Production process of high-strength polyester filament tire base cloth
High-strength polyester filament base fabric is produced through polyester spunbond and needle-punching reinforcement processes, and through glue-impregnation shaping treatment, the problem of insufficient product strength and wear resistance in the existing technology is solved, and high strength, long life and Good heat shrinkage resistance, suitable for the needs of modern waterproof coils.
Patent Information
- Application Number
- CN202410644582.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-23
- Publication Date
- 2024-11-08
AI Technical Summary
In the production process of existing high-strength polyester filament base cloth, the strength, aspect ratio, fracture strength, wear resistance and fatigue resistance of the product are relatively low, which cannot meet the high requirements of modern engineering for the performance of waterproof materials.
The high-strength polyester filament base cloth semi-finished products are produced by polyester spunbond and needle-punching reinforcement, and processed through the glue-impregnation shaping process to finally obtain high-strength polyester filament base cloth product. The specific steps include the polyester slices being crystallized and dried and melted in a screw extruder, forming primary fibers through a single screw extruder with a diamond-shaped pin mixing head, performing airflow drafting and filament distribution mesh, and pre-needle and main Needle-punching reinforcement, cutting and winding, followed by heat setting and glue-soaking and drying.
The tensile strength, top breaking strength and elongation of the filament base cloth are improved. The fracture form is continuous filament breaking, and the elongation is higher than that of short fiber products. It has better resistance to external loads and uniform stress distribution, and its service life is also Longer, physical properties are better than staple fiber products, suitable for the process requirements of waterproof coils.
Smart Images

Figure CN118910896A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of high-strength polyester filament base cloth, in particular to a production process of high-strength polyester filament base cloth. Background Art
[0002] The main application areas of waterproofing membranes include: urban housing construction, high-speed railways, highways and urban roads and bridges, subways and urban rails, airports, water conservancy facilities, ports and docks, nuclear power facilities, sanitation projects, national defense projects, energy and mining projects, etc. Nonwoven fabrics are one of the most important raw materials for the production of modified asphalt membranes.
[0003] Traditional base fabric is made by short fiber combing and needle punching consolidation. The fibers are opened and mixed, combed (or airflow) into a net, laid, drawn and needle punched to form a finished product. The processing technology of short fiber needle punched base fabric has the characteristics of strong adaptability, flexibility and easy to master technology. It has developed rapidly in the early stage of base fabric development. With the advancement of technology and the continuous improvement of the country's requirements for engineering quality, various projects have higher and higher requirements for the performance indicators of waterproof materials. The situation that has been dominated by short fiber needle punched geotextiles has gradually been broken.
[0004] The invention patent with application number: 2010101413465 discloses a production process of polyester filament felt base cloth, including the steps of: pre-crystallization and drying of polyester chips; conveying the pre-crystallization and drying polyester chips to a screw extruder to melt the chips at high temperature; conveying the melted chips to a metering pump to obtain spinning; airflow stretching spinning; needle punching to entangle the spinning together to form a semi-finished cloth; high-temperature shaping of the semi-finished cloth after needle punching; passing the shaped product through a dipping tank, extrusion, high-temperature drying drum drying and rolling. This invention patent directly produces polyester chips as raw materials. Compared with the existing technology, it reduces the process of producing chemical fibers, shortens the process, and reduces production costs and links. However, the strength, aspect ratio, breaking strength, wear resistance, and fatigue resistance of the obtained products are relatively low. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a production process of a high-strength polyester filament tire base cloth to solve the problem raised in the background technology.
[0006] In order to solve the above technical problems, the technical solution of the present invention is: a production process of high-strength polyester filament tire base cloth; first, a high-strength polyester filament tire base cloth semi-finished product is produced by polyester spunbonding and needle punching reinforcement methods, and then it is treated by a dipping and shaping process to finally obtain a high-strength polyester filament tire base cloth product.
