Cotton fiber coupling enzyme synergistic green pretreatment process
Through the combination of coupling enzymes and high-efficiency surfactants, the use of low-temperature and low-alkali synergistic process, the problems of high energy consumption and large wastewater in the traditional cotton fiber pretreatment process are solved, and efficient cotton fiber pretreatment is achieved, improving the The whiteness and softness of the product have significant economic and environmental benefits.
Patent Information
- Application Number
- CN202411321352.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-23
- Publication Date
- 2024-11-08
AI Technical Summary
The traditional cotton fiber pretreatment process has problems such as many types of materials, large usage, high energy consumption, long time consumption, large water consumption, large sewage, low production efficiency, yellowing, uneven whiteness, and astringent and hard feel of the hand.
Coupling enzymes, high-efficiency surfactants and chelating dispersants are used in combination. Through the coupling synergistic process of low-temperature and low-alkali, the cotton seed shell and wax in cotton fibers are degraded, and the green pretreatment of cotton fibers is carried out, including heating, insulation, and water washing. And neutralization steps, use KA-BiO green pretreatment agent and materials such as water, caustic soda, hydrogen peroxide.
It has achieved low temperature and low alkali green processing, energy saving and consumption reduction, water use, improved production efficiency and product whiteness and softness, reduced sewage treatment costs, and has significant economic, social and environmental benefits.
Smart Images

Figure CN118910894A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of fiber processing, and in particular relates to a cotton fiber coupled enzyme coordinated green pretreatment process. Background Art
[0002] In recent years, various products such as spunlace nonwoven fabrics, gauze, and loose fibers based on cotton fibers have been increasingly widely used, and their consumer market is huge. In particular, cotton fiber nonwoven fabrics are widely used in many fields due to their wide application fields, short production process, and low comprehensive cost. All-cotton spunlace nonwoven fabrics are made of natural fiber pure cotton. After opening and loosening the cotton, the cotton fibers are arranged into a net using a carding machine, a web laying machine, and a drafting machine. The high-density needle-shaped water columns formed after pressure are used to promote the entanglement of cotton fibers into cloth through a spunlace machine. It only takes 5 minutes from raw cotton to finished cloth, which saves spinning, weaving and other links compared to traditional woven fabrics, shortens working hours, saves a lot of energy consumption, labor and equipment, is low-carbon and environmentally friendly, saves energy and emissions, and reduces costs by about 30%. Its process has the world's advanced level of cloth technology. The process of all-cotton spunlace nonwoven fabrics meets the strategic requirements of "low-carbon environmental protection, energy conservation and emission reduction, and green development to promote green consumption models" proposed by the national plan.
[0003] my country is a major cotton producer and consumer. The production of nonwoven fabrics has grown rapidly, and China has become the world's largest producer and consumer of nonwoven fabrics. With the changes in the raw materials of nonwoven fabrics and the advancement of technology, cotton spunlace nonwoven fabrics have emerged as the industry has developed rapidly, as wood pulp and man-made fibers are subject to environmental protection constraints and national industrial policy restrictions.
[0004] The downstream applications of cotton fiber non-woven fabrics in my country are mainly medical and health care, household goods, clothing, daily sanitation products (such as baby diapers, adult incontinence products and female hygiene products, etc.), wiping cleaning materials, packaging materials, filter materials, automotive interiors, environmental protection, etc. In particular, in the medical and health fields, the demand for non-woven fabrics continues to grow, such as medical non-woven fabrics and wet wipes. In the future, with the improvement of people's living standards and the change of consumption concepts, the market demand for cotton fiber non-woven fabrics, gauze and loose fibers will continue to maintain a high growth trend. With the continuous innovation and progress of science and technology, new products will continue to emerge, further promoting the expansion of the market scale. The industry will pay more attention to the research and development and innovation of materials to meet the special requirements of different fields. For example, by improving the pre-treatment production process of cotton fiber non-woven fabrics, gauze and loose fibers, energy conservation and emission reduction, green environmental protection, improved production efficiency and product quality, and reduced production costs can be achieved.
