Preparation method of stitch-bonded all-cotton medical dressing with stable structure

By preparing multi-layer or single-layer fiber webs using nonwoven technology and sewing them on a Mariwatt sewing machine, the problem of insufficient permeability in existing medical dressings is solved, achieving higher absorption and permeability and structural stability, and reducing wound dehydration and mechanical damage.

CN118910799APending Publication Date: 2024-11-08JIANGNAN UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410989038.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing medical dressings lack sufficient permeability and absorption capacity, which can easily lead to wound dehydration and infection risks.

Method used

Multi-layer or single-layer fiber webs are prepared using nonwoven technology and then sewn on a Mariwatt sewing machine. By changing parameters such as fiber web thickness, comb transverse displacement, and yarn fineness, the absorption and permeability and structural stability of the dressing are improved.

Benefits of technology

It improves the absorption and permeability of dressings and their structural stability, reduces the risk of wound dehydration and mechanical damage, and enhances wound moisturization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910799A_ABST
    Figure CN118910799A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of a stitch-bonded all-cotton medical dressing with a stable structure, and belongs to the technical field of textiles. A single-layer or multi-layer fiber net is prepared through a non-weaving process, and the fiber net is stitched and knitted by utilizing a Mariwatt stitch-knitting machine, so that the absorption and infiltration capacity of the dressing is effectively improved, and the stitch-knitting speed is also increased; wherein the multiple layers of non-woven fiber nets are stitched and knitted by means of overlapping, and the single-layer non-woven fiber nets respectively perform chaining motion and weft insertion motion by utilizing two guide bars, so that the stability and the mechanical property of the dressing structure can be effectively improved, meanwhile, the wound surface can be kept moist, and mechanical injury is prevented from occurring again when the dressing is replaced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a sewn all-cotton medical dressing with a stable structure, and belongs to the technical field of textiles. Background Art

[0002] With the in-depth study of the pathophysiology of wound healing, people have a deeper understanding of the wound healing process, which has led to the continuous improvement and development of medical wound dressings. Natural gauze is widely used in the wound healing process because of its advantages of rapid absorption of wound exudate and relatively simple production and processing. However, due to the high permeability of pure cotton dressings, it is easy to dehydrate the wound surface, and the large amount of use and frequent replacement gradually limit its application. In view of this, it is necessary to improve the existing products.

[0003] At present, the existing technology only has wound dressings such as those shown in CN110013382A and CN114401703A. Although they can heal wounds, their technical means have not improved the permeability and absorption and penetration capacity of the dressings, which may easily cause a certain infection risk to the wound. Summary of the invention

[0004] In order to solve the above problems, in a first aspect, the present invention provides a method for preparing a stitched all-cotton medical dressing with a stable structure, wherein after the dressing is prepared by a non-woven process, the multi-layer fiber web on the dressing is stitched on a Maliwatt stitching machine, and then finished;

[0005] The dressing comprises 4.7% of 32S / 2-60S / 2 pure cotton staple yarn and 95.3% of long-staple cotton; the base fabric used in the nonwoven process is a finished lining fabric that has been processed by an opener, a cotton feeder, a carding machine, a web laying machine, a needle punching machine, an ironing machine, and a winding machine in sequence;

[0006] The Maliwatt stitching machine includes a yarn guide needle located in front of the grey cloth, a groove needle located behind the grey cloth, a needle core located above the groove needle, a lower baffle located on one side of the grey cloth, and a knock-off sinker matched with the lower baffle, wherein the lower baffle is provided with a baffle needle; the yarn guide needle leads the stitching yarn to the stitching area, and the plane where the multi-layer fiber web is located is tilted at an angle of 45 degrees to the vertical plane to feed it into the stitching area.

[0007] The preparation method specifically comprises the following steps:

[0008] Step 1: Select 32S / 2~60S / 2 pure cotton short-fiber yarn and long-staple cotton as raw materials;

[0009] Step 2: Fiber web forming: The long-staple cotton is processed into a multi-layer fiber web structure through a non-woven process, and the multi-layer fiber web is fed into the Maliwatt stitching machine at the same time; wherein the fiber web thickness is 1mm to 2mm, and the square meter weight is 190 to 334g / m2;

[0010] Step 3: Sewing the multi-layer fiber mesh on the dressing on a Maliwatt sewing machine;

[0011] Step 4: Perform quality inspection on the woolen cloth obtained after stitching in step 3 to obtain the finished dressing product, and then package it.

