Machine-washable durable antistatic mulberry silk fabric and finishing process thereof
By using the combination technology of cationic alkoxyamine compounds and polyether polyurethane compounds on silk fabrics, a mesh electrostatic shielding layer is formed, which solves the problems of electrostatic adsorption and washing resistance of silk fabrics after machine washing, and achieves low temperature The durable and anti-static effect of the styling ensures the machine-washing resistance and anti-static properties of the fabric.
Patent Information
- Application Number
- CN202411014494.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-08
AI Technical Summary
Silk fabrics are prone to dust damage and reduced gloss after machine washing, and have strong electrostatic adsorption effect, resulting in problems with clothing production and body fitting. The existing anti-static technology is not suitable for silk fabrics, and dry cleaning is expensive and inconvenient, and large. Some dry cleaning agents are toxic to the environment.
The combination of cationic alkoxyamine compounds as antistatic finishing agents and polyether polyurethane compounds as moisture absorption and quick-drying agents is formed to form a mesh electrostatic shielding layer, which is uniformly distributed on the surface of mulberry silk fabrics through hydrogen bonds and chemical bonds, and is low-temperature The styling treatment is carried out at 120-130℃ to achieve durable and anti-static effect.
The machine-resistant and durable anti-static properties of silk fabrics are realized. The fabric is still hydrophilic after 10 machine-washings, maintaining good anti-static functions. The drip diffusion time is less than 5s, the resistance is less than 1012Ω, and the feel and color of the fabric before and after treatment. Small changes.
Smart Images

Figure BDA0004965315530000071 
Figure BDA0004965315530000072
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of textiles, and in particular to a machine-washable durable antistatic mulberry silk fabric and a finishing process thereof. Background Art
[0002] Silk is the only filament fiber among the four major natural fibers, with unique properties. Silk fabrics made from it are light, smooth, soft and skin-friendly, with good moisture absorption, breathability and soft luster. They have always been popular as high-end clothing fabrics. However, silk fabrics are relatively fragile and cannot be machine washed. After machine washing, the fabrics will be grayed, the glossiness will be reduced, and even irregular white marks will appear, which seriously affects the appearance of the silk fabrics; in addition, the silk fabrics have strong electrostatic adsorption after drying, which will cause problems such as adsorption on the cutting bed and wearing close to the body during subsequent clothing production. In addition, silk is not resistant to drying, so it is generally cleaned by dry cleaning, which is expensive and inconvenient, and most of the dry cleaning agents are toxic to the environment. Therefore, improving the machine washable antistatic properties of silk has also become a difficult and important issue in the research of silk fabrics.
[0003] At present, the methods to improve the antistatic properties of fabrics can be divided into physical methods and chemical methods. Physical methods include blending conductive fibers, increasing fabric moisture, grounding conductivity and reducing friction, but they are not suitable for the operation and application of silk fabrics to be washable and antistatic. Chemical methods include adding antistatic agents during spinning, fiber surface modification, blending or embedding conductive fibers, and antistatic agent finishing. Silk is a natural filament fiber. Under the premise of not affecting the special properties of the fabric, antistatic agent finishing is currently the most effective and convenient solution.
[0004] At present, Ding Xingxing et al. use polyester polyether raw materials to prepare universal washable antistatic agents, and apply them to polyester fabrics and polyester wool fabrics. After finishing, the surface resistance of the fabrics can be increased from 10 15 Ω down to 10 9 Ω, and can be washed 50 times; Hong Jiayong prepared a durable antistatic agent of polyether polyamide and applied it to nylon. After finishing, the hydrophilicity was enhanced, the half-life of the induced voltage was reduced to 2.45s, and it could be washed at least 30 times; Zhou Yongkai et al. used synthetic polyester antistatic agents to antistatic finish wool / polyester fiber fabrics. After finishing, the static voltage half-life of the fabric was reduced to 3.2 seconds, and it could be washed 50 times. However, the baking temperature of the above finishing methods is above 150℃, which is not suitable for mass production of silk fabrics.