[0005] In terms of technology, the green pre-treatment technology in the field of cotton fiber is relatively backward. The materials required for the traditional pre-treatment process are scouring agents, penetrants, hydrogen peroxide oxygen bleaching stabilizers, chelating dispersants, hydrogen peroxide, caustic soda, neutralizers, etc. There are many varieties, large dosages, high surface activity, high energy consumption, long time, high water consumption, large amount of sewage, low production efficiency, and yellowing, uneven whiteness, and hard feel of the products after pre-treatment. Summary of the invention
[0006] In view of the deficiencies in the above-mentioned prior art, the present invention provides a green pretreatment process for cotton fiber coupled enzyme synergistically. The present invention utilizes the synergistic function of coupling enzymes, high-efficiency surfactants, and chelating dispersants to swell, degrade, and remove cottonseed hulls and wax in cotton fibers, and uses low-temperature and low-alkali coupling to synergistically complete the pretreatment process of cotton fibers, effectively solving the problems of traditional pretreatment processes such as the use of a variety of materials, large amounts, high surface activity, high energy consumption, long time consumption, high water consumption, large amounts of sewage, low production efficiency, and yellowing, uneven whiteness, and astringent feel of products after pretreatment. The method of the present invention can be widely used in green pretreatment processes for spunlace nonwovens, gauze, and loose fibers with cotton fibers as the substrate, and has significant economic, social, and environmental benefits.
[0007] The cotton fiber coupled enzyme synergistic green pretreatment process of the present invention comprises the following steps:
[0008] S1. Cotton fiber entering the tank: add cotton fiber into the pre-treatment tank and pump in a certain amount of water;
[0009] S2. Feeding: At room temperature, pump KA-BiO green pretreatment agent aqueous solution into the cylinder, heat it at a rate of 2°C / min, heat it to 50-60°C, keep it warm for 30-40min, pump caustic soda aqueous solution into the cylinder, circulate it for 5-10min, and then pump hydrogen peroxide solution into the cylinder. After these three materials are added and run evenly in the cylinder, they are the green pretreatment working solution;
[0010] S3, heating and heat preservation treatment: heating at a rate of 2°C / min, heating to 90-95°C and then keeping warm for 60-80min;
[0011] S4, water washing: drain the working fluid, pump 50-60℃ hot water into the tank for washing for 15-20min, drain the hot water, pump in normal temperature water for washing for 10-15min, drain the water, and further remove the residual impurities, etc.;
[0012] S5, neutralization: after the cotton fiber is washed with water, a citric acid aqueous solution is pumped into the tank for neutralization for 10-15 minutes, and when the pH of the neutralized solution is 6-8, the neutralized solution is discharged;
[0013] S6, out of the vat: remove the neutralized cotton fibers from the vat for dehydration, drying and other subsequent processes.
[0014] Furthermore, the green pretreatment working solution is composed of water, KA-BiO green pretreatment agent, 99% by mass of flake caustic soda and 27.5% by mass of hydrogen peroxide.
[0015] Among them, the amount of water added is 800.0%-1000.0% (owf) of the weight of the cotton fiber, that is, the amount of water added is 8-10 times the weight of the cotton fiber; the amount of KA-BiO green pretreatment agent added is 2.0%-3.0% (owf) of the weight of the cotton fiber; the amount of 99% flake caustic soda added is 1.5%-2.5% (owf) of the weight of the cotton fiber; the amount of 27.5% hydrogen peroxide added is 8.0%-12.0% (owf) of the weight of the cotton fiber.
[0016] Furthermore, the specific preparation method of the green pretreatment working solution is as follows: first, add KA-BiO green pretreatment agent at room temperature, heat it to 50°C at a heating rate of 2°C / min, and the main pump circulates for 30-40 minutes, then add flake caustic soda, circulate for 5-10 minutes, add hydrogen peroxide, and then heat it to 90-95°C at a heating rate of 2°C / min, and keep it in a circulating state for 60-80 minutes; in the above process, add water in batches, and the green pretreatment working solution is obtained after the above materials are added and run evenly in the cylinder.