[0012] Furthermore, the step 4 also includes performing two performance tests on the finished dressing, including:

[0013] Water vapor permeability test: Place the dressing sample to be tested at the mouth of a sample bottle filled with distilled water, seal the part of the dressing sample in contact with the bottle mouth with a sealing film, and ensure that the height between the dressing sample and the water surface is maintained at 20 mm. Then place the dressing sample bottle in an environment with a temperature of 37°C and a humidity of 50±5% for 24 hours; finally, use an electronic balance to weigh the total mass of the sample bottle before and after the experiment, and calculate the water vapor permeability according to the following formula to analyze the water vapor permeability:

[0014] Where: G is mass change; t is time; A is the area of ​​the sample bottle;

[0015] Mechanical property test: Cut the finished dressing product of step 4 into dressing samples with a size of 1 cm×5 cm, and test the tensile fracture performance of the dressing samples on an electronic universal tensile testing machine, setting the tensile speed to 5 mm / min and the effective clamping distance to 2 cm.

[0016] In the step 3, an RFX fiber mesh sewing machine with a machine gauge of 3.5 needles is used for sewing, and the width is set to 1700 mm; wherein the warp knitting structure and the threading method during the sewing process are:

[0017] Organization: GB1 comb: 0-1 / / , full penetration A;

[0018] Raw materials: GB1:32S / 2 pure cotton staple yarn;

[0019] The yarn and the comb are matched as follows: GB1 is stitched with pure cotton staple yarn; the weight is changed by changing the thickness of the fiber web, the lateral displacement of the comb, the threading rate and the fineness of the yarn, and the weight per square meter of the finished dressing is 200-350g / m2;

[0020] During the stitching process, the fabric yarn digital data, warp let-off and drawing density are transmitted to the control cabinet and saved.

[0021] In a second aspect, the present invention provides another method for preparing a stitched all-cotton medical dressing with a stable structure, wherein after the dressing is prepared by a nonwoven process, a single-layer fiber web on the dressing is stitched on a Maliwatt stitching machine, and then finished;

[0022] The dressing comprises 9.8% of 32S / 2-60S / 2 pure cotton staple yarn and 90.2% of long-staple cotton; the base fabric used in the nonwoven process is a finished lining fabric that has been processed by an opener, a cotton feeder, a carding machine, a web laying machine, a needle punching machine, an ironing machine, and a winding machine in sequence;

[0023] The Maliwatt stitching machine comprises a GB1 yarn guide needle and a GB2 yarn guide needle located in front of the grey cloth, a groove needle located behind the grey cloth, a needle core located above the groove needle, a lower baffle plate located on one side of the grey cloth, and a knock-off sinker matched with the lower baffle plate, wherein the lower baffle plate is provided with a baffle needle; the GB1 yarn guide needle and the GB2 yarn guide needle respectively lead the stitching yarn to the stitching area, and the plane where the multi-layer fiber web is located is tilted to form an angle of 45 degrees with the vertical plane to feed the stitching area;

[0024] The Maliwatt stitch-bonding machine is knitted by the cooperation of two comb bars, one comb bar performs chain-knitting motion, and the other comb bar performs weft-inserting motion.

[0025] The preparation method specifically comprises the following steps:

[0026] Step 1: Select 32S / 2~60S / 2 pure cotton short-fiber yarn and long-staple cotton as raw materials;

[0027] Step 2: Fiber web forming: The long-staple cotton is processed into a single-layer fiber web structure through a non-woven process, and the single-layer fiber web is fed into a Maliwatt stitching machine; wherein the fiber web thickness is 0.5 mm to 1.5 mm, and the square meter grammage is 161 to 278 g / m2;

[0028] Step 3: Stitching the single-layer fiber mesh on the dressing on a Maliwatt stitching machine;

[0029] Step 4: Perform quality inspection on the woolen cloth obtained after stitching in step 3 to obtain the finished dressing product, and then package it.

