Persistent antistatic treatment method for high-elastic polyester fibers

By blending polyester fibers with amide-based fibers and forming an antistatic coating on their surfaces, combined with carbon nanotube antistatic materials, the problem of insufficient antistatic performance of polyester fibers in the prior art is solved, and efficient electrostatic protection and heat are achieved Improved stability.

CN118910891APending Publication Date: 2024-11-08JIANGSU DINGXIN PRINTING & DYEING
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411159766.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing antistatic treatment methods have limited improvements in the antistatic properties of polyester fibers, resulting in static problems that affect product user experience and safety.

Method used

Aimide-based fiber is prepared by blending polyester fibers with amide-based fibers and forming an antistatic coating on its surface. Amid-based fibers are prepared by polyethylene glycol, maleic anhydride and bio-based amides, and combined with carbon nanotube antistatic materials to enhance the fiber resistance. Electrostatic and thermal stability.

Benefits of technology

It significantly improves the anti-static and wear resistance of polyester composite fibers, extends the anti-static effect, and improves the thermal stability and mechanical properties of the fibers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005006104640000081
    Figure BDA0005006104640000081
  • Figure BDA0005006104640000091
    Figure BDA0005006104640000091
Patent Text Reader

Abstract

The invention relates to a lasting antistatic treatment method for high-elastic polyester fibers, which comprises the following steps: S1, immersing polyester composite fibers into an antistatic solution, and attaching an antistatic coating to the surfaces of the polyester composite fibers; s2, the soaked polyester composite fibers are taken out and dried, and then the antistatic coating forms an antistatic coating on the surfaces of the polyester composite fibers; s3, carrying out heat treatment on the dried composite fiber to obtain the polyester antistatic fiber; the polyester composite fibers are obtained by blending polyester fibers and amide-based fibers, and the amide-based fibers comprise polyethylene glycol, maleic anhydride and bio-based polyamide. The antistatic polyester fiber has the antistatic effect of the polyester fiber.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of textile fiber processing, and in particular to a method for persistent electrostatic processing of highly elastic fibers. Background Art

[0002] Polyester fiber has good elasticity and wear resistance and is widely used in fabrics.

[0003] However, polyester fibers are prone to generate and accumulate static electricity, which not only affects the product experience, but also causes safety issues. Most of the existing antistatic treatment methods directly coat the surface of polyester fibers with antistatic agents, but the improvement of the antistatic properties of polyester fibers is limited. Therefore, the development of a method that can maintain the antistatic properties of polyester fibers has become an urgent need in the current textile industry. Summary of the invention

[0004] In order to further improve the antistatic performance of polyester fibers, the present application provides a durable antistatic treatment method for high-elastic polyester fibers.

[0005] The present application provides a durable antistatic treatment method for high-elastic polyester fibers using the following technical solutions: A durable antistatic treatment method for high-elastic polyester fiber comprises the following steps: S1, immersing the polyester composite fiber in an antistatic solution, and attaching an antistatic coating to the surface of the polyester composite fiber; S2, taking out the soaked polyester composite fiber, and drying it, so that the antistatic coating forms an antistatic coating on the surface of the polyester composite fiber; S3, heat-treating the dried composite fiber to obtain polyester antistatic fiber; The polyester composite fiber is obtained by blending polyester fiber with amide-based fiber, and the amide-based fiber includes polyethylene glycol, maleic anhydride and bio-based polyamide.

[0006] By adopting the above technical scheme, polyester composite fiber is prepared by blending polyester fiber and amide-based fiber, and amide-based fiber is prepared by polyethylene glycol, maleic anhydride and bio-based amide. Bio-based polyamide has good mechanical and thermal properties. Polyethylene glycol is a polyether polymer compound with excellent performance and good biocompatibility. Amide-based fiber prepared by maleic anhydride compound has good antistatic and wear resistance. The polyester fiber obtained by blending amide-based fiber and polyester fiber can directly improve the antistatic property of the fiber. The antistatic coating is combined on the surface of the polyester composite fiber to form an antistatic coating on the surface of the polyester composite fiber. The antistatic coating has good antistatic properties. After being combined with the polyester composite fiber, the antistatic property of the polyester composite fiber can be effectively improved.