[0005] Therefore, there is an urgent need to develop a machine-washable durable antistatic mulberry silk fabric and a durable antistatic finishing technology that can be baked at low temperature and is suitable for mulberry silk fabric. Summary of the invention
[0006] The purpose of the present invention is to provide a machine-washable durable antistatic mulberry silk fabric and its finishing process, the fabric has good hydrophilic and antistatic effects, and has excellent machine washability and durable antistatic performance. After 10 machine washes, the fabric is still hydrophilic and can maintain good antistatic function. The antistatic finishing process is simple and reliable, and can achieve a durable antistatic effect under low temperature conditions of 120-130°C, and the fabric feel and color change before and after treatment is small.
[0007] In order to achieve the above object, the present invention adopts the following technical solutions:
[0008] In a first aspect of the present invention, there is provided a machine-washable durable antistatic mulberry silk fabric, wherein the mulberry silk fabric is dipped or padded into a finishing liquid to form a hydrophilic mesh electrostatic shielding layer on its surface;
[0009] The finishing liquid comprises an antistatic finishing agent and a moisture absorbing and quick-drying agent, wherein the antistatic finishing agent is a cationic alkoxyamine compound, and the moisture absorbing and quick-drying agent is a polyether polyurethane compound.
[0010] Using the above technical solution:
[0011] Although the cationic alkoxyamine compound used alone as an antistatic finishing agent has excellent antistatic effect, it has low affinity to the fibers in mulberry silk fabrics, resulting in the antistatic effect of the fabric not being durable and not resistant to machine washing.
[0012] In the present application, a hydrophilic polyether polyurethane compound is creatively selected as a moisture absorbing and quick-drying agent, and the polyether polyurethane compound is compounded with a cationic alkoxyamine compound. The polyether polyurethane chemical has a strong polymerization film-forming ability, and forms a polyurethane film layer on the surface of the mulberry silk fabric. The antistatic finishing agent-cationic alkoxyamine compound is evenly distributed in the polyurethane film in a network through hydrogen bonds and chemical bonds. Through the synergistic effect of the above two additives, they effectively form a hydrophilic network electrostatic shielding layer on the fabric, accelerate the dissipation of the surface charge of the fabric, thereby enhancing the antistatic performance of the fabric, achieving durable antistatic performance, and solving the problem of low affinity of the antistatic finishing agent-cationic alkoxyamine compound to the fibers in the mulberry silk fabric. The mulberry silk fabric treated with the antistatic finishing agent and the moisture absorbing quick-drying agent has excellent hydrophilic and antistatic properties, and has good durability and machine washability. After 5 to 10 machine washes, the fabric is still hydrophilic and can maintain good antistatic function. The drip diffusion time can still reach less than 5s, and the specific resistivity is still within 10 12 Ω or less.
[0013] Furthermore, the concentration of the antistatic finishing agent in the finishing liquid is 10-30 g / L, and the concentration of the moisture absorbing quick-drying agent is 20-60 g / L.
[0014] Furthermore, the dosage ratio of the antistatic finishing agent to the moisture absorbing quick-drying agent in the finishing liquid is 1:2.
[0015] Furthermore, the antistatic finishing agent is TANASTAT WP or HEALTHBAO 2022.
[0016] Furthermore, the moisture absorbing and quick-drying agent is Transtex 6220 or Hydroperm RPU.
[0017] Furthermore, the mulberry silk fabric is not dyed, and after being dipped into the finishing liquid, the mulberry silk fabric is baked and set at 120-130°C.
[0018] After the mulberry silk fabric is treated with the finishing liquid with a specific formula ratio in the present application, it is baked at a low temperature of 120-130°C to achieve a durable antistatic effect on the fabric, and the feel and color of the fabric before and after the treatment change little.