[0017] The raw materials of the KA-BiO green pretreatment agent are composed of the following by weight percentage: 3-6% alkaline pectinase, 2-4% alkaline ligninase, 1-3% cutinase, 10-15% alkyl polysaccharide, 10-15% fatty alcohol polyoxyethylene ether, 5-8% polyacrylate, 5-8% gluconate, and the balance is water.
[0018] The preparation method of the KA-BiO green pretreatment agent comprises the following steps:
[0019] ① First, slowly add alkaline pectinase, alkaline ligninase and cutinase into water respectively, stirring at a speed of 60-100 rpm. After 30-40 minutes, add the mixture completely, stir for another 10-15 minutes, stop the machine, and let it stand for use;
[0020] ②Add fatty alcohol polyoxyethylene ether and polyacrylate to alkyl polysaccharide respectively, stirring at a speed of 60-100 rpm. Add after 10-20 minutes, stir for another 5-10 minutes, stop the machine, and let it stand for use;
[0021] ③ Slowly add the prepared materials in step ② to the prepared materials in step ①, stirring while adding, with a stirring speed of 60-100 rpm. After 30-40 minutes, add the materials, stir for another 5-10 minutes, stop the machine, and let it stand for use;
[0022] ④ Slowly add gluconate to the prepared preparation in ③ above, stirring at a speed of 60-100 rpm, add after 20-30 minutes, stir for 5-10 minutes, stop, let stand for 40-60 minutes, filter with a 100-mesh nylon net, discharge and package to obtain KA-BiO green pretreatment agent.
[0023] Alkaline pectinase has a good effect on removing cotton fiber colloids, and has little damage to natural cellulose fibers, which can make the fibers have good physical properties. Compared with traditional high-temperature and high-alkali pretreatment, it has the advantages of protecting fibers, improving refining efficiency, and reducing energy consumption and pollution.
[0024] Alkaline ligninase can degrade xylan into oligosaccharides and xylose under alkaline conditions.
[0025] Cutinase can hydrolyze the cuticle and improve the wettability of cotton fiber. It has a good synergistic effect with pectinase, which is beneficial to maintaining the good physical properties of cotton fiber. It can catalyze the hydrolysis of the ester bonds of insoluble polymer plant cutin, and can also act on other long-chain and short-chain fatty acid esters and soluble synthetic esters. The combined use of cutinase and enzyme preparations such as alkaline pectinase and alkaline ligninase can realize the green pre-treatment of cotton fiber and reduce pollution to the environment.
[0026] Alkyl polyglycosides have low surface tension, no cloud point, strong wetting power, strong detergency, and good compatibility. They can be compounded with various ionic and non-ionic surfactants to produce a synergistic effect. They have good foaming properties, are resistant to alkalis and electrolytes, and significantly improve the mildness of the formula. They are non-toxic, non-irritating, and easily biodegradable, thereby reducing wastewater discharge in the cotton fiber pretreatment process. They are widely used in the cotton fiber pretreatment process, which contributes to environmentally friendly and clean production.
[0027] Fatty alcohol polyoxyethylene ether is a non-ionic surfactant with good emulsification, wetting, penetration, washing, decontamination and dispersion effects.
[0028] Polyacrylate has good chelating dispersibility and good scale inhibition effect. It can form chelates with scale-forming ions in medium-hardness water and flow with the water, and can prevent the formation of iron oxide scale. In the cotton fiber pretreatment process, it can significantly improve water quality and increase the whiteness of cotton fibers.
[0029] Gluconate has excellent chelating and dispersing, corrosion and scale inhibition, water quality stabilization, washing and decontamination, hydrogen peroxide stabilization, obvious coordination effect, strong scale inhibition ability, and strong complexing ability for calcium, magnesium, and iron salts, especially for Fe 3+ It has excellent chelating effect and works in the whole pH range. It has a mild and stable decomposition effect on hydrogen peroxide in the pre-treatment working liquid system, is environmentally friendly and pollution-free, and is conducive to the green processing of cotton fiber pre-treatment.