[0007] Preferably, the amide-based fiber is prepared by the following method: Polyethylene glycol, maleic anhydride and pyridine are mixed, heated to react, cooled after the reaction, and the product is separated and extracted to obtain a double-terminal hydroxyl complex; the double-terminal hydroxyl complex, pentanediol, bio-based amide and water are mixed, heated to react while maintaining stirring conditions to obtain an amide product, the amide product is dried, and melt-spinning is performed to obtain amide fibers.

[0008] By adopting the above technical scheme, the polyethylene glycol is modified with terminal hydroxyl groups and then copolymerized with bio-based polyamide. The amide-based fibers obtained after spinning have good antistatic properties, good tensile strength and breaking growth rate, so that the comprehensive performance of the polyester composite fiber is improved. The prepared polyester composite fiber also has good hydrophilicity and can be combined with antistatic coatings more stably.

[0009] Preferably, the mass ratio between the double-terminal hydroxyl complex and the bio-based polyamide is 1:(3.4-3.8).

[0010] By adopting the above technical solution, the mass ratio between the double-terminal hydroxyl compound and the bio-based polyamide is preferably within the above range, which can further improve the comprehensive performance of the prepared amide-based fiber.

[0011] Preferably, the antistatic coating comprises waterborne polyurethane, a dispersant and a carbon nanotube antistatic material.

[0012] By adopting the above technical solution and adding carbon nanotube antistatic material to the electrostatic coating, the antistatic material can be more stably bonded to the surface of the polyester composite fiber, thereby improving the antistatic durability of the polyester composite fiber after antistatic treatment. Carbon nanotubes have good thermal conductivity and antistatic properties, which can further improve the antistatic properties and thermal stability of the prepared polyester composite fiber, while improving the mechanical properties of the prepared antistatic coating, making the antistatic coating more stable.

[0013] Preferably, the carbon nanotube antistatic material comprises modified carbon nanotubes, nanosilver and paraffin.

[0014] By adopting the above technical scheme, paraffin has good physical and chemical stability and large phase change latent heat, and nanosilver particles also have good thermal stability and antistatic properties. Phase change composite materials are prepared by paraffin, nanosilver and modified carbon nanotubes, which can improve the thermal stability and antistatic properties of antistatic coatings. After combining with polyester composite fibers, the overall antistatic properties and thermal stability of the fibers are further improved.

[0015] Preferably, the carbon nanotube antistatic material is prepared by the following method: Silver nitrate and modified carbon nanotubes are mixed and added to oleylamine, stirred and added to molten paraffin, reacted under nitrogen atmosphere and oil bath conditions, and finally aged, cooled, crushed and ground to obtain carbon nanotube antistatic material.

[0016] By adopting the above technical solution, nanosilver particles are modified on multi-walled carbon nanotubes, and then the carbon nanotube antistatic material is prepared by paraffin compounding, so that the system has good synergistic antistatic performance and thermal stability.

[0017] Preferably, the mass ratio of the modified carbon nanotubes, silver nitrate and paraffin is (0.42-0.46):0.26:1.

[0018] By adopting the above technical solution, the mass ratio of silver nitrate, modified carbon nanotubes and paraffin is preferably within the above range, which can further improve the comprehensive performance of the carbon nanotube antistatic material.

[0019] Preferably, the modified carbon nanotubes include multi-walled carbon nanotubes and dopamine hydrochloride.

[0020] Preferably, the modified carbon nanotubes are prepared by the following method: Multi-walled carbon nanotubes are added into Tris buffer and ultrasonically treated to obtain a carbon nanotube dispersion; dopamine is mixed with water, added into the carbon nanotube dispersion to stir for reaction, then washed, and finally dried to obtain modified carbon nanotubes.