[0030] The step 4 also includes two performance tests on the finished dressing, including:

[0031] Water vapor permeability test: Place the dressing sample to be tested at the mouth of a sample bottle filled with distilled water, seal the part of the dressing sample in contact with the bottle mouth with a sealing film, and ensure that the height between the dressing sample and the water surface is maintained at 20 mm. Then place the dressing sample bottle in an environment with a temperature of 37°C and a humidity of 50±5% for 24 hours; finally, use an electronic balance to weigh the total mass of the sample bottle before and after the experiment, and calculate the water vapor permeability according to the following formula to analyze the water vapor permeability:

[0032] Where: G is mass change; t is time; A is the area of ​​the sample bottle;

[0033] Mechanical property test: Cut the finished dressing product of step 4 into dressing samples with a size of 1 cm×5 cm, and test the tensile fracture performance of the dressing samples on an electronic universal tensile testing machine, setting the tensile speed to 5 mm / min and the effective clamping distance to 2 cm.

[0034] In the step 3, a RFX fiber mesh sewing machine with a machine gauge of 5 needles is used for sewing, and the width is set to 1700 mm; wherein the warp knitting structure and the threading method during the sewing process are:

[0035] organize:

[0036] GB1 comb: 0-1 / / , full penetration A;

[0037] GB2 comb: 0-0 / 2-2 / 2-2 / 2-2 / 2-2 / 0-0 / 0-0 / 0-0 / / , full penetration A;

[0038] raw material:

[0039] GB1: 32S / 2 pure cotton staple yarn;

[0040] GB2: 32S / 2 pure cotton staple yarn;

[0041] The yarn and the comb are matched as follows: GB1 and GB2 are both stitched with pure cotton staple yarn; the weight is changed by changing the thickness of the fiber web, the lateral displacement of the comb, the threading rate and the fineness of the yarn, and the weight per square meter of the finished dressing is 180-310 g / m2;

[0042] During the stitching process, the fabric yarn digital data, warp let-off and drawing density are transmitted to the control cabinet and saved.

[0043] Beneficial effects of the present invention:

[0044] The present invention manufactures a single-layer or multi-layer fiber web through a non-woven process, and uses a Maliwatt sewing machine to sew the fiber web, which not only effectively improves the absorption and penetration capacity of the dressing, but also improves the sewing speed; wherein, the multi-layer non-woven fiber web is sewn by means of overlapping, and the single-layer non-woven fiber web uses two combs to perform chain movement and weft insertion movement respectively, which can effectively improve the stability and mechanical properties of the dressing structure, and at the same time can help keep the wound surface moist, avoiding mechanical damage again when changing the dressing. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 This is a diagram of the stitching structure of the Maliwatt stitching machine of Example 1 of the present invention.

[0046] Figure 2 This is a diagram of the stitching structure of the Maliwatt stitching machine of Example 2 of the present invention.

[0047] Figure 3 This is a stitching structure diagram and a physical picture of the finished dressing product of Example 1 of the present invention.

[0048] Figure 4 This is a stitching structure diagram and a physical picture of the finished dressing product of Example 2 of the present invention.

[0049] Figure 1 Among them, 1. knock-over sinker; 2. groove needle; 3. needle core; 4. single-layer fiber net; 5. baffle needle; 6. stitching yarn; 7. yarn guide needle; 8. lower baffle; 9. grey cloth;

[0050] Figure 2 Among them, 1. knock-over sinker; 2. groove needle; 3. needle core; 4. multi-layer fiber net; 5. baffle needle; 6. GB1 stitching yarn; 7. GB1 guide needle; 8. GB2 stitching yarn; 9. GB2 guide needle; 10. lower baffle; 11. grey cloth. DETAILED DESCRIPTION

[0051] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0052] In the present invention, unless otherwise clearly specified and limited, the terms "connected", "connected", and "fixed" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0053] In the present invention, the "first" and "second" are only used to distinguish similar components / parts with different positions or different characteristics, and have no other limiting meanings; the "upper" refers to the direction of each component away from the ground, and the "lower" refers to the direction of each component away from the ground.