[0019] Furthermore, before the mulberry silk fabric is treated with the finishing liquid, it is re-scouted with a rapid refining agent, and the rapid refining agent is a compound of a buffer alkali and a non-ionic surfactant.
[0020] Under alkaline conditions, non-ionic surfactants are first used to remove grease and wax on the surface of silk fabrics, making it easier for the auxiliaries in the finishing liquid to adsorb and form a film on the fabric surface.
[0021] In the present application, the mulberry silk fabric (the scoured white embryo of the mulberry silk fabric) is firstly subjected to a re-scouring treatment, then treated with a finishing liquid, and then subjected to a dyeing treatment, which will not affect the dyeing effect of the fabric.
[0022] A second aspect of the present invention provides a machine washable durable antistatic finishing process for mulberry silk fabrics, comprising the following steps:
[0023] S1. Re-scouring the undyed silk fabric with a rapid scouring agent;
[0024] S2, mixing an antistatic finishing agent, a moisture absorbing quick-drying agent and water to form a finishing liquid, wherein the concentration of the antistatic finishing agent in the finishing liquid is 10-30 g / L, and the concentration of the moisture absorbing quick-drying agent is 20-60 g / L;
[0025] S3, applying the finishing liquid to the mulberry silk fabric after the re-scouring treatment by dipping or padding;
[0026] S4, the mulberry silk fabric after the dipping or padding treatment is baked and set by a setting machine, the baking temperature is 120-130° C., and the baking time is 90-110 seconds.
[0027] Furthermore, the antistatic finishing agent is a cationic alkoxyamine compound, and the moisture absorbing and quick-drying agent is a polyether polyurethane compound.
[0028] Furthermore, the rapid refining agent is a compound of a buffer alkali and a nonionic surfactant.
[0029] Compared with the prior art, the present invention has the following beneficial effects:
[0030] (1) In the present application, a hydrophilic polyether polyurethane compound is selected as a moisture absorbing and quick-drying agent, and the polyether polyurethane compound is compounded with a cationic alkoxyamine compound. The polyether polyurethane chemical has a strong polymerization film-forming ability, and forms a polyurethane film layer on the surface of the mulberry silk fabric. The antistatic finishing agent-cationic alkoxyamine compound is evenly distributed in the polyurethane film in a network through hydrogen bonds and chemical bonds. Through the synergistic effect of the above two additives, they effectively form a hydrophilic network electrostatic shielding layer on the fabric, accelerate the dissipation of the surface charge of the fabric, thereby enhancing the antistatic performance of the fabric, achieving durable antistatic performance, and solving the problem of low affinity of the antistatic finishing agent-cationic alkoxyamine compound to the fibers in the mulberry silk fabric;
[0031] (2) The mulberry silk fabric treated with the above antistatic finishing agent and moisture absorbing quick-drying agent has excellent hydrophilic and antistatic properties, and has excellent machine wash resistance and durable antistatic properties. After 5 to 10 machine washes, the fabric is still hydrophilic and can maintain good antistatic function. The drip diffusion time can still reach less than 5s, and the specific resistivity is still within 10 12 Ω or less;
[0032] (3) Moreover, the durable antistatic finishing technology for mulberry silk fabrics is simple and reliable, and can achieve a durable antistatic effect at low temperatures of 120-130°C. The feel and color of the fabric change little before and after treatment. DETAILED DESCRIPTION
[0033] The technical solutions in the present invention will be described clearly and completely below in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] The present invention is further described below by way of examples. Unless otherwise specified, the various reagents and raw materials used in the present invention are all commercially available products or products that can be prepared by known methods.