[0007] The method specifically comprises the following steps: the polyester chips are crystallized and dried, fed into a screw extruder, passed through a filter and a metering pump and entered into a spinning box, the melt is quantitatively passed through a spinneret to form primary fibers, the filaments after being drawn are separated and swung, and evenly laid on a mesh curtain to form a fiber web, the fiber web is reinforced by pre-needling and main needling, and is cut and rolled to obtain a semi-finished product of a high-strength polyester filament tire base cloth, and the semi-finished product of the high-strength polyester filament tire base cloth is heat-set, dipped in glue, dried and then finished to obtain a finished product of the high-strength polyester filament tire base cloth.
[0008] In the above steps, a single screw extruder with a diamond pin mixing head is used as a tool for the spinning process, and the cooling side blowing of the spinning is set. The side blowing air duct is a tapered type with a guide plate, a damping rectifying layer composed of a porous plate and a stainless steel mesh, so that the longitudinal velocity gradient of the side blowing air is completed to complete the spinning process.
[0009] In the above steps, a tubular drafter is used for drafting, and the drafting rate and the drafting ratio are regulated by increasing the number of drafting tubes and controlling the drafting air flow speed / temperature.
[0010] In the above steps, a reciprocating traverse mechanism is used to perform mechanical wire separation by lateral swinging, and then a web laying machine system is used to lay the web.
[0011] Needle punching reinforcement method is used as the fiber web consolidation method.
[0012] The tubular drafter is a HY-II type drafter.
[0013] The drawing speed of the tractor is 5000-6000m / min.
[0014] The height of the tractor drawing tube is 1000-1200mm, the inner diameter of the tractor drawing tube is 10mm, and the drawing wind pressure is 0.5MPa.
[0015] The swing amplitude of the reciprocating traverse mechanism is 50-54 mm.
[0016] Compared with the prior art, the present invention has the following beneficial effects:
[0017] The present invention adopts polyester filaments to directly lay into a net, and the spinning adopts air flow drawing. Since the air flow drawing is different from the mechanical drawing of conventional chemical fiber spinning, the orientation degree of the polymer is limited, which determines that the filament base cloth has high tensile strength, bursting strength and elongation. From the damage mechanism of the filament base cloth, it is found that the fracture form of the filament base cloth is mainly the fracture of continuous filaments, while the fracture of the staple base cloth is mainly manifested as the destruction of the cloth structure and the slippage of the staple fibers. This also explains why the elongation at break of the filament base cloth is higher than that of similar staple fiber products. Therefore, in practical applications, the linoleum felt with long-line polyester linoleum as the linoleum body has better resistance to external loads, uniform distribution of external stress and deformation resistance, and its service life is also much longer than that of similar staple fiber linoleum felt. In addition, the filament polyester linoleum is composed of uniform and continuous filaments, and the product is uniform, strong and has good heat shrinkage resistance. Its physical properties are better than those of the staple polyester linoleum. After a suitable starch dipping process, it is more suitable for the process requirements of the waterproof coil production line, and its coil has uniform heat shrinkage resistance and longer waterproof durability. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 is a process flow chart of the present invention;
[0019] Figure 2 It is the principle diagram of the drafter of the present invention. DETAILED DESCRIPTION
[0020] The specific embodiments of the present invention are further described below in conjunction with the accompanying drawings. It should be noted that the description of these embodiments is used to help understand the present invention, but does not constitute a limitation of the present invention. In addition, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0021] like Figure 1 As shown, this project firstly utilizes polyester spunbond and needle punching reinforcement methods to produce high-strength polyester filament base cloth (PET) semi-finished products, and then processes them through dipping and shaping to finally obtain high-strength polyester filament base cloth (PET) products.
[0022] From the production process point of view, the production of long-fiber polyester tires reduces the production links such as opening, feeding, and combing compared to short-fiber polyester tires, and has the advantages of stable quality, energy saving and environmental protection.
[0023] The basic production process of polyester spunbond needle punched tire base fabric includes: polyester (PET) chips are crystallized and dried, fed into the screw extruder, and then enter the spinning box through the filter and metering pump. The melt passes through the spinneret to form primary fibers. The filaments after drawing are evenly laid on the mesh curtain to form a fiber net after being divided and swinging. The fiber net is reinforced by pre-needling and main needling, and then cut and rolled to obtain a semi-finished high-strength polyester filament tire base fabric. The semi-finished high-strength polyester filament tire base fabric is finished by heat setting, dipping, drying, etc. to obtain a finished high-strength polyester filament tire base fabric.