[0054] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may include that the first and second features are in direct contact, or may include that the first and second features are not in direct contact but are in contact through another feature between them. Moreover, a first feature being "above", "above" and "above" a second feature includes that the first feature is directly above and obliquely above the second feature, or simply indicates that the first feature is higher in level than the second feature. A first feature being "below", "below" and "below" a second feature includes that the first feature is directly below and obliquely below the second feature, or simply indicates that the first feature is lower in level than the second feature.

[0055] Example 1

[0056] like Figure 1 , Figure 3 As shown, the present invention provides a method for preparing a stitched all-cotton medical dressing with a stable structure. After the dressing is prepared by a non-woven process, the multi-layer fiber web on the dressing is stitched on a Maliwatt stitching machine, and then finished;

[0057] The dressing comprises 4.7% of 32S / 2-60S / 2 pure cotton staple yarn and 95.3% of long-staple cotton; the base fabric used in the nonwoven process is a finished lining fabric that has been processed by an opener, a cotton feeder, a carding machine, a web laying machine, a needle punching machine, an ironing machine, and a winding machine in sequence;

[0058] The Maliwatt stitching machine includes a yarn guide needle 7 located in front of the grey cloth 9, a groove needle 2 located behind the grey cloth 9, a needle core 3 located above the groove needle 2, a lower baffle 8 located on one side of the grey cloth 9, and a knock-off sedimentation plate 1 coordinated with the lower baffle 8, wherein the lower baffle 8 is provided with a baffle needle 5; the yarn guide needle 7 leads the stitching yarn to the stitching area, and the plane where the multi-layer fiber web is located is tilted at an angle of 45 degrees to the vertical plane and fed into the stitching area.

[0059] The preparation method specifically comprises the following steps:

[0060] Step 1: Select 32S / 2~60S / 2 pure cotton short-fiber yarn and long-staple cotton as raw materials;

[0061] Step 2: Fiber web forming: The long-staple cotton is processed into a multi-layer fiber web structure through a non-woven process, and the multi-layer fiber web is fed into the Maliwatt stitching machine at the same time; wherein the fiber web thickness is 1mm to 2mm, and the square meter weight is 190 to 334g / m2;

[0062] Step 3: Sewing the multi-layer fiber mesh on the dressing on a Maliwatt sewing machine;

[0063] Step 4: Perform quality inspection on the woolen cloth obtained after stitching in step 3 to obtain the finished dressing product, and then package it.

[0064] Furthermore, the step 4 also includes performing two performance tests on the finished dressing, including:

[0065] Water vapor permeability test: Place the dressing sample to be tested at the mouth of a sample bottle filled with distilled water, seal the part of the dressing sample in contact with the bottle mouth with a sealing film, and ensure that the height between the dressing sample and the water surface is maintained at 20 mm. Then place the dressing sample bottle in an environment with a temperature of 37°C and a humidity of 50±5% for 24 hours; finally, use an electronic balance to weigh the total mass of the sample bottle before and after the experiment, and calculate the water vapor permeability according to the following formula to analyze the water vapor permeability:

[0066] Where: G is mass change; t is time; A is the area of ​​the sample bottle;

[0067] Mechanical property test: Cut the finished dressing product of step 4 into dressing samples with a size of 1 cm×5 cm, and test the tensile fracture performance of the dressing samples on an electronic universal tensile testing machine, setting the tensile speed to 5 mm / min and the effective clamping distance to 2 cm.

[0068] In the step 3, an RFX fiber mesh sewing machine with a machine gauge of 3.5 needles is used for sewing, and the width is set to 1700 mm; wherein the warp knitting structure and the threading method during the sewing process are:

[0069] Organization: GB1 comb: 0-1 / / , full penetration A;

[0070] Raw materials: GB1:32S / 2 pure cotton staple yarn;

[0071] The yarn and the comb are matched as follows: GB1 is stitched with pure cotton staple yarn; the weight is changed by changing the thickness of the fiber web, the lateral displacement of the comb, the threading rate and the fineness of the yarn, and the weight per square meter of the finished dressing is 200-350g / m2;

[0072] During the stitching process, the fabric yarn digital data, warp let-off and drawing density are transmitted to the control cabinet and saved.