[0035] Example 1
[0036] Fabric: 16m / m silk crepe satin
[0037] (1) Pretreatment: The 16 m / m silk crepe satin scouring white embryo fabric was rolled up on the warp beam for rescouring, and the fabric was rescored at 90 °C for 50 min using 2 g / L rapid refining agent (Miltopan SE), and then dried at 120 °C for 1 min in a setting machine;
[0038] (2) Ingredients: Add 1 kg of antistatic finishing agent (TANASTATWP) to 100 L of water, stir evenly, then add 2 kg of moisture absorbing quick-drying agent (Transtex 6220), stir evenly to prepare a finishing liquid, and add the prepared finishing liquid into the rolling tank;
[0039] (3) Padding: The roller pressure is set to 3 kg, and the fabric is padded once with the finishing liquid, with a liquid rate of about 80%. The padded fabric is then baked on a setting machine at 130°C for 90 seconds to obtain a finished fabric.
[0040] Example 2
[0041] Fabric: 16m / m silk crepe satin
[0042] (1) Pretreatment: The 16 m / m silk crepe satin scouring white embryo fabric was rolled up on the warp beam for rescouring, and the fabric was scouted at 90 °C for 30 min using 2 g / L rapid scouring agent (Miltopan SE), and then dried at 120 °C for 1 min in a setting machine;
[0043] (2) Ingredients: Add 2 kg of antistatic finishing agent (HEALTHBAO 2022) to 100 L of water and stir evenly, then add 4 kg of moisture absorbing quick-drying agent (Hydroperm RPU) and stir evenly to prepare a finishing liquid, and add the prepared finishing liquid into the rolling tank;
[0044] (3) Padding: The roller pressure is set to 3 kg, and the fabric is padded once with the finishing liquid, with a liquid rate of about 80%. The padded fabric is then baked on a setting machine at 120°C for 110 seconds to obtain a finished fabric.
[0045] Example 3
[0046] Fabric: 19m / m silk stretch satin
[0047] (1) Pretreatment: The 19 m / m silk stretch satin scouring blank fabric was rolled up on the warp beam for rescouring, and the fabric was scouted at 90°C for 40 min using 2 g / L rapid scouring agent (Miltopan SE), and then dried at 120°C for 1 min in a setting machine;
[0048] (2) Ingredients: Add 3 kg of antistatic finishing agent (TANASTATWP) to 100 L of water and stir evenly, then add 6 kg of moisture absorbing quick-drying agent (Transtex 6220) and stir evenly to prepare a finishing liquid, and add the prepared finishing liquid into the rolling tank;
[0049] (3) Padding: The roller pressure is set to 3 kg, and the fabric is padded once with the finishing liquid, with a liquid rate of about 80%. The padded fabric is then baked on a setting machine at 120°C for 100 seconds to obtain a finished fabric.
[0050] Example 4
[0051] Fabric: 16m / m silk crepe satin
[0052] (1) Pretreatment: The 16 m / m silk crepe satin scouring white embryo fabric was rolled up on the warp beam for rescouring, and the fabric was scouted at 90 °C for 40 min using 2 g / L rapid scouring agent (Miltopan SE), and then dried at 120 °C for 1 min in a setting machine;
[0053] (2) Ingredients: Add 2 kg of antistatic finishing agent (TANASTAT WP) to 100 L of water and stir evenly, then add 6 kg of moisture absorbing quick-drying agent (Transtex 6220) and stir evenly to prepare a finishing solution, and add the prepared finishing solution into the rolling tank;
[0054] (3) Padding: The roller pressure is set to 3 kg, and the fabric is padded once with the finishing liquid, with a liquid rate of about 80%. The padded fabric is then baked on a setting machine at 120°C for 100 seconds to obtain a finished fabric.
[0055] Example 5
[0056] Fabric: 16m / m silk crepe satin
[0057] (1) Pretreatment: The 16 m / m silk crepe satin scouring white embryo fabric was rolled up on the warp beam for rescouring, and the fabric was scouted at 90°C for 40 min using 2 g / L rapid scouring agent (Miltopan SE), and then dried in a setting machine;
[0058] (2) Ingredients: Add 3 kg of antistatic finishing agent (TANASTAT WP) to 100 L of water and stir evenly, then add 3 kg of moisture absorbing quick-drying agent (Transtex 6220) and stir evenly to prepare a finishing solution, and add the prepared finishing solution into the rolling tank;
[0059] (3) Padding: The roller pressure is set to 3 kg, and the fabric is padded once with the finishing liquid, with a liquid rate of about 80%. The padded fabric is then baked on a setting machine at 120°C for 100 seconds to obtain a finished fabric.
