hydrogen evolution reaction at the cathode and the oxygen evolution reaction at the anode. In the actual process of water electrolysis, an additional voltage is usually applied to speed up the reaction rate. The working voltage of water decomposition can be described as: the applied voltage is equal to the theoretical decomposition voltage + the overpotential of the solution impedance + the overpotential required to overcome the inherent activation barrier of the anode and cathode. Based on this, efficient electrocatalysts are required to reduce the overpotential and improve the energy conversion efficiency of the system.
[0004] Among many transition metal-based materials, transition metal sulfides have excellent electrocatalytic activity as electrodes. Many researchers have synthesized them into heterogeneous composite catalysts through different synthesis methods, or doped P, V, B and other atoms to rearrange the charge, so as to achieve the purpose of regulating the material morphology and structure, improving the material conductivity and metallic properties, and realizing the application of transition metal sulfide catalysts in the electrolysis of water to produce hydrogen.
[0005] Looking back at the research and development history of transition metal sulfide electrocatalytic materials, catalysts with different morphologies have a lot of influence on the mass transfer of the reaction process and a great influence on the activity. One-dimensional nanowires, especially nanotube structures, are a unique structure with nanometer-scale diameters and have been a research interest since the early 1990s. Its structure has the characteristics of large aspect ratio, porous characteristics, large specific surface area, and high degree of graphitization, which meet the requirements of an ideal catalyst. Compared with the preparation method of traditional one-dimensional hollow carbon nanofibers, hollow carbon nanofibers prepared by coaxial electrospinning can provide abundant active sites in the radial direction, achieve rapid electron transfer in the axial direction, and interweave to form a three-dimensional electrocatalytic conductive network, thereby effectively reducing the contact resistance and improving the electrolytic water activity.
[0006] The present invention proposes to take coaxial electrospun nanofiber composite materials as the main research object, design and synthesize a series of 1D carbon-supported phosphorus-doped sulfide nanotubes for water electrolysis, and the prepared catalysts show excellent electrocatalytic activity. Summary of the invention
[0007] The present invention proposes a 1D carbon-supported phosphorus-doped sulfide nanotube catalyst with a high specific surface area prepared by a coaxial electrospinning method. The catalyst prepared by this method provides abundant active sites, and the three-dimensional electrocatalytic conductive network formed by the interweaving of nanotubes realizes the rapid transmission of electrons. The electrochemical activity of water electrolysis was tested under alkaline conditions. At 10 mA cm -2 The overpotential is only 85mV and the Tafel slope is as low as 68.6mV dec -1 The prepared catalyst exhibits excellent electrocatalytic activity. In addition, the present invention can directly prepare spinning membranes, and preparing electrodes by in-situ growth is beneficial to subsequent experimental amplification.
[0008] In order to achieve the above object, the technical solution adopted by the present invention is:
[0009] A preparation method for a 1D carbon-supported phosphorus-doped sulfide nanotube catalyst for water electrolysis, wherein the preparation method firstly prepares hollow carbon nanofibers by coaxial electrospinning; secondly, in-situ grows MoS2 / CoS2 on the surface of the hollow carbon nanofibers by a hydrothermal method; and finally, improves the intrinsic activity of the catalyst active sites by a phosphorus doping strategy to obtain a 1D carbon-supported phosphorus-doped sulfide nanotube catalyst. The specific steps are:
[0010] Step (1) preparing shell layer solution and core layer solution:
[0011] Add polyacrylonitrile PAN into N,N-dimethylformamide DMF and stir until completely dissolved to obtain a shell layer solution, wherein the mass concentration of PAN in the shell layer solution is 9-10%.
[0012] Add polymethyl methacrylate (PMMA) into DMF and stir until it is completely dissolved to obtain a core layer solution. The mass concentration of PMMA in the core layer solution is 9.5-10.5%.
[0013] Step (2) preparing hollow carbon nanofibers by coaxial electrospinning:
[0014] The shell layer solution and the core layer solution obtained in step (1) are respectively injected into the two solution channels of the coaxial electrospinning, and the coaxial electrospinning parameters are adjusted to perform electrospinning to obtain a PAN / PMMA film; in this step, the spinning system is composed of two coaxial tubes with different inner diameters. Under the action of a high-voltage electric field, the shell layer liquid flows out and merges with the core layer liquid. The shell layer liquid is stretched at high frequency, and a strong shear stress is generated at the interface of the inner and outer layer solutions during high-speed spraying. Under the action of the shear stress, the core layer solution moves coaxially along the shell layer, bends and deforms electrically, and solidifies into a coaxial composite nanofiber.