[0021] By adopting the above technical scheme, the surface of the carbon nanotubes is modified by dopamine, and a large number of functional groups are introduced into the surface of the carbon nanotubes, which effectively reduces the surface energy of the carbon nanotubes and effectively improves the self-aggregation problem of the carbon nanotubes, making the carbon nanotubes more stably dispersed in the system. The dopamine coated on the surface of the carbon nanotubes is an organic modification layer, which can improve the interface effect of the carbon nanotubes, so that the carbon nanotube antistatic material has good bonding performance and is more stable with the polyester composite fiber.

[0022] Preferably, the mass ratio of the multi-walled carbon nanotubes to dopamine hydrochloride is 1:(0.4-0.6).

[0023] By adopting the above technical solution, preferably the mass ratio of multi-walled carbon nanotubes to dopamine hydrochloride is within the above range, which can further improve the stability of the prepared modified carbon nanotubes.

[0024] In summary, the present application includes at least one of the following beneficial technical effects: 1. The antistatic and mechanical properties of polyester composite fibers prepared by blending amide-based fibers with polyester fibers prepared by polyethylene glycol, maleic anhydride and bio-based amides are improved, so that the fiber components have good antistatic and wear resistance; 2. Adding carbon nanotube antistatic material to antistatic coating can improve the overall antistatic performance of polyester composite fiber together with antistatic agent. At the same time, the carbon nanotube antistatic material prepared by modifying carbon nanotubes, nanosilver and paraffin has good thermal stability, which further improves the thermal stability of polyester composite fiber. 3. The surface of the carbon nanotubes is modified by dopamine, so that the surface of the carbon nanotubes has a large number of functional groups, which reduces the surface energy of the carbon nanotubes and enables the carbon nanotubes to be more evenly dispersed in the system. DETAILED DESCRIPTION

[0025] The present application is further described in detail below with reference to the embodiments: Raw material description: All raw materials in the examples can be obtained commercially; the dispersant in the antistatic coating is BYK-194N.

[0026] Example 1 Preparation of modified carbon nanotubes: A 0.1 mol / L Tris solution was mixed with a 0.1 mol / L hydrochloric acid solution to obtain a Tris buffer solution with a pH value of 8.5, and 21.13 g of multi-walled carbon nanotubes (CAS No.: 1333-86-4) were added to 5000 ml of Tris buffer solution, and ultrasonicated for 1 hour to obtain a carbon nanotube dispersion; 8.87 g of dopamine (CAS No.: 51-61-6) was mixed with 20 g of deionized water, added to the carbon nanotube dispersion, and stirred at a speed of 300 r / min for 4 hours. Then, the product was washed alternately with ethanol and deionized water for 3 times, and finally dried in an oven at 70°C for 4 hours to obtain modified carbon nanotubes.

[0027] Preparation of carbon nanotube antistatic materials: 12.38 g of silver nitrate was mixed with 20 g of modified carbon nanotubes, then added to 700 g of oleylamine, stirred at 300 r / min at 50°C for 30 min, then added to 47.62 g of molten paraffin, nitrogen was introduced, and the temperature was raised to 200°C under nitrogen atmosphere and oil bath conditions, followed by reaction for 2 h, and finally matured at 150°C for 6 h, and then crushed and ground after cooling to obtain a carbon nanotube antistatic material.

[0028] Preparation of antistatic coating: 400 g of waterborne polyurethane, 20 g of carbon nanotube antistatic material, 2.2 g of antistatic agent and 7 g of dispersant were mixed, and stirred at a speed of 600 r / min for 15 min to obtain an antistatic coating.

[0029] Wherein, the antistatic agent is polyethylene glycol (CAS No.: 25322-68-3).