[0060] Comparative Example 1
[0061] Fabric: 16m / m silk crepe satin
[0062] (1) Pretreatment: The 16 m / m silk crepe satin scouring white embryo fabric was rolled up on the warp beam for rescouring, and the fabric was scouted at 90 °C for 40 min using 2 g / L rapid scouring agent (Miltopan SE), and then dried at 120 °C for 1 min in a setting machine;
[0063] (2) Ingredients: Add 0.7 kg of antistatic finishing agent (TANASTAT WP) to 100 L of water and stir evenly, then add 1.4 kg of moisture absorbing quick-drying agent (Transtex 6220) and stir evenly to prepare a finishing solution, and add the prepared finishing solution into the rolling tank;
[0064] (3) Padding: The roller pressure is set to 3 kg, and the fabric is padded once with the finishing liquid, with a liquid rate of about 80%. The padded fabric is then baked on a setting machine at 120°C for 100 seconds to obtain a finished fabric.
[0065] Comparative Example 2
[0066] Fabric: 16m / m silk crepe satin
[0067] (1) Pretreatment: The 16 m / m silk crepe satin scouring white embryo fabric was rolled up on the warp beam for rescouring, and the fabric was scouted at 90 °C for 40 min using 2 g / L rapid scouring agent (Miltopan SE), and then dried at 120 °C for 1 min in a setting machine;
[0068] (2) Ingredients: Add 3.5 kg of antistatic finishing agent (TANASTAT WP) to 100 L of water and stir evenly, then add 7 kg of moisture absorbing quick-drying agent (Transtex 6220) and stir evenly to prepare a finishing liquid, and add the prepared finishing liquid into the rolling tank;
[0069] (3) Padding: The roller pressure is set to 3 kg, and the fabric is padded once with the finishing liquid, with a liquid rate of about 80%. The padded fabric is then baked on a setting machine at 120°C for 100 seconds to obtain a finished fabric.
[0070] Comparative Example 3
[0071] Fabric: 16m / m silk crepe satin
[0072] (1) Pretreatment: The 16 m / m silk crepe satin scouring white embryo fabric was rolled up on the warp beam for rescouring, and the fabric was scouted at 90 °C for 40 min using 2 g / L rapid scouring agent (Miltopan SE), and then dried at 120 °C for 1 min in a setting machine;
[0073] (2) Ingredients: Add 6 kg of antistatic finishing agent (TANASTAT WP) to 100 L of water, stir evenly to prepare a finishing solution, and add the prepared finishing solution into the rolling tank;
[0074] (3) Padding: The roller pressure is set to 3 kg, and the fabric is padded once with the finishing liquid, with a liquid rate of about 80%. The padded fabric is then baked on a setting machine at 120°C for 100 seconds to obtain a finished fabric.
[0075] Comparative Example 4
[0076] Fabric: 16m / m silk crepe satin
[0077] (1) Pretreatment: The 16 m / m silk crepe satin scouring white embryo fabric was rolled up on the warp beam for rescouring, and the fabric was scouted at 90 °C for 40 min using 2 g / L rapid scouring agent (Miltopan SE), and then dried at 120 °C for 1 min in a setting machine;
[0078] (2) Ingredients: Add 6 kg of moisture absorbing quick-drying agent (Transtex 6220) to 100 L of water, stir evenly to prepare a finishing liquid, and add the prepared finishing liquid into the rolling tank;
[0079] (3) Padding: The roller pressure is set to 3 kg, and the fabric is padded once with the finishing liquid, with a liquid rate of about 80%. The padded fabric is then baked on a setting machine at 120°C for 100 seconds to obtain a finished fabric.