[0030] Beneficial effects of the present invention:
[0031] The present invention adopts a green pretreatment process to achieve low-temperature and low-alkali green processing, energy saving and consumption reduction, reduce water use, reduce sewage treatment costs, improve production efficiency, improve the quality and output rate of cotton fibers after treatment, and obtain excellent whiteness and softness. The green pretreatment process has the advantages of simple operation, easy control, stable quality, etc. The present invention can be widely used in green pretreatment processes of spunlace nonwoven fabrics, gauze, and loose fibers with cotton fibers as the base material, and its application has significant economic, social and environmental benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 This is a comparison between the green pretreatment process of the present invention and the traditional process route. DETAILED DESCRIPTION
[0033] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] Example 1: Preparation of KA-BiO green pretreatment agent
[0035] The weight percentages of the raw materials of the KA-BiO green pretreatment agent are: 3-6% alkaline pectinase, 2-4% alkaline ligninase, 1-3% cutinase, 10-15% alkyl polysaccharide, 10-15% fatty alcohol polyoxyethylene ether, 5-8% polyacrylate, 5-8% gluconate, and the balance is water.
[0036] The preparation method of the KA-BiO green pretreatment agent comprises the following steps:
[0037] ① First, slowly add alkaline pectinase, alkaline ligninase and cutinase into water respectively, stirring at a speed of 60-100 rpm. After 30-40 minutes, add the mixture completely, stir for another 10-15 minutes, stop the machine, and let it stand for use;
[0038] ②Add fatty alcohol polyoxyethylene ether and polyacrylate to alkyl polysaccharide respectively, stirring at a speed of 60-100 rpm. Add after 10-20 minutes, stir for another 5-10 minutes, stop the machine, and let it stand for use;
[0039] ③ Slowly add the prepared materials in step ② to the prepared materials in step ①, stirring while adding, with a stirring speed of 60-100 rpm. After 30-40 minutes, add the materials, stir for another 5-10 minutes, stop the machine, and let it stand for use;
[0040] ④ Slowly add gluconate to the prepared preparation in ③ above, stirring at a speed of 60-100 rpm, add after 20-30 minutes, stir for 5-10 minutes, stop, let stand for 40-60 minutes, filter with a 100-mesh nylon net, discharge and package to obtain KA-BiO green pretreatment agent.
[0041] The KA-BiO green pretreatment agent is a product that has been strictly tested and passed by an international ecological certification agency and has obtained the ECO PASSPORT Authorization to use Label, KA-BiO green pretreatment agent is used for the production of human ecologically optimized textiles. Textiles processed with this product will not cause harmful effects on humans and the environment, and can fully meet the needs of medical, sanitary, nursing and other fields.
[0042] KA-BiO green pretreatment agent product parameters:
[0043] Product name: KA-BiO green pretreatment agent; Model: KA-BiO; Manufacturer: Hefei Dongfang Meijie Molecular Materials Technology Co., Ltd.
[0044] Embodiment 2:
[0045] A cotton fiber coupled enzyme synergistic green pretreatment process, specifically comprising the following steps:
[0046] S1, cotton fiber non-woven fabric into the cylinder: 1800kg specification of 35g / m 2 Double-sided plain cotton fiber non-woven fabric is added into a special pre-treatment tank, the special pre-treatment equipment is manufactured by Lixin Dyeing and Finishing Machinery (Shenzhen) Co., Ltd., name: dye tank;
[0047] S2. Feeding: The green pretreatment working solution is composed of KA-BiO green pretreatment agent, 99% flake caustic soda by mass, 27.5% hydrogen peroxide and water; the specific preparation method is: first, add 14400kg of quantitative water at room temperature, add 45kg of KA-BiO green pretreatment agent, heat to 50℃ at a heating rate of 2℃ / min, and the main pump circulates for 30-40min, then add 36kg of 99% flake caustic soda by mass, circulate for 5-10min, and then add 180kg of 27.5% hydrogen peroxide by mass. After the above three materials are added and run evenly in the cylinder, they are the green pretreatment working solution.