[0024] Nowadays, the span of buildings is getting bigger and bigger, and the structural design is getting lighter and lighter, which requires waterproof materials to have sufficient tensile strength, puncture resistance and appropriate elongation to bear the corresponding load. In addition, in some areas, the temperature difference between day and night changes greatly, which requires waterproof materials to be able to adapt to such temperature changes, and have high temperature resistance and flexibility under low temperature conditions. APP and SBS modified asphalts have good adaptability to climate, but they must be matched with high-elongation and high-strength tire base fabrics, otherwise the temperature difference deformation of APP and SBS modified asphalts will cause the tire base to break, affecting the waterproof effect.
[0025] In the production process of high-strength polyester filament base cloth, factors such as the draft ratio of spunbond filaments, fiber uniformity, elongation, web laying uniformity, production stability, environmental protection and economy of dipping will directly affect the final performance of the product and the economic and social benefits of actual production.
[0026] Ensure the strength and elongation of spunbond filaments
[0027] Generally speaking, the performance of spunbond filaments is the most important factor affecting the final performance of tire base fabric products. The physical and mechanical properties of primary fibers are relatively poor. The drafting process makes the filaments gradually thinner, which is the secondary molding of the fibers. The macromolecules in the fibers are oriented along the fiber axis and formed, so that the fiber's breaking strength, wear resistance, fatigue resistance, etc. meet the use requirements. The continuous stability of the spinning process and sufficient drafting are the most important to ensure the quality of the filaments.
[0028] Spinning process
[0029] The spinning technology of polyester spunbond nonwovens is based on polyester filament spinning. The spinning of polyester spunbond nonwovens requires a sufficient number of yarns per unit length in the width direction and a high density. Due to the influence of the circular spinning assembly and tubular drafting process, it is very difficult to obtain the ideal number of yarns and density. Several processes such as spinneret diameter, drafting tube arrangement density, and swinging device design are interrelated and mutually restricted.
[0030] The present invention adopts a single screw extruder with a diamond pin mixing head, a circular top-loading spinning assembly, and a spinneret for each assembly; a box double-die head is adopted, each die head has 72 bundles of silk, and the spinning box adopts a double-sided operation form. The structure in the box has equal diameter melt branch pipes with the same length and curvature, which ensures the fluidity and uniformity of the melt in each pipeline. The design and distribution principle of the melt distribution pipeline is that the flow rate per unit time of each melt pipeline is consistent, and the residence time of the melt in each pipeline is the same: that is, the melt in each part is under the same conditions, experiences the same residence time, and produces the same pressure drop. The spinneret arrangement and spinneret hole design are adjusted accordingly, and the cooling side blowing of spinning is specially designed. The side blowing air duct is a gradually shrinking type, and a damping rectifying layer composed of a guide plate, a porous plate, a stainless steel mesh, etc. is provided inside, which can make the side blowing have a more reasonable longitudinal velocity gradient, which is beneficial to the cooling and solidification effect of the bundle, thereby ensuring the continuous stability of the spinning process. The actual operating parameters are as follows: crystallization temperature: 170°C, drying temperature: 160°C, screw extruder temperature: 270°C, ~296°C, spinning box temperature: 286°C, ~296°C, metering pump specifications: 2.4cc / revx8, 2.4cc / revx4, 2.4cc / revx2, spinneret specifications: medium 65mmx30 holes, number of filament bundles: 72 bundles x2, screw aspect ratio: L / D=25, side blowing wind speed, 0.4~0.7m / s.
[0031] Drafting process
[0032] The present invention adopts a tubular airflow drafting method, which increases the number of drafting tubes and controls the drafting airflow speed / temperature to adjust the drafting rate and drafting ratio, optimize product performance, reduce the drafting air pressure, and reduce energy consumption.