[0080] Comparative Example 5
[0081] Fabric: 16m / m silk crepe satin
[0082] (1) Pretreatment: The 16 m / m silk crepe satin scouring white embryo fabric was rolled up on the warp beam for rescouring, and the fabric was scouted at 90 °C for 40 min using 2 g / L rapid scouring agent (Miltopan SE), and then dried at 120 °C for 1 min in a setting machine;
[0083] (2) Padding: The fabric is padded once with clean water, with a liquid rate of about 80%. The padded fabric is then baked on a setting machine at 120°C for 100s to obtain a finished fabric.
[0084] The surface resistance and water drop diffusion time of the fabrics in Examples 1-5 and Comparative Examples 1-5 were tested before and after finishing. The surface resistance test process of the fabric surface was based on the test standard GBT 12703.4-2010 Evaluation of electrostatic properties of textiles Part 4: Resistivity, and the water drop diffusion time test process was based on the test standard GBT 21655.1-2008 Evaluation of moisture absorption and quick-drying properties of textiles Part 1. The specific data are shown in Tables 1 and 2.
[0085] Table 1 Surface resistance test results
[0086]
[0087] Table 2 Water drop diffusion time test results
[0088]
[0089]
[0090] It can be seen from the test results in Table 1 and Table 2 that the present invention selects a hydrophilic polyether polyurethane compound as a moisture absorbing and quick-drying agent, and selects a cationic alkoxyamine compound as an antistatic finishing agent. The two additives are used in a quantitative ratio, and the two cooperate to form a hydrophilic mesh electrostatic shielding layer on the fabric, accelerate the dissipation of the surface charge of the fabric, thereby enhancing the antistatic performance of the fabric, and achieving durable antistatic performance. The water diffusion time of the mulberry silk fabric after shaping and finishing is within 5s, and the specific resistance is less than 10 11 Ω, after 10 machine washes, the fabric water diffusion time is within 5s, the specific resistance is less than 10 12 Ω.
[0091] In Examples 1-3, the dosage ratio of the antistatic finishing agent to the moisture absorbing and quick-drying agent in the finishing liquid is 1:2. The surface resistance of the mulberry silk fabric after shaping and finishing is low, and it has excellent antistatic performance. Moreover, after multiple washings, the surface resistance of the fabric does not change much, and it has excellent machine washability and durable antistatic performance. In Example 4, the dosage ratio of the antistatic finishing agent to the moisture absorbing and quick-drying agent in the finishing liquid is 1:3, and in Example 5, the dosage ratio of the antistatic finishing agent to the moisture absorbing and quick-drying agent in the finishing liquid is 1:1. Although the mulberry silk fabrics after shaping and finishing in Examples 4 and 5 have good antistatic performance, their water washing resistance is poor. After multiple washings, the surface resistance of the mulberry silk fabric increases significantly. It shows that the dosage ratio of the antistatic finishing agent to the moisture absorbing and quick-drying agent in the finishing liquid is 1:2, and the mulberry silk fabric after shaping and finishing has better machine washability and more excellent durable antistatic performance.
[0092] When the content of the antistatic finishing agent and the moisture absorbing quick-drying agent in the finishing liquid in the comparative example 1 system is too low, the antistatic performance of the mulberry silk fabric after the shaping finishing is poor, and the durability is poor and it is not resistant to water washing.
[0093] When the content of the antistatic finishing agent and the hygroscopic quick-drying agent in the finishing liquid in the comparative example 2 system is too high, the mulberry silk fabric after the shaping finishing has excellent durable antistatic properties and good machine wash resistance. However, due to the excessive addition of the antistatic finishing agent and the hygroscopic quick-drying agent, on the one hand, the overall cost is high, and on the other hand, it will affect the performance of the mulberry silk fabric. The mulberry silk fabric treated with the finishing liquid feels greasy and has poor splitting resistance.