[0015] The PAN / PMMA film is then pre-oxidized in a muffle furnace and carbonized in a tube furnace to obtain hollow carbon nanofibers. In this step, the core layer PMMA is pyrolyzed and removed, and the PAN in the shell layer is converted into carbon, eventually forming HCNFs.
[0016] Furthermore, in step (2), the pre-oxidation temperature is 230-270° C., and the time is 1-2 h; the carbonization temperature is 750-850° C., and the time is 1-2 h.
[0017] Furthermore, in step (2), when two relatively independent nozzles are used for spinning simultaneously, the pushing speeds of the outer layer solution (shell layer solution) and the inner layer solution (core layer solution) are controlled at 0.08-0.09 mm / min and 0.03-0.05 mm / min, respectively. The distance between the nozzle and the receiver is fixed at 14-16 cm, and the applied high voltage is 14-16 KV.
[0018] Step (3) Preparation of MoS2 / CoS2@HCNFs:
[0019] First, the hollow carbon nanofibers obtained in step (2) are activated with concentrated nitric acid. In this step, after the HCNFs are treated with concentrated nitric acid, organic matter on the surface is removed and more nucleation sites are generated.
[0020] Then, the HCNFs were immersed in a homogeneous aqueous solution containing ammonium molybdate tetrahydrate, cobalt nitrate hexahydrate and thiourea for hydrothermal treatment to obtain MoS2 / CoS2@HCNFs. In this step, vertically aligned MoS2 / CoS2 nanosheets were in situ grown on the surface of HCNFs activated by concentrated nitric acid.
[0021] Furthermore, in the step (3), the nitric acid activation treatment is specifically as follows: HCNFs are ultrasonicated in a concentrated nitric acid solution for 1 to 2 hours, and then washed and dried for later use.
[0022] Furthermore, in the step (3), the molar ratio of ammonium molybdate tetrahydrate, cobalt nitrate hexahydrate and thiourea is 1:1:33 to 1:3:33.
[0023] Furthermore, in the step (3), the temperature of the hydrothermal treatment is 160 to 220° C., and the time is 18 to 24 hours.
[0024] Step (4) Take 0.1g MoS2 / CoS2@HCNFs and 1g sodium hypophosphite from step (3) and place them in the center and upstream of the tube furnace respectively. Inert gas is introduced to exclude air, and then inert gas is continued to be introduced. 1D carbon-supported phosphorus-doped sulfide nanotubes P-MoS2 / CoS2@HCNFs are obtained by high-temperature phosphating under the protection of inert gas. In this step, a gas-solid phase phosphating method mediated by sodium hypophosphite is used. Using sodium hypophosphite as a phosphorus source, MoS2 / CoS2@HCNFs are phosphated in an inert gas atmosphere, and the catalyst P-MoS2 / CoS2@HCNFs is obtained after cooling.
[0025] Furthermore, in the step (4), when the tubular furnace is used, the inert gas is nitrogen, the phosphating temperature is 300-400° C., and the time is 1-2 hours.
[0026] A 1D carbon-supported phosphorus-doped sulfide nanotube catalyst used for water electrolysis is obtained by adopting the above preparation method.
[0027] An application of a 1D carbon-supported phosphorus-doped sulfide nanotube catalyst for water electrolysis. When used, the electrochemical activity of the catalyst for water electrolysis is tested under alkaline conditions, 10 mA cm -2 The overpotential is only 85mV and the Tafel slope is as low as 68.6mVdec -1 , showing excellent catalytic performance in water electrolysis.
[0028] Beneficial effects of the present invention:
[0029] (1) The present invention provides a method for preparing 1D carbon-supported phosphorus-doped sulfide nanotube catalysts by coaxial electrospinning. The nanotubes obtained by electrospinning have significant internal channels and low mass transfer resistance.
[0030] (2) Using the catalyst prepared by this method, the vertically aligned MoS2 / CoS2 nanosheets can fully expose the edge sites to present an overall increased catalyst loading, thus bringing about significant HER performance.
[0031] (3) Phosphorus-doped sulfides can effectively optimize the electronic structure, accelerate the dissociation of water, and simultaneously regulate H* adsorption and H2 desorption during HER catalysis, further promoting the kinetics of water electrolysis.