[0033] The principle of the drafter is to use a jet airflow with a higher pressure to attract the induced airflow with a lower pressure and entraining the filament bundle (referred to as the induced airflow). The drafter can be divided into four parts: the jet nozzle, the induced airflow, the mixing section and the drafting section. In gas dynamics, the mixing section is called the initial section, and the drafting section is called the main section. The mixing of the jet airflow and the induced airflow can be divided into two types: equal cross-section mixing and shrinking cross-section mixing. The working principle of the drafter can be seen in Figure 2, the jet gas is ejected from the jet nozzle (slit) at a high speed through the tapered flow channel at a pressure of P1 to the mixing section, the speed increases from V0 to V1, and the pressure drops to P. It can be seen from the Bernoulli equation that when the drafting gas speed increases, the pressure must drop. By selecting appropriate geometric parameters of the drafter structure, a negative pressure can be formed at the nozzle, and the induced airflow entrained with the filament bundle is sucked into the mixing section at a speed of V2. The length of the mixing section is 5 to 8 times its diameter. The jet gas and the induced gas are mixed at the terminal section of the mixing section to exchange energy. The two gases are gradually mixed into a uniform fluid, the speed V3 tends to balance, the pressure rises to P3, and then flows into the drafting section. In the drafting section, the filament bundle is rubbed by the airflow, and the airflow draws the filament bundle to make the filament thinner, and then the gas pressure drops to P4, and the airflow speed becomes V4. Finally, the mixed gas and the stretched filament bundle are ejected from the outlet of the drafter together to complete the drawing process of the filament bundle.
[0034] The tow is subjected to a drafting force due to the friction of the surrounding airflow. According to the principle of chemical fiber spinning, the drafting force formula is:
[0035]
[0036] C=0.37(Re) 0.61
[0037] Re=Vd / v
[0038] V=V3-U0
[0039] Where: CF-friction coefficient,
[0040] Determined by Matsui's empirical formula: v-kinematic viscosity of gas; V3-air flow velocity; U0-spinning speed; d-tow diameter; ρ3-fluid density; Re-Reynolds number; L-drawing section length.
[0041] It can be seen from the formula that the drafting force is proportional to the fluid density, the diameter of the tow, the length of the drafting section, and is also proportional to the square of the speed difference between the airflow and the tow. The flow field in the drafter is characterized by small volume and high turbulence. The airflow speed and direction change at any time in different parts and at different times, which brings great difficulties to theoretical analysis and practical research. But in general, the research direction of the drafter is towards fast spinning speed, low air pressure, and low gas consumption.
[0042] The present invention decomposes and analyzes several tubular drafters, combines theoretical calculations, and conducts a large number of tests, calculations, designs and studies on the geometric parameters of the drafter structure, the characteristics of the airflow field in the drafter, the airflow parameters, the spinning parameters, the forces on the filament bundles, etc., and summarizes the relative change relationship between the different parts, different times, and different airflow speeds in the drafter and the filament bundles; the relationship between the intake pressure and the flow rate of the filament suction port and the air outlet; the relationship between the intake pressure and the pressure of the filament suction port with different slit widths; the relationship between the intake pressure and the inlet and outlet pressure difference with different slit widths; the relationship between the intake pressure and the flow rate with different inlet diameters, etc. The airflow drafter has undergone two upgrades, and the diameter of the drafting tube of the HY-II drafter is further reduced, and the drafting airflow and the drafting bundle can be further concentrated to flow in the center of the air duct, which greatly improves the holding effect of the drafting airflow on the fiber bundle, accelerates the fiber drafting speed, increases the drafting multiple, improves the efficiency, and further reduces the energy consumption. After online verification on the production line, all performance indicators of its products have reached the advanced level of similar foreign products.
[0043] Effect of drawing speed
[0044] In practice, the relationship between the drawing speed and the filament properties was studied by adjusting the drawing pressure (Table 1). It can be seen that with the increase of the drawing speed, the strength of the filament increases and the elongation decreases. This is because during the drawing process, the orientation degree of the macromolecules along the fiber axis increases under the friction of the air flow, thereby increasing the fiber's breaking strength and decreasing the elongation. In practice, considering the energy consumption and performance factors, the fiber drawing speed is determined to be between 5000-6000m / min.