[0030] Preparation of amide fibers: 109.4 g of polyethylene glycol, 30 g of maleic anhydride (CAS No.: 108-31-6) and 0.1 g of pyridine (CAS No.: 110-86-1) were mixed, and the temperature was raised to 170 ° C under a nitrogen atmosphere and maintained for 6 hours. After the reaction, the mixture was cooled to 25 ° C, the product was separated, and ether was used to extract a brown viscous substance to obtain a double-terminal hydroxyl complex; 24.39 g of the double-terminal hydroxyl complex, 12 g of pentanediol, and 75.61 g of bio-based amide (CAS No.: 41724-56-5) were mixed. The mixture was mixed with 120 g of deionized water, and the pH value of the system was adjusted to 9. The mixture was mechanically stirred under a nitrogen atmosphere and vacuum conditions. The stirring condition was maintained and the temperature was raised to 235°C. When the pressure reached 1.8 MPa, the pressure condition was maintained and the temperature was raised to 265°C. The mixture was vacuumed and then discharged to obtain an amide product. The amide product was dried in a vacuum oven at 100°C for 48 hours. The mixture was melt-spun using a torque rheometer. The temperatures of the spinning screw zone 1, zone 2, zone 3, zone 4 and zone 4 were set to 170°C, 260°C, 280°C and 280°C, and amide fibers were obtained after spinning.

[0031] Preparation of polyester composite fiber: The polyester fiber and the amide-based composite fiber are mixed in a mass ratio of 7:3, and then blended to obtain the polyester composite fiber.

[0032] Preparation of polyester antistatic fiber: S1. Completely immersing the polyester composite fiber into the antistatic solution so that the antistatic coating adheres to the surface of the polyester composite fiber; S2, taking out the soaked polyester composite fiber, and drying it with hot air for 30 minutes at 60° C., so that an antistatic coating is formed on the surface of the polyester composite fiber; S3. The dried polyester composite fiber is heat treated at 120° C. for 15 minutes to obtain polyester antistatic fiber.

[0033] Example 2 Preparation of modified carbon nanotubes: A 0.1 mol / L Tris solution was mixed with a 0.1 mol / L hydrochloric acid solution to obtain a Tris buffer solution with a pH value of 8.5, and 20.27 g of multi-walled carbon nanotubes were added to 5000 ml of Tris buffer solution, and ultrasonicated for 1 hour to obtain a carbon nanotube dispersion. 9.73 g of dopamine was mixed with 20 g of deionized water, added to the carbon nanotube dispersion, and stirred at a speed of 300 r / min for 4 hours. The product was then washed alternately with ethanol and deionized water for 3 times, and finally dried in an oven at 70°C for 4 hours to obtain modified carbon nanotubes.

[0034] Preparation of carbon nanotube antistatic materials: 12.09 g of silver nitrate was mixed with 21.4 g of modified carbon nanotubes, then added to 700 g of oleylamine, stirred at 300 r / min at 50 ° C for 30 min, then added to 46.51 g of molten paraffin, nitrogen was introduced, and the temperature was raised to 200 ° C under nitrogen atmosphere and oil bath conditions, followed by reaction for 2 h, and finally matured at 150 ° C for 6 h, and then crushed and ground after cooling to obtain a carbon nanotube antistatic material.

[0035] Preparation of antistatic coating: 420 g of waterborne polyurethane, 28 g of carbon nanotube antistatic material, 9.5 g of antistatic agent and 11 g of dispersant were mixed, and stirred at a speed of 600 r / min for 15 min to obtain an antistatic coating.

[0036] Among them, the antistatic agent is antistatic agent SH-105.

[0037] Preparation of amide fibers: 109.4 g of polyethylene glycol, 30 g of maleic anhydride and 0.1 g of pyridine were mixed, and the temperature was raised to 170 ° C under a nitrogen atmosphere and kept at the temperature for 6 hours. After the reaction, the mixture was cooled to 25 ° C, the product was separated, and a brown viscous substance was extracted with ether to obtain a double-terminal hydroxyl complex; 20.83 g of the double-terminal hydroxyl complex, 12 g of pentyl salt, 79.17 g of bio-based amide and 120 g of deionized water were mixed, and the pH value of the system was adjusted to 9. Mechanical stirring was performed under nitrogen atmosphere and vacuum conditions, and the temperature was raised to 235°C while maintaining the stirring conditions. When the pressure reached 1.8 MPa, the pressure conditions were maintained and the temperature was raised to 265°C. After vacuuming, the material was discharged to obtain an amide product. The amide product was dried in a vacuum oven at 100°C for 48 hours, and melt-spun using a torque rheometer. The temperatures of the spinning screw zone 1 were set to 170°C, zone 2 to 260°C, zone 3 to 280°C, and zone 4 to 280°C. After spinning, amide fibers were obtained.