[0032] (4) The catalyst prepared by this method can be used to directly prepare spinning membranes, and the preparation of electrodes through in situ growth is beneficial to subsequent experimental scale-up. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 a is a scanning electron microscope image of the product of Example 1; Figure 1 b is a scanning electron microscope image of the product of Example 2; Figure 1 c is a scanning electron microscope image of the product of Example 3; Figure 1 d is a scanning electron microscope image of the carbon nanowires in Comparative Example 2;
[0034] Figure 1 e is the scanning electron microscope image of the product of Comparative Example 2; Figure 1 f is the SEM image of the product P-MoS2 / CoS2-2@CNFs prepared in comparative example 1;
[0035] Figure 2 The XRD spectra of the products prepared in Comparative Example 1 and Example 2 are shown below;
[0036] Figure 3 a is the LSV graph of the prepared product of Example 1, the prepared product of Example 2, the prepared product of Example 3, the prepared product of Comparative Example 1, the prepared product of Comparative Example 2, and Pt / C in 1M KOH solution;
[0037] Figure 3 b is the Tafel diagram of the prepared product of Example 2, the prepared product of Comparative Example 1, the prepared product of Comparative Example 2, and Pt / C in 1M KOH solution; Figure 3 c is the C of the product prepared in Example 2, the product prepared in Comparative Example 1, and the product prepared in Comparative Example 2 measured in 1M KOH solution. dl picture; Figure 3 d is the IT diagram of the product prepared in Example 2. Specific implementation methods
[0039] The present invention is further described below in conjunction with specific embodiments.
[0040] The present invention utilizes coaxial electrospinning technology to prepare a 1D carbon-supported phosphorus-doped sulfide nanotube catalyst with a high specific surface area for water electrolysis. In order to further understand the present invention, the electrocatalyst and its application provided by the present invention are specifically described below in conjunction with the embodiments, but the present invention is not limited to these embodiments. Non-essential improvements and adjustments made by technicians in this field under the core guiding idea of the present invention still belong to the protection scope of the present invention. The specific implementation method is as follows:
[0041] Example 1
[0042] (1) Add PAN and PMMA to DMF and stir until completely dissolved to obtain shell and core layer solutions. The mass concentration of the shell layer solution is 9.5%, and the mass concentration of the core layer solution is 10%;
[0043] (2) The obtained shell and core layer solutions were respectively injected into the two solution channels of the coaxial electrospinning, and the coaxial electrospinning parameters were adjusted for electrospinning to obtain a PAN / PMMA film; after pre-oxidation at 250°C in a muffle furnace and carbonization at 800°C in a tubular furnace, hollow carbon nanofibers were obtained. When two relatively independent nozzles were used for simultaneous spinning, the pushing speeds of the outer layer solution and the inner layer solution were controlled at 0.085 mm / min and 0.04 mm / min, respectively. The distance between the nozzle and the receiver was fixed at 15 cm, and the applied high voltage was 15 KV.
[0044] (3) The obtained hollow carbon nanofibers were activated by concentrated nitric acid and then immersed in a homogeneous aqueous solution containing ammonium molybdate tetrahydrate, cobalt nitrate hexahydrate and thiourea. The molar ratio of ammonium molybdate tetrahydrate, cobalt nitrate hexahydrate and thiourea was 1:1:33. The hydrothermal condition was maintained at 220°C for 18 hours. MoS2 / CoS2-1@HCNFs were obtained by the hydrothermal method.
[0045] (4) 0.1 g of MoS2 / CoS2-1@HCNFs and 1 g of sodium hypophosphite obtained in step (3) were placed in the center and upstream of the tube furnace, respectively, and N2 was introduced to remove the air, and then N2 was continued to be introduced, and 1D carbon-supported phosphorus-doped sulfide nanotube P-MoS2 / CoS2-1@HCNFs catalyst was obtained by high-temperature phosphating under N2 protection. The phosphating temperature was 350°C and the time was 2 h.
[0046] Figure 1 a is the SEM image of the product P-MoS2 / CoS2-1@HCNFs prepared in Example 1, from which it can be seen that the P-MoS2 / CoS2 nanosheets grow vertically on the surface of the hollow carbon nanofibers. Figure 3 The HER activity test showed that the product P-MoS2 / CoS2-1@HCNFs obtained in Example 1 had a HER activity of 10 mA cm -2 The overpotential at is 98mV.