[0048] S3, heating and heat preservation treatment: heating at a heating rate of 2°C / min, heating to 90°C, and then heat preservation for 80 minutes to perform green pretreatment of the cotton fiber non-woven fabric;
[0049] S4, water washing: after the green pretreatment is completed, the working liquid is discharged, and 50°C hot water is pumped into the tank for washing for 15 minutes. After the hot water is discharged, normal temperature water is added for washing for 10 minutes, and the water is drained to further remove residual impurities, etc.;
[0050] S5, neutralization: after the cotton fiber non-woven fabric is washed with water, 3 kg of citric acid aqueous solution is pumped into the tank for neutralization for 10-15 minutes, and when the pH of the neutralized solution is 6-8, the neutralized solution is discharged;
[0051] S6, out of the vat: the neutralized cotton fiber non-woven fabric is removed from the vat and subjected to subsequent processes such as dehydration and drying, so that the degreased and bleached cotton fiber non-woven fabric is obtained.
[0052] Embodiment 3:
[0053] The KA-BiO green pretreatment agent with different formulations was used at 35g / m 2 The double-sided plain cotton fiber non-woven fabric is pre-treated according to the same process, and the formula is shown in the following table:
[0054] Recipe ingredients Solution 1 Solution 2 Solution 3 Solution 4 Solution 5 Solution 6 Solution 7 water 57 58 59 53 54 55 54 Alkaline pectinase 5 - - 5 5 - 4 Alkaline ligninase - 4 - 4 - 4 2 Cutinase - 3 - 3 3 2 Alkyl polysaccharide 12 12 12 12 12 12 12 Fatty alcohol polyoxyethylene ether 14 14 14 14 14 14 14 Polyacrylate 6 6 6 6 6 6 6 Gluconate 6 6 6 6 6 6 6
[0055] The specific application process is as follows: (taking the pre-treatment of cotton fiber non-woven fabric as an example, the amount of water added is 8 times the weight of the cotton fiber)
[0056] Process dosage:
[0057] ①Pretreatment agent 2.0%% (owf)
[0058] ②99%Flake caustic soda 2.0%(owf)
[0059] ③27.5% hydrogen peroxide 10.0% (owf)
[0060] ④Citric acid 0.2% (owf)
[0061] Process flow:
[0062] Preparation→ Cotton fiber non-woven fabric is put into the cylinder→ Add material (pretreatment agent) at room temperature→ Heating (heating rate: 2℃ / min, to 50℃)→ Keep warm (50℃, keep warm for 30min)→ Add material (add flake caustic soda, circulate for 5min and then add hydrogen peroxide)→ Heating (heating rate: 2℃ / min, to 95℃, keep warm for 80min)→ Drainage→ Hot water washing (50℃, 15min)→ Drainage→ Cold water washing (10min)→ Neutralization (add citric acid, 15min)→ Drainage→ Out of the cylinder.
[0063] Test items Solution 1 Solution 2 Solution 3 Solution 4 Solution 5 Solution 6 Solution 7 Whiteness YY0331-2002 81 79 75 82 80 79 87 Water absorption speed (mm) 78 73 71 83 80 78 92 Feel Hard Hard Hard Softer Softer Softer soft
[0064] Conclusion: The above data show that the application effect (whiteness, water absorption rate) of Scheme 7 is better than that of other schemes. The effective combination of biological enzyme preparations such as alkaline pectinase, alkaline ligninase and cutinase, and the combination with high-efficiency surfactants and chelating dispersants have obvious synergistic enhancement functions.