[0038] Preparation of polyester composite fiber: The polyester fiber and the amide-based composite fiber are mixed in a mass ratio of 3:2, and then blended to obtain the polyester composite fiber.

[0039] Preparation of polyester antistatic fiber: S1. Completely immersing the polyester composite fiber into the antistatic solution so that the antistatic coating adheres to the surface of the polyester composite fiber; S2, taking out the soaked polyester composite fiber, and drying it with hot air for 10 minutes at 80° C., so that an antistatic coating is formed on the surface of the polyester composite fiber; S3. The dried polyester composite fiber is heat treated at 150° C. for 5 minutes to obtain polyester antistatic fiber.

[0040] Example 3 Preparation of modified carbon nanotubes: A 0.1 mol / L Tris solution was mixed with a 0.1 mol / L hydrochloric acid solution to obtain a Tris buffer solution with a pH value of 8.5, and 20.69 g of multi-walled carbon nanotubes were added to 5000 ml of Tris buffer solution, and ultrasonicated for 1 hour to obtain a carbon nanotube dispersion. 9.31 g of dopamine was mixed with 20 g of deionized water, added to the carbon nanotube dispersion, and stirred at a speed of 300 r / min for 4 hours. The product was then washed alternately with ethanol and deionized water for 3 times, and finally dried in an oven at 70°C for 4 hours to obtain modified carbon nanotubes.

[0041] Preparation of carbon nanotube antistatic materials: 12.23 g of silver nitrate was mixed with 20.71 g of modified carbon nanotubes, then added to 700 g of oleylamine, stirred at 300 r / min at 50 ° C for 30 min, then added to 47.06 g of molten paraffin, nitrogen was introduced, and the temperature was raised to 200 ° C under nitrogen atmosphere and oil bath conditions, followed by reaction for 2 h, and finally matured at 150 ° C for 6 h, and then crushed and ground after cooling to obtain a carbon nanotube antistatic material.

[0042] Preparation of antistatic coating: 410 g of waterborne polyurethane, 24 g of carbon nanotube antistatic material, 4.8 g of antistatic agent and 9 g of dispersant were mixed, and stirred at a speed of 600 r / min for 15 min to obtain an antistatic coating.

[0043] Wherein, the antistatic agent is polyethylene glycol.

[0044] Preparation of amide fibers: 109.4 g of polyethylene glycol, 30 g of maleic anhydride and 0.1 g of pyridine were mixed, and the temperature was raised to 170 ° C under a nitrogen atmosphere and kept at the temperature for 6 hours. After the reaction, the mixture was cooled to 25 ° C, the product was separated, and a brown viscous substance was extracted with ether to obtain a double-terminal hydroxyl complex; 21.74 g of the double-terminal hydroxyl complex, 12 g of pentyl salt, 78.26 g of bio-based amide and 120 g of deionized water were mixed, and the pH value of the system was adjusted to 9. Mechanical stirring was performed under nitrogen atmosphere and vacuum conditions, and the temperature was raised to 235°C while maintaining the stirring conditions. When the pressure reached 1.8 MPa, the pressure conditions were maintained and the temperature was raised to 265°C. After vacuuming, the material was discharged to obtain an amide product. The amide product was dried in a vacuum oven at 100°C for 48 hours, and melt-spun using a torque rheometer. The temperatures of the spinning screw zone 1 were set to 170°C, zone 2 to 260°C, zone 3 to 280°C, and zone 4 to 280°C. After spinning, amide fibers were obtained.

[0045] Preparation of polyester composite fiber: The polyester fiber and the amide-based composite fiber are mixed in a mass ratio of 3:2, and then blended to obtain the polyester composite fiber.