[0073] Example 2

[0074] like Figure 2 , Figure 4 As shown, the present invention provides another method for preparing a sewn all-cotton medical dressing with a stable structure. After the dressing is prepared by a non-woven process, the single-layer fiber web on the dressing is sewn on a Maliwatt sewing machine and then finished.

[0075] The dressing comprises 9.8% of 32S / 2-60S / 2 pure cotton staple yarn and 90.2% of long-staple cotton; the base fabric used in the nonwoven process is a finished lining fabric that has been processed by an opener, a cotton feeder, a carding machine, a web laying machine, a needle punching machine, an ironing machine, and a winding machine in sequence;

[0076] The Maliwatt stitching machine comprises a GB1 yarn guide needle 7 and a GB2 yarn guide needle 9 located in front of the grey cloth 11, a groove needle 2 located behind the grey cloth 11, a needle core 3 located above the groove needle 2, a lower baffle plate 10 located on one side of the grey cloth 11, and a knock-over sinker 1 matched with the lower baffle plate 10, wherein the lower baffle plate 10 is provided with a baffle needle 5; the GB1 yarn guide needle 7 and the GB2 yarn guide needle 9 respectively lead the GB1 stitching yarn 6 and the GB2 stitching yarn 8 to the stitching area, and the plane where the multi-layer fiber web is located is tilted to form an angle of 45 degrees with the vertical plane to feed into the stitching area;

[0077] The Maliwatt stitch-bonding machine is knitted by the cooperation of two comb bars, one comb bar performs chain-knitting motion, and the other comb bar performs weft-inserting motion.

[0078] The preparation method specifically comprises the following steps:

[0079] Step 1: Select 32S / 2~60S / 2 pure cotton short-fiber yarn and long-staple cotton as raw materials;

[0080] Step 2: Fiber web forming: The long-staple cotton is processed into a single-layer fiber web structure through a non-woven process, and the single-layer fiber web is fed into a Maliwatt stitching machine; wherein the fiber web thickness is 0.5 mm to 1.5 mm, and the square meter grammage is 161 to 278 g / m2;

[0081] Step 3: Stitching the single-layer fiber mesh on the dressing on a Maliwatt stitching machine;

[0082] Step 4: Perform quality inspection on the woolen cloth obtained after stitching in step 3 to obtain the finished dressing product, and then package it.

[0083] The step 4 also includes two performance tests on the finished dressing, including:

[0084] Water vapor permeability test: Place the dressing sample to be tested at the mouth of a sample bottle filled with distilled water, seal the part of the dressing sample in contact with the bottle mouth with a sealing film, and ensure that the height between the dressing sample and the water surface is maintained at 20 mm. Then place the dressing sample bottle in an environment with a temperature of 37°C and a humidity of 50±5% for 24 hours; finally, use an electronic balance to weigh the total mass of the sample bottle before and after the experiment, and calculate the water vapor permeability according to the following formula to analyze the water vapor permeability:

[0085] Where: G is mass change; t is time; A is the area of ​​the sample bottle;

[0086] Mechanical property test: Cut the finished dressing product of step 4 into dressing samples with a size of 1 cm×5 cm, and test the tensile fracture performance of the dressing samples on an electronic universal tensile testing machine, setting the tensile speed to 5 mm / min and the effective clamping distance to 2 cm.

[0087] In the step 3, a RFX fiber mesh sewing machine with a machine gauge of 5 needles is used for sewing, and the width is set to 1700 mm; wherein the warp knitting structure and the threading method during the sewing process are:

[0088] organize:

[0089] GB1 comb: 0-1 / / , full penetration A;

[0090] GB2 comb: 0-0 / 2-2 / 2-2 / 2-2 / 2-2 / 0-0 / 0-0 / 0-0 / / , full penetration A;

[0091] raw material:

[0092] GB1: 32S / 2 pure cotton staple yarn;

[0093] GB2: 32S / 2 pure cotton staple yarn;

[0094] The yarn and the comb are matched as follows: GB1 and GB2 are both stitched with pure cotton staple yarn; the weight is changed by changing the thickness of the fiber web, the lateral displacement of the comb, the threading rate and the fineness of the yarn, and the weight per square meter of the finished dressing is 180-310 g / m2;

[0095] During the stitching process, the fabric yarn digital data, warp let-off and drawing density are transmitted to the control cabinet and saved.