[0065] Comparative Example:
[0066] Comparison between green pretreatment technology and traditional pretreatment technology for cotton fiber nonwoven fabrics
[0067] (1) Comparison of green pretreatment process and traditional process material formula (taking 1800kg / cylinder as an example)
[0068]
[0069] It can be seen from the table above that the traditional pre-treatment material combination has seven materials: scouring agent, penetrant, chelating dispersant, oxygen bleaching stabilizer, 99% flake caustic soda, 27.5% hydrogen peroxide, and citric acid, while the green pre-treatment process application materials of the present invention only have four materials: KA-BiO green pre-treatment agent, 99% flake caustic soda, 27.5% hydrogen peroxide, and citric acid; the amount of materials used is greatly reduced, and the labor intensity is significantly reduced. At the same time, KA-BiO green pre-treatment agent obviously has special functions, which is to intensively coordinate the functions of bio-enzyme catalysis, scouring, penetration, emulsification, chelation, dispersion, oxidation stabilization, and cleaning, and combine them into one to synergize and enhance the efficiency, which not only reduces the variety and amount of feed, but also can obtain good green pre-treatment effects; KA-BiO green pre-treatment agent is a product that has been strictly tested and passed by international ecological certification agencies and has obtained ECOPASSPORT by Authorization to use Label, used for the production of human ecologically optimized textiles. Textiles processed with this product will not cause harmful effects on humans and the environment, and can fully meet the needs of medical, hygiene, nursing and other fields.
[0070] (2) Comparison between green pretreatment process and traditional process (taking 1800kg / cylinder as an example)
[0071]
[0072] From the above comparison, we can see that the traditional process adopts a two-step method, which is time-consuming, while the green pre-treatment process adopts a one-step method, which is time-saving, saves more than 40% of water, electricity and steam, and increases production efficiency by about 50%. The green pre-treatment process obviously reduces energy consumption, saves energy and water.
[0073] (3) Comparison of the application effects of green pretreatment technology and traditional technology (taking 1800kg / cylinder as an example)
[0074]
[0075]
[0076] It can be seen from the above table that the various test indicators of the cotton fiber non-woven fabric processed by the green pre-treatment process are higher than those of the traditional process. In particular, the present invention adopts "low temperature and low alkali, coupled synergy" to complete the pre-treatment process. The non-woven fabric after treatment has a noticeably soft feel and meets consumer demand.
[0077] (4) Cost comparison between traditional process and green pretreatment process (taking 1800kg / cylinder as an example)
[0078]
[0079]
[0080] From the table above, we can see that the material cost per cylinder of the green pretreatment process is reduced by 22.5% compared with the traditional process. The application of the green pretreatment process has significant economic benefits.
[0081] (5) Comparison of water consumption between traditional process and green pretreatment process (taking 1800kg / tank as an example)
[0082] Type: 35g / m 2 Double-sided plain cotton fiber non-woven fabric, weight: 1.8 tons.
[0083] Traditional crafts Green pre-treatment process Equipment size <![CDATA[15m 3 ]]> <![CDATA[15m 3 ]]> Drainage times 7 4 Water consumption per tank <![CDATA[Approximately 90m 3 > <![CDATA[Approximately 50m 3 >
[0084] From the table above, we can see that the water consumption per cylinder of the green pretreatment process is reduced by 44% compared with the traditional process, which reduces the burden of sewage treatment and reduces the cost of sewage treatment. The green pretreatment process has significant social and environmental benefits.
[0085] (6) Comparison of the reduction rate between green pretreatment process and traditional process (taking 1800kg / cylinder as an example)
[0086]
[0087] It can be seen from the above table that the green pre-treatment process adopts "low temperature and low alkali, coupled synergy" to complete the pre-treatment process. The treated non-woven fabric retains some beneficial cotton wax and fat in the cotton fiber while meeting the hydrophilicity, so that the non-woven fabric has an excellent soft feel. At the same time, it effectively reduces the reduction rate and increases the output rate by about 3.5%.
[0088] In summary, the cotton fiber coupled enzyme synergistic green pretreatment process screens and effectively combines the characteristics of biological enzyme preparations to obtain efficient coupled enzyme preparations suitable for the cotton fiber green pretreatment process, and combines with efficient surfactants and chelating dispersants to utilize their synergistic enhancement functions to swell, degrade and remove cottonseed hulls and wax in cotton fibers. The pretreatment process of cotton fibers is completed by "low temperature and low alkali, coupled synergy", realizing low temperature and low alkali green processing, energy saving and consumption reduction, reducing water use, reducing sewage treatment costs, improving production efficiency, and improving the quality and output rate of cotton fibers after treatment, and can obtain excellent whiteness, strength and softness. The green pretreatment process has the advantages of simple operation, easy control, stable quality, etc. The present invention can be widely used in green pretreatment processes of spunlace non-woven fabrics, gauze, and loose fibers with cotton fibers as the base material, and its application has significant economic benefits, social benefits and environmental benefits.