[0046] Preparation of polyester antistatic fiber: S1. Completely immersing the polyester composite fiber into the antistatic solution so that the antistatic coating adheres to the surface of the polyester composite fiber; S2, taking out the soaked polyester composite fiber, and drying it with hot air for 20 minutes at 70° C., so that an antistatic coating is formed on the surface of the polyester composite fiber; S3. The dried polyester composite fiber is heat treated at 135° C. for 8 minutes to obtain polyester antistatic fiber.

[0047] Example 4 Example 4 is based on Example 3. The difference between Example 4 and Example 3 is that in Example 4, when preparing modified carbon nanotubes, 22.22 g of carbon nanotubes and 7.78 g of dopamine are used.

[0048] Example 5 Example 5 is based on Example 3. The difference between Example 5 and Example 3 is that in Example 5, when preparing modified carbon nanotubes, 19.35 g of carbon nanotubes and 10.65 g of dopamine are used.

[0049] Example 6 Example 6 is based on Example 3. The difference between Example 6 and Example 3 is that when preparing the carbon nanotube antistatic material, Example 6 uses 17.39 g of modified carbon nanotubes, 12.92 g of silver nitrate, and 49.69 g of paraffin.

[0050] Example 7 Example 7 is based on Example 3. The difference between Example 7 and Example 3 is that when preparing the carbon nanotube antistatic material, Example 7 uses 24.31 g of modified carbon nanotubes, 11.49 g of silver nitrate, and 44.2 g of paraffin.

[0051] Example 8 Example 8 is based on Example 3. The difference between Example 8 and Example 3 is that when preparing the carbon nanotube antistatic material, Example 8 replaces the modified carbon nanotubes with ordinary carbon nanotubes.

[0052] Example 9 Example 9 is based on Example 3. The difference between Example 9 and Example 3 is that the carbon nanotube antistatic material in Example 9 is prepared by physically mixing nanosilver particles and modified carbon nanotubes.

[0053] Example 10 Example 10 is based on Example 3. The difference between Example 10 and Example 3 is that in Example 10, when preparing amide-based fibers, 25 g of the double-terminal hydroxyl complex and 75 g of the bio-based amide are used.

[0054] Embodiment 11 Example 11 is based on Example 3. The difference between Example 11 and Example 3 is that in Example 11, when preparing amide-based fibers, 19.23 g of the double-terminal hydroxyl complex and 80.77 g of the bio-based amide are used.

[0055] Example 12 Example 12 is based on Example 3. The difference between Example 12 and Example 3 is that in Example 12, 1 g of antistatic agent is used when preparing the antistatic coating.

[0056] Embodiment 13 Example 13 is based on Example 3. The difference between Example 13 and Example 3 is that in Example 13, 15 g of antistatic agent is used when preparing the antistatic coating.

[0057] Embodiment 14 Example 14 is based on Example 3. The difference between Example 14 and Example 3 is that in Example 14, when preparing polyester antistatic fiber, in step S2, the temperature of hot air drying treatment is 40°C.

[0058] Embodiment 15 Example 15 is based on Example 3. The difference between Example 15 and Example 3 is that in Example 15, when preparing polyester antistatic fiber, in step S2, the temperature of hot air drying treatment is 100°C.

[0059] Example 16 Example 16 is based on Example 3. The difference between Example 16 and Example 3 is that in Example 16, when preparing polyester antistatic fiber, in step S3, the heat treatment temperature is 100°C.

[0060] Embodiment 17 Example 17 is based on Example 3. The difference between Example 17 and Example 3 is that in Example 17, when preparing polyester antistatic fiber, in step S3, the heat treatment temperature is 170°C.

[0061] Comparative Example 1 Comparative Example 1 is based on Example 3, and in Comparative Example 1, the polyester composite fiber is replaced by polyester fiber.

[0062] Comparative Example 2 Comparative Example 2 is based on Example 3, and in Comparative Example 2, the carbon nano antistatic composite material is replaced by modified carbon nanotubes.