[0096] Although the present invention has been disclosed as above in the form of a preferred embodiment, it is not intended to limit the present invention. Anyone familiar with this technology can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be based on the definition of the claims.

Claims

1. A method for preparing a structurally stable stitched all-cotton medical dressing, characterized in that: After the dressing is made by nonwoven process, the multi-layer fiber web on the dressing is stitched on the Maliwatt stitching machine and then finished; The dressing comprises 4.7% of 32S / 2-60S / 2 pure cotton staple yarn and 95.3% of long-staple cotton; the base fabric used in the nonwoven process is a finished lining fabric that has been processed by an opener, a cotton feeder, a carding machine, a web laying machine, a needle punching machine, an ironing machine, and a winding machine in sequence; The Maliwatt stitching machine includes a yarn guide needle located in front of the grey cloth, a groove needle located behind the grey cloth, a needle core located above the groove needle, a lower baffle located on one side of the grey cloth, and a knock-off sinker matched with the lower baffle, wherein the lower baffle is provided with a baffle needle; the yarn guide needle leads the stitching yarn to the stitching area, and the plane where the multi-layer fiber web is located is tilted at an angle of 45 degrees to the vertical plane to feed it into the stitching area.

2. The method for preparing a structurally stable stitched all-cotton medical dressing according to claim 1, characterized in that: The preparation method specifically comprises the following steps: Step 1: Select 32S / 2~60S / 2 pure cotton short-fiber yarn and long-staple cotton as raw materials; Step 2: Fiber web forming: The long-staple cotton is processed into a multi-layer fiber web structure through a non-woven process, and the multi-layer fiber web is fed into the Maliwatt stitching machine at the same time; wherein the fiber web thickness is 1mm to 2mm, and the square meter weight is 190 to 334g / m 2 ; Step 3: Sewing the multi-layer fiber mesh on the dressing on a Maliwatt sewing machine; Step 4: Perform quality inspection on the woolen cloth obtained after stitching in step 3 to obtain the finished dressing product, and then package it.

3. The method for preparing a structurally stable stitched all-cotton medical dressing according to claim 2, characterized in that: The step 4 also includes two performance tests on the finished dressing, including: Water vapor permeability test: Place the dressing sample to be tested at the mouth of a sample bottle filled with distilled water, seal the part of the dressing sample in contact with the bottle mouth with a sealing film, and ensure that the height between the dressing sample and the water surface is maintained at 20 mm. Then place the dressing sample bottle in an environment with a temperature of 37°C and a humidity of 50±5% for 24 hours; finally, use an electronic balance to weigh the total mass of the sample bottle before and after the experiment, and calculate the water vapor permeability according to the following formula to analyze the water vapor permeability: Where: G is mass change; t is time; A is the area of ​​the sample bottle; Mechanical property test: Cut the finished dressing product of step 4 into dressing samples with a size of 1 cm×5 cm, and test the tensile fracture performance of the dressing samples on an electronic universal tensile testing machine, setting the tensile speed to 5 mm / min and the effective clamping distance to 2 cm.

4. The method for preparing a structurally stable stitched all-cotton medical dressing according to claim 3, characterized in that: In the step 3, an RFX fiber mesh sewing machine with a machine gauge of 3.5 needles is used for sewing, and the width is set to 1700 mm; wherein the warp knitting structure and the threading method during the sewing process are: Organization: GB1 comb: 0-1 / / , full penetration A; Raw materials: GB1:32S / 2 pure cotton staple yarn; The yarn and the comb are matched as follows: GB1 is sewn with pure cotton staple yarn; the weight is changed by changing the thickness of the fiber web, the lateral displacement of the comb, the threading rate and the fineness of the yarn. The weight per square meter of the finished dressing is 200-350 g / m 2 ; During the stitching process, the fabric yarn digital data, warp let-off and drawing density are transmitted to the control cabinet and saved.