[0047] Example 2
[0048] (1) Add PAN and PMMA to DMF and stir until completely dissolved to obtain shell and core layer solutions. The mass concentration of the shell layer solution is 9.5%, and the mass concentration of the core layer solution is 10%;
[0049] (2) The obtained shell and core layer solutions were respectively injected into the two solution channels of the coaxial electrospinning, and the coaxial electrospinning parameters were adjusted for electrospinning to obtain PAN / PMMA membranes; after pre-oxidation at 250°C in a muffle furnace and carbonization at 800°C in a tubular furnace, hollow carbon nanotubes were obtained. When two relatively independent nozzles were used for simultaneous spinning, the pushing speeds of the outer layer solution and the inner layer solution were controlled at 0.085 mm / min and 0.04 mm / min, respectively. The distance between the nozzle and the receiver was fixed at 15 cm, and the applied high voltage was 15 KV.
[0050] (3) The obtained hollow carbon nanofibers were activated by concentrated nitric acid and then immersed in a homogeneous aqueous solution containing ammonium molybdate tetrahydrate, cobalt nitrate hexahydrate and thiourea. The molar ratio of ammonium molybdate tetrahydrate, cobalt nitrate hexahydrate and thiourea was 1:2:33. The hydrothermal condition was maintained at 220°C for 18 hours. MoS2 / CoS2-2@HCNFs were obtained by the hydrothermal method.
[0051] (4) 0.1 g of MoS2 / CoS2-2@HCNFs and 1 g of sodium hypophosphite obtained in step (3) were placed in the center and upstream of the tube furnace, respectively, and N2 was introduced to remove the air, and then N2 was continued to be introduced, and 1D carbon-supported phosphorus-doped sulfide nanotube P-MoS2 / CoS2-2@HCNFs catalyst was obtained by high-temperature phosphating under N2 protection. The phosphating temperature was 350°C and the time was 2 h.
[0052] Figure 1 b is the SEM image of the product P-MoS2 / CoS2-2@HCNFs obtained in Example 2, which also shows a good morphology. Figure 2 The XRD pattern of the product prepared in Example 2 is shown. The characteristic peaks of P-MoS2 / CoS2-2@HCNFs and MoS2 / CoS2-2@HCNFs are basically the same, indicating that phosphorus doping does not change the crystal structure. Figure 3 The HER activity test showed that the product P-MoS2 / CoS2@HCNFs obtained in Example 2 had an activity of 10 mA cm -2 The overpotential at is only 85 mV. The product prepared in Example 2 has better electrochemical performance. The stability test was carried out using the chronoamperometry method. Figure 3As shown in Figure d, the electrocatalytic activity remained stable during the 36 h test, confirming that the product P-MoS2 / CoS2-2@HCNFs obtained in Example 2 has good stability.
[0053] Example 3
[0054] (1) Add PAN and PMMA to DMF and stir until completely dissolved to obtain shell and core layer solutions. The mass concentration of the shell layer solution is 9.5%, and the mass concentration of the core layer solution is 10%;
[0055] (2) The obtained shell and core layer solutions were respectively injected into the two solution channels of the coaxial electrospinning, and the coaxial electrospinning parameters were adjusted for electrospinning to obtain a PAN / PMMA film; after pre-oxidation at 250°C in a muffle furnace and carbonization at 800°C in a tubular furnace, hollow carbon nanofibers were obtained. When two relatively independent nozzles were used for simultaneous spinning, the pushing speeds of the outer layer solution and the inner layer solution were controlled at 0.085 mm / min and 0.04 mm / min, respectively. The distance between the nozzle and the receiver was fixed at 15 cm, and the applied high voltage was 15 KV.
[0056] (3) The obtained hollow carbon nanofibers were activated by concentrated nitric acid and then immersed in a homogeneous aqueous solution containing ammonium molybdate tetrahydrate, cobalt nitrate hexahydrate and thiourea. The molar ratio of ammonium molybdate tetrahydrate, cobalt nitrate hexahydrate and thiourea was 1:3:33. The hydrothermal condition was maintained at 220°C for 18 hours. MoS2 / CoS2-3@HCNFs were obtained by the hydrothermal method.
[0057] (4) 0.1 g of MoS2 / CoS2-3@HCNFs and 1 g of sodium hypophosphite obtained in step (3) were placed in the center and upstream of the tube furnace, respectively, and N2 was introduced to remove the air, and then N2 was continued to be introduced, and 1D carbon-supported phosphorus-doped sulfide nanotube P-MoS2 / CoS2-3@HCNFs catalyst was obtained by high-temperature phosphating under N2 protection. The phosphating temperature was 350°C and the time was 2 h.