[0063] Performance testing The samples of Examples 1-17 and Comparative Examples 1-2 were sampled and the following performance tests were performed: (1) Antistatic performance test The surface resistance of the fiber was tested. Each sample was tested three times, the average value was taken, and the test results were filled in Table 1.

[0064] (2) Wear resistance test The wear resistance of the samples was tested according to GB T 21196.2-2007. Each sample was tested 3 times, and the average value was taken. The test results were filled in Table 1.

[0065] (3) Tensile strength test The tensile strength of the sample fibers was tested three times, and the test results were filled in Table 1.

[0066] Table 1 Test results of antistatic polyester fiber performance of Examples 1-17 and Comparative Examples 1-2 Data analysis Combined with Table 1, it can be seen that the surface resistance of Examples 1-3 is 6.0Ω or less, indicating that the fibers prepared in the present application have good antistatic properties; the wear times of Examples 1-3 are 50,000 times or more, indicating that the fibers prepared in the present application have good wear resistance; the tensile strength of Examples 1-3 is 60.0cN / dtex or more, indicating that the fibers prepared in the present application have good tensile resistance.

[0067] The mass ratios of carbon nanotubes to dopamine in Examples 4 and 5 are not within the range defined in the present application. When the dopamine content is too high, a thick coating will be formed on the surface of the carbon nanotubes, affecting the overall stability of the carbon nanotubes, thereby reducing the binding ability between the carbon nanotubes and nanosilver and paraffin, and affecting the overall performance of the carbon nanotube antistatic material; when the dopamine content is too low, it is difficult to graft uniformly on the surface of the carbon nanotubes, making it difficult to further improve the surface energy of the carbon nanotubes, and the dispersion performance in the system is reduced, which will also affect the dispersion performance of the carbon nanotubes.

[0068] The mass ratio of modified carbon nanotubes, silver nitrate and paraffin in Examples 6 and 7 is reduced. When the content of modified carbon nanotubes is too much, too many carbon nanotubes will agglomerate in the system, thereby affecting the overall stability of the prepared carbon nanotube antistatic material. When the content of modified carbon nanotubes is too little, it is difficult to make the nanosilver particles grow uniformly on the surface of the carbon nanotubes, thus affecting the overall performance of the carbon nanotube antistatic material.

[0069] In Example 8, when preparing the carbon nanotube antistatic material, the modified carbon nanotubes were replaced with ordinary carbon nanotubes. The surface energy of the unmodified carbon nanotubes is difficult to improve and it is difficult to disperse them evenly in the system, which reduces the stability of the prepared carbon nanotube antistatic material and affects the overall performance of the system.

[0070] In Example 9, the modified carbon nanotubes are only physically mixed with the nanosilver particles. It is difficult to further combine the carbon nanotubes and the nanosilver particles with ordinary mixing, and it is difficult to obtain a continuous skeleton structure and a stable phase change material. The thermal stability of the system is reduced.

[0071] In Examples 10 and 11, when preparing amide-based fibers, the mass ratio between the double-terminal hydroxyl complex and the bio-based amide is not within the range specified in the present application. When the content of the bio-based amide is too little, the excessive double-terminal hydroxyl complex destroys the crystallization ability of the bio-based amide and affects the overall stability of the system. When the content of the bio-based amide is too much, the entanglement effect between the double-terminal hydroxyl complex and the bio-based amide is difficult to be further improved, and the binding effect between the two is reduced, affecting the overall stability of the system.

[0072] The content of the antistatic agent in Example 12 is too little, and the improvement of the antistatic performance of the polyester composite fiber is reduced. The content of the antistatic agent in Example 13 is too much, which may affect the stability of the polyester composite fiber. Therefore, the performance of Examples 12 and 13 are both reduced.

[0073] When treating polyester antistatic fibers, if the hot air drying temperature is too high or too low, or the heat treatment temperature is too high or too low, it will affect the bonding performance between the polyester composite fiber and the antistatic coating, thereby affecting the comprehensive performance of the polyester antistatic fibers. Therefore, the performance of Examples 14-17 is reduced.