[0094] It can be seen from Comparative Example 5 that without antistatic treatment (no antistatic finishing and moisture absorbing quick-drying agent is added to the system), the specific resistance of the fabric is greater than 10 12 Ω, the drip diffusion time is always higher than 5s.
[0095] It can be seen from Comparative Example 3 that only antistatic finishing agent is added to the system, and the drip diffusion time of the mulberry silk fabric after styling finishing is 6s, and the specific resistivity is 2*10 8 , but the washing resistance is poor, and the washing resistance is much lower than the performance of the mulberry silk fabric after the shaping and finishing in Examples 1-5 of the present invention. It can be seen from Comparative Example 4 that only the moisture absorption and quick-drying agent is added to the system, and the drip diffusion time of the mulberry silk fabric after the shaping and finishing is 0.9s, but the antistatic performance is poor, and the specific resistivity of the treated sample is 2*10 10 , after washing 10 times, the specific resistance is greater than 10 12 Ω, which shows that the moisture absorbing and quick-drying agent improves the drip diffusion time and the washing resistance. The moisture absorbing and quick-drying agent in the present invention cooperates with the antistatic finishing agent to achieve a durable and excellent antistatic effect.
[0096] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A machine washable durable antistatic mulberry silk fabric, characterized in that: The mulberry silk fabric is immersed or rolled into the finishing liquid to form a hydrophilic mesh electrostatic shielding layer on the surface; The finishing liquid comprises an antistatic finishing agent and a moisture absorbing and quick-drying agent, wherein the antistatic finishing agent is a cationic alkoxyamine compound, and the moisture absorbing and quick-drying agent is a polyether polyurethane compound.
2. The machine washable durable antistatic mulberry silk fabric according to claim 1, characterized in that: The concentration of the antistatic finishing agent in the finishing liquid is 10-30 g / L, and the concentration of the moisture absorbing quick-drying agent is 20-60 g / L.
3. The machine washable durable antistatic mulberry silk fabric according to claim 2, characterized in that: The dosage ratio of the antistatic finishing agent to the moisture absorbing quick-drying agent in the finishing liquid is 1:
2.
4. The machine washable durable antistatic mulberry silk fabric according to claim 1, characterized in that: The mulberry silk fabric is not dyed, and after being dipped into a finishing liquid, the mulberry silk fabric is baked and shaped at 120-130°C.
5. The machine washable durable antistatic mulberry silk fabric according to claim 4, characterized in that: Before the mulberry silk fabric is treated with the finishing liquid, it is re-scouted with a rapid refining agent, wherein the rapid refining agent is a compound of a buffer alkali and a non-ionic surfactant.
6. A machine washable durable antistatic finishing process for mulberry silk fabric, characterized in that: The steps include: S1. Re-scouring the undyed silk fabric with a rapid scouring agent; S2, mixing an antistatic finishing agent, a moisture absorbing quick-drying agent and water to form a finishing liquid, wherein the concentration of the antistatic finishing agent in the finishing liquid is 10-30 g / L, and the concentration of the moisture absorbing quick-drying agent is 20-60 g / L; S3, applying the finishing liquid to the mulberry silk fabric after the re-scouring treatment by dipping or padding; S4, the mulberry silk fabric after the dipping or padding treatment is baked and set by a setting machine, the baking temperature is 120-130° C., and the baking time is 90-110 seconds.
7. The machine washable durable antistatic finishing process for mulberry silk fabric according to claim 6, characterized in that: The antistatic finishing agent is a cationic alkoxyamine compound, and the moisture absorbing and quick-drying agent is a polyether polyurethane compound.
8. The machine washable durable antistatic finishing process for mulberry silk fabric according to claim 6, characterized in that: The rapid refining agent is a compound of a buffer alkali and a nonionic surfactant.