5. A method for preparing a structurally stable stitched all-cotton medical dressing, characterized in that: After the dressing is made by nonwoven process, the single-layer fiber web on the dressing is stitched on a Maliwatt stitching machine and then finished; The dressing comprises 9.8% of 32S / 2-60S / 2 pure cotton staple yarn and 90.2% of long-staple cotton; the base fabric used in the nonwoven process is a finished lining fabric that has been processed by an opener, a cotton feeder, a carding machine, a web laying machine, a needle punching machine, an ironing machine, and a winding machine in sequence; The Maliwatt stitching machine comprises a GB1 yarn guide needle and a GB2 yarn guide needle located in front of the grey cloth, a groove needle located behind the grey cloth, a needle core located above the groove needle, a lower baffle plate located on one side of the grey cloth, and a knock-off sinker matched with the lower baffle plate, wherein the lower baffle plate is provided with a baffle needle; the GB1 yarn guide needle and the GB2 yarn guide needle respectively lead the stitching yarn to the stitching area, and the plane where the multi-layer fiber web is located is tilted to form an angle of 45 degrees with the vertical plane to feed the stitching area; The Maliwatt stitch-bonding machine is knitted by the cooperation of two comb bars, one comb bar performs chain-knitting motion, and the other comb bar performs weft-inserting motion.

6. The method for preparing a structurally stable stitched all-cotton medical dressing according to claim 5, characterized in that: The preparation method specifically comprises the following steps: Step 1: Select 32S / 2~60S / 2 pure cotton short-fiber yarn and long-staple cotton as raw materials; Step 2: Fiber web forming: The long-staple cotton is processed into a single-layer fiber web structure through a non-woven process, and the single-layer fiber web is fed into the Maliwatt stitching machine; wherein the fiber web thickness is 0.5mm to 1.5mm, and the square meter grammage is 161 to 278g / m 2 ; Step 3: Stitching the single-layer fiber mesh on the dressing on a Maliwatt stitching machine; Step 4: Perform quality inspection on the woolen cloth obtained after stitching in step 3 to obtain the finished dressing product, and then package it.

7. The method for preparing a structurally stable stitched all-cotton medical dressing according to claim 6, characterized in that: The step 4 also includes two performance tests on the finished dressing, including: Water vapor permeability test: Place the dressing sample to be tested at the mouth of a sample bottle filled with distilled water, seal the part of the dressing sample in contact with the bottle mouth with a sealing film, and ensure that the height between the dressing sample and the water surface is maintained at 20 mm. Then place the dressing sample bottle in an environment with a temperature of 37°C and a humidity of 50±5% for 24 hours; finally, use an electronic balance to weigh the total mass of the sample bottle before and after the experiment, and calculate the water vapor permeability according to the following formula to analyze the water vapor permeability: Where: G is mass change; t is time; A is the area of ​​the sample bottle; Mechanical property test: Cut the finished dressing product of step 4 into dressing samples with a size of 1 cm×5 cm, and test the tensile fracture performance of the dressing samples on an electronic universal tensile testing machine, setting the tensile speed to 5 mm / min and the effective clamping distance to 2 cm.

8. The method for preparing a structurally stable stitched all-cotton medical dressing according to claim 7, characterized in that: In the step 3, a RFX fiber mesh sewing machine with a machine gauge of 5 needles is used for sewing, and the width is set to 1700 mm; wherein the warp knitting structure and the threading method during the sewing process are: organize: GB1 comb: 0-1 / / , full penetration A; GB2 comb: 0-0 / 2-2 / 2-2 / 2-2 / 2-2 / 0-0 / 0-0 / 0-0 / / , full penetration A; raw material: GB1: 32S / 2 pure cotton staple yarn; GB2: 32S / 2 pure cotton staple yarn; The yarn and the comb are matched as follows: GB1 and GB2 are both stitched with pure cotton staple yarn; the weight is changed by changing the thickness of the fiber web, the lateral displacement of the comb, the threading rate and the yarn fineness, and the weight per square meter of the finished dressing is 180-310 g / m 2 ; During the stitching process, the fabric yarn digital data, warp let-off and drawing density are transmitted to the control cabinet and saved.

Citation Information

Patent Citations

  • Vertical fiber web type non-yarn knit-stitch machine with clamping and feeding devices

    CN112853597A

  • Functional medical wound dressing and preparation method thereof

    CN117338987A

  • Process for making nonwoven fabrics

    CN1629382A

  • Method for producing all cotton non-woven fabric medical dressing

    CN1664210A