[0058] Figure 1 c is the SEM image of the product P-MoS2 / CoS2-3@HCNFs prepared in Example 3, and similarly, P-MoS2 / CoS2 nanosheets grow vertically on the surface of hollow carbon nanofibers. Figure 3 The HER activity test showed that the product P-MoS2 / CoS2-3@HCNFs obtained in Example 3 had an activity of 10 mA cm -2 The overpotential at is 103mV, which has better electrochemical performance.
[0059] Comparative Example 1
[0060] Without adding phosphating treatment, other conditions were the same as in Example 2 to prepare MoS2 / CoS2-2@HCNFs catalyst.
[0061] Figure 1 d is the SEM image of the product MoS2 / CoS2-2@HCNFs prepared in Example 1. After the in-situ growth of MoS2 / CoS2, it can be seen that the nanosheets grow vertically on the surface of the hollow carbon nanofibers. Figure 3 The HER activity test showed that the product MoS2 / CoS2@HCNFs (112mV@10mA cm -2 ), the product P-MoS2 / CoS2@HCNFs obtained in Example 2 was -2 The overpotential is lower (85mV@10mA cm -2 ), Tafel slope is 68.6mV dec -1 This indicates that the electrochemical performance of the catalyst is improved after phosphorus doping.
[0062] Comparative Example 2
[0063] (1) Add PAN into DMF and stir until it is completely dissolved to obtain a homogeneous solution having a mass concentration of 9.5%.
[0064] (2) The obtained PAN solution was injected into a syringe, and the uniaxial electrospinning parameters were adjusted for electrospinning to obtain a PAN film; after pre-oxidation in a muffle furnace at 250°C and carbonization in a tubular furnace at 800°C, carbon nanowires were obtained. During the spinning process, the needle pushing speed was controlled at 0.085 mm / min, the distance between the nozzle and the receiver was fixed at 15 cm, and the applied high voltage was 15 KV.
[0065] Except for preparing carbon nanowires as a substrate by uniaxial electrospinning, other conditions were the same as those in Example 2 to prepare P-MoS2 / CoS2-2@CNFs catalyst.
[0066] Figure 1 e is the SEM image of CNFs prepared by uniaxial electrospinning. Figure 1 f is the SEM image of the product P-MoS2 / CoS2-2@CNFs prepared in Example 1. It can be seen that P-MoS2 / CoS2 maintains the original nanosheet morphology. Compared with the product P-MoS2 / CoS2@CNFs (250mV@100mAcm) obtained in Example 2 using carbon nanowires as the substrate, -2 ), the product P-MoS2 / CoS2@HCNFs obtained in Example 2 was -2 The overpotential of the catalyst is lower, which is 196 mV. This indicates that the electrocatalyst prepared on the hollow carbon nanofibers has better mass transfer performance.
[0067] According to the CV curves at different scan rates, the C dl , revealing the electrode kinetics and interfacial reactions. Figure 3 As shown in c, the Cdl value of the product P-MoS2 / CoS2@HCNFs obtained in Example 2 is 13.4 mF cm -2 , which is significantly higher than the product MoS2 / CoS2@HCNFs (9.4 mF cm) obtained in Comparative Example 1. -2 ) and the product P-MoS2 / CoS2@CNFs (11.2 mF cm) obtained in Comparative Example 2 -2 ), indicating that the structural advantages brought by phosphorus-doped MoS2 / CoS2 and nanotubes provide more surface active sites.
[0068] The above-described embodiments merely express the implementation methods of the present invention, but they cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that for those skilled in the art, several modifications and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention.
Claims
1. A method for preparing a 1D carbon-supported phosphorus-doped sulfide nanotube catalyst for water electrolysis, It is characterized in that The preparation method firstly adopts coaxial electrospinning to prepare hollow carbon nanofibers; secondly, a hydrothermal method is used to in-situ grow MoS on the surface of the hollow carbon nanofibers. 2 / CoS 2 ; Finally, through the phosphorus doping strategy, the intrinsic activity of the catalyst active sites was improved to obtain 1D carbon-supported phosphorus-doped sulfide nanotube catalyst.