[0089] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.
Claims
1. A cotton fiber coupled enzyme synergistic green pretreatment process, characterized in that The following steps are involved: S1. Cotton fiber entering the tank: add cotton fiber into the pre-treatment tank and pump in a certain amount of water; S2. Feeding: At room temperature, pump the green pretreatment working solution into the cylinder, and run it evenly in the cylinder after adding; the green pretreatment working solution is composed of water, KA-BiO green pretreatment agent, flake caustic soda and hydrogen peroxide with a mass fraction of 27.5%; S3, heating and heat preservation treatment: heating at a rate of 2°C / min, heating to 90-95°C and then keeping warm for 60-80min; S4, water washing: drain the working fluid, pump 50-60℃ hot water into the tank for 15-20min, drain the hot water, pump in normal temperature water for 10-15min, drain the water, and further remove residual impurities; S5, neutralization: after the cotton fiber is washed with water, a citric acid aqueous solution is pumped into the tank for neutralization for 10-15 minutes, and when the pH of the neutralized solution is 6-8, the neutralized solution is discharged; S6, out of the vat: remove the neutralized cotton fibers from the vat for dehydration, drying and other subsequent processes.
2. The cotton fiber coupled enzyme synergistic green pretreatment process according to claim 1, characterized in that: In the green pretreatment working solution, the addition amount of KA-BiO green pretreatment agent is 2.0%-3.0% of the weight of cotton fiber, the addition amount of flake caustic soda is 1.5%-2.5% of the weight of cotton fiber, and the addition amount of hydrogen peroxide with a mass fraction of 27.5% is 8.0%-12.0% of the weight of cotton fiber.
3. The cotton fiber coupled enzyme synergistic green pretreatment process according to claim 2, characterized in that: The preparation method of the green pretreatment working solution is as follows: first, add KA-BiO green pretreatment agent at room temperature, heat it to 50°C at a heating rate of 2°C / min, and circulate the main pump for 30-40min, then add flake caustic soda, circulate it for 5-10min, add hydrogen peroxide, then heat it to 90-95°C at a heating rate of 2°C / min, and circulate it for 60-80min; in the above process, add water in batches, and the green pretreatment working solution is obtained after the above materials are added and mixed evenly.
4. The cotton fiber coupled enzyme synergistic green pretreatment process according to claim 1, characterized in that The raw materials of the KA-BiO green pretreatment agent are composed of the following by weight percentage: 3-6% alkaline pectinase, 2-4% alkaline ligninase, 1-3% cutinase, 10-15% alkyl polysaccharide, 10-15% fatty alcohol polyoxyethylene ether, 5-8% polyacrylate, 5-8% gluconate, and the balance is water.
5. The cotton fiber coupled enzyme synergistic green pretreatment process according to claim 4, characterized in that The preparation method of the KA-BiO green pretreatment agent comprises the following steps: ① First, slowly add alkaline pectinase, alkaline ligninase and cutinase into water respectively, stirring at a speed of 60-100 rpm. After 30-40 minutes, add the mixture completely, stir for another 10-15 minutes, stop the machine, and let it stand for use; ②Add fatty alcohol polyoxyethylene ether and polyacrylate to alkyl polysaccharide respectively, stirring at a speed of 60-100 rpm. Add after 10-20 minutes, stir for another 5-10 minutes, stop the machine, and let it stand for use; ③ Slowly add the prepared product in step ② to the prepared product in step ① above, stirring while adding, with a stirring speed of 60-100 rpm. After 30-40 minutes, add the product, stir for another 5-10 minutes, stop the machine, and let it stand for use; ④ Slowly add gluconate to the prepared preparation in ③ above, stirring at a speed of 60-100 rpm, add after 20-30 minutes, stir for 5-10 minutes, stop, let stand for 40-60 minutes, filter with a 100-mesh nylon net, discharge and package to obtain KA-BiO green pretreatment agent.