[0074] In Comparative Example 1, amide-based fibers and polyester fibers are not blended, the hydrophilicity of ordinary polyester fibers is reduced, and the bonding performance with antistatic coatings is difficult to be further improved. At the same time, the mechanical properties of unblended fibers are also reduced.

[0075] In Comparative Example 2, the carbon nanotube antistatic composite material is replaced by modified carbon nanotubes. It is difficult to further improve the overall antistatic performance of the antistatic coating system using only carbon nanotubes, and the thermal stability is also difficult to be further improved.

[0076] This specific embodiment is only an explanation of the present application, and it is not a limitation of the present application. Through the above description, relevant staff can make various changes and modifications without deviating from the technical idea of ​​the present application. The technical scope of the present application is not limited to the content in the specification, and its technical scope must be determined according to the scope of the claims.

Claims

1. A durable antistatic treatment method for high-elastic polyester fiber, characterized in that: The steps include: S1, immersing the polyester composite fiber in an antistatic solution, and attaching an antistatic coating to the surface of the polyester composite fiber; S2, taking out the soaked polyester composite fiber, and drying it, so that the antistatic coating forms an antistatic coating on the surface of the polyester composite fiber; S3, heat-treating the dried composite fiber to obtain polyester antistatic fiber; The polyester composite fiber is obtained by blending polyester fiber with amide-based fiber, and the amide-based fiber includes polyethylene glycol, maleic anhydride and bio-based polyamide.

2. The method for durable antistatic treatment of high elastic polyester fiber according to claim 1, characterized in that: The amide-based fiber is prepared by the following method: Polyethylene glycol, maleic anhydride and pyridine are mixed, heated to react, cooled after the reaction, and the product is separated and extracted to obtain a double-terminal hydroxyl complex; the double-terminal hydroxyl complex, pentanediol, bio-based amide and water are mixed, heated to react while maintaining stirring conditions to obtain an amide product, the amide product is dried, and melt-spinning is performed to obtain amide fibers.

3. The method for treating high-elastic polyester fiber with a durable antistatic property according to claim 2, characterized in that: The mass ratio between the double-terminal hydroxyl compound and the bio-based polyamide is 1:(3.4-3.8).

4. The method for durable antistatic treatment of high elastic polyester fiber according to claim 1, characterized in that: The antistatic coating comprises waterborne polyurethane, a dispersant and a carbon nanotube antistatic material.

5. The method for durable antistatic treatment of high elastic polyester fiber according to claim 4, characterized in that: The carbon nanotube antistatic material comprises modified carbon nanotubes, nanosilver and paraffin.

6. The method for durable antistatic treatment of high elastic polyester fiber according to claim 4, characterized in that: The carbon nanotube antistatic material is prepared by the following method: Silver nitrate and modified carbon nanotubes are mixed and added to oleylamine, stirred and added to molten paraffin, reacted under nitrogen atmosphere and oil bath conditions, and finally aged, cooled, crushed and ground to obtain carbon nanotube antistatic material.

7. The method for durable antistatic treatment of high elastic polyester fiber according to claim 5, characterized in that: The mass ratio of the modified carbon nanotubes, silver nitrate and paraffin is (0.42-0.46):0.26:

1.

8. The method for durable antistatic treatment of high elastic polyester fiber according to claim 5, characterized in that: The modified carbon nanotubes include multi-walled carbon nanotubes and dopamine hydrochloride.

9. A durable antistatic treatment method for high-elastic polyester fiber according to claim 8, characterized in that: The modified carbon nanotubes are prepared by the following method: Multi-walled carbon nanotubes are added into Tris buffer and ultrasonically treated to obtain a carbon nanotube dispersion; dopamine is mixed with water, added into the carbon nanotube dispersion to stir for reaction, then washed, and finally dried to obtain modified carbon nanotubes.

10. The method for durable antistatic treatment of high elastic polyester fiber according to claim 8, characterized in that: The mass ratio between the multi-walled carbon nanotubes and dopamine hydrochloride is 1:(0.4-0.6).