2. A method for preparing a 1D carbon-supported phosphorus-doped sulfide nanotube catalyst for water electrolysis according to claim 1, It is characterized in that The following steps are involved: Step (1) preparing shell layer solution and core layer solution: Add polyacrylonitrile (PAN) into N,N-dimethylformamide (DMF) and stir until completely dissolved to obtain a shell layer solution; add polymethyl methacrylate (PMMA) into DMF and stir until completely dissolved to obtain a core layer solution; Step (2) preparing hollow carbon nanofibers by coaxial electrospinning: The shell layer solution and the core layer solution obtained in step (1) are respectively injected into two solution channels of the coaxial electrospinning, and the coaxial electrospinning parameters are adjusted to perform electrospinning to obtain a PAN / PMMA film; Then, the PAN / PMMA film was pre-oxidized in a muffle furnace and carbonized in a tube furnace to obtain hollow carbon nanofibers HCNFs; Step (3) Preparation of MoS 2 / CoS 2 @HCNFs: The hollow carbon nanofibers obtained in step (2) are activated by concentrated nitric acid; the hollow carbon nanofibers are immersed in a homogeneous aqueous solution containing ammonium molybdate tetrahydrate, cobalt nitrate hexahydrate and thiourea for hydrothermal treatment to obtain MoS 2 / CoS 2 @HCNFs; Step (4) The MoS 2 / CoS 2 @HCNFs and sodium hypophosphite were placed in the center and upstream of the tube furnace respectively; 1D carbon-supported phosphorus-doped sulfide nanotubes P-MoS were obtained by high-temperature phosphating under inert gas protection. 2 / CoS 2 @HCNFs.
3. A method for preparing a 1D carbon-supported phosphorus-doped sulfide nanotube catalyst for water electrolysis according to claim 2, It is characterized in that In the step (1), the mass concentration of PAN in the shell layer solution is 9-10%, and the mass concentration of PMMA in the core layer solution is 9.5-10.5%.
4. The method for preparing a 1D carbon-supported phosphorus-doped sulfide nanotube catalyst for water electrolysis according to claim 2, It is characterized in that In the step (2), the pre-oxidation temperature is 230-270° C., and the time is 1-2 h; the carbonization temperature is 750-850° C., and the time is 1-2 h.
5. The method for preparing a 1D carbon-supported phosphorus-doped sulfide nanotube catalyst for water electrolysis according to claim 2, It is characterized in that In the step (2), during the coaxial electrospinning process, when two relatively independent nozzles are used for simultaneous spinning, the pushing speeds of the shell solution and the inner solution are controlled at 0.08-0.09 mm / min and 0.03-0.05 mm / min, respectively; the distance between the nozzle and the receiver is fixed at 14-16 cm, and the applied high voltage is 14-16 KV.
6. A method for preparing a 1D carbon-supported phosphorus-doped sulfide nanotube catalyst for water electrolysis according to claim 2, It is characterized in that In the step (3): The nitric acid activation treatment comprises: ultrasonicating the HCNFs in a concentrated nitric acid solution for 1 to 2 hours, washing and drying them for later use; The molar ratio of the ammonium molybdate tetrahydrate, the cobalt nitrate hexahydrate and the thiourea is 1:1:33 to 1:3:33; The temperature of the hydrothermal treatment is 160-220° C., and the time is 18-24 hours.
7. The method for preparing a 1D carbon-supported phosphorus-doped sulfide nanotube catalyst for water electrolysis according to claim 2, It is characterized in that In the step (4): The inert gas is nitrogen; The temperature of the high temperature phosphating is 300-400°C and the time is 1-2h; The MoS 2 / CoS 2 @The mass ratio of HCNFs to 1g sodium hypophosphite is 1:
10.
8. A 1D carbon-supported phosphorus-doped sulfide nanotube catalyst for water electrolysis. It is characterized in that The nanotube catalyst is obtained by the preparation method described in any one of claims 1-7.
9. Use of the 1D carbon-supported phosphorus-doped sulfide nanotube catalyst for water electrolysis according to claim 8, It is characterized in that The 1D carbon-supported phosphorus-doped sulfide nanotube catalyst is applied to water electrolysis and has excellent water electrolysis catalytic performance.
10. Use of a 1D carbon-supported phosphorus-doped sulfide nanotube catalyst according to claim 9, It is characterized in that The electrochemical activity of 1D carbon-supported phosphorus-doped sulfide nanotube catalyst for water electrolysis was tested under alkaline conditions, 10 mA cm -2 The overpotential is 85 mV and the Tafel slope is 68.6 mV dec. -1 .
Citation Information
Cited By
Cerium-doped carbon-coated iron oxide composite fiber and preparation method thereof
CN122358366A