[0045] Table 1 Relationship between drawing speed and filament properties
[0046]
[0047] Table 2 Effect of single hole flow rate change on filament properties
[0048]
[0049] From (Table 2), it can be seen that when the drafting pressure remains unchanged, the single hole flow rate is increased, the single filament fineness is increased, the drafting speed is reduced, the single filament strength is slightly reduced, and the single filament elongation is increased. This shows that within a certain range, the single hole flow rate has little effect on the performance of the single filament. In practice, according to the specific product indicators, the appropriate extrusion volume will be selected and the cooling air and drafting air conditions will be adjusted to achieve the optimal value of production efficiency and product quality.
[0050] Table 3 Effect of drawing head height on filament properties
[0051]
[0052] From the data in (Table 3), we can see that: the influence of the drawing head height on the properties of the filament, when the drawing speed is below 5000m / min, the single filament fineness is higher than the planned value, and when the drawing speed is around 5000m / min, the fineness is close to the set value. In addition, it can be seen that when the drawing head height is 1200mm, the drawing speed required to achieve the planned fineness is smaller than that when the drawing head height is 800mm, that is, when the drawing head height is 1200mm, less air pressure is required to achieve the same drawing speed than when the drawing head height is 800mm.
[0053] The present invention finally adopts 144 drawing tubes, double-row wires with 72 wires in each row, the drawing tube height is 1000-1200mm, the inner diameter of the drawing tube is 10mm, the drawing wind pressure is about 0.5MPa, and the drawing speed is controlled at 5000-6000m / min.
[0054] Ensure the uniformity of wire separation and web laying
[0055] The web forming technology affects the uniformity of the fiber web and is an important process in spunbond nonwoven fabrics. The filaments after spinning and drawing must be separated and laid in a very short time. In addition, the high-speed drawing airflow makes it difficult to evenly separate and lay the filaments after drawing, and it is very important to the quality of the base fabric. Advanced and reasonable separation, laying and suction technology are required. The separation and laying mainly include airflow separation, electrostatic separation, mechanical separation and the like. The present invention adopts a mechanical separation method that can swing horizontally, and selects an advanced linear reciprocating traverse mechanism to replace the traditional arc traverse mechanism, so that the range of the swing frequency and the swing amplitude is greatly improved to meet the needs of producing different products. It has been proved that the use of this technology can improve the weft distribution of the filament fibers in the fiber web during laying, thereby improving the lateral strength of the product and reducing the longitudinal and lateral strength ratio. (Table 4) and (Table 5) show the effects of different swing amplitudes and swing frequencies on the longitudinal and transverse strength ratio of the product in the test. It can be seen that the increase of the swing frequency is beneficial to the longitudinal and transverse strength ratio. The longitudinal and transverse strength is better when the swing amplitude is within the range of 50-54mm.
[0056] Table 4 Effect of swing amplitude on longitudinal and transverse strength ratio
[0057]
[0058] Table 5 Effect of swing frequency on longitudinal and transverse strength ratio
[0059]
[0060] Spunbond web forming technology is the main factor that directly affects the uniformity and production efficiency of spunbond nonwoven products. The uniformity of web laying determines the uniformity of indicators such as weight and strength of the product. There are many factors that affect the uniformity of web laying. In addition to the influence of the filament separation and swinging mentioned in the previous section, it mainly depends on the uniformity of the suction wind speed of the web laying machine system, the stability of the net curtain operation, the technical level of the static elimination system, and the quality of the net curtain itself. The web laying machine consists of a suction area, a suction air duct and an adjustment device, a suction fan, a guide roller, a static eliminator, a frame, a transmission and control system, etc. A good web laying machine can not only lay a uniform fiber web, but also overcome the influence of external airflow, friction static electricity and other factors, and stably deliver the fiber web to the next process at a higher speed without causing the phenomenon of web flipping and fiber web sliding. The higher the speed, the greater the influence of the external airflow on the fiber web, and the higher the static electricity generated by friction. Therefore, the technical level of the web laying machine also affects the production speed and output.
[0061] Selecting the appropriate web consolidation process
[0062] The fiber web consolidation processes commonly used in the spunbond process mainly include needle punching reinforcement, hydroentanglement reinforcement, thermal bonding reinforcement and composite reinforcement. Among them, the thermal bonding reinforcement method has high energy consumption, and has poor reinforcement effect and easy delamination for thick products; the hydroentanglement reinforcement method has high investment cost, high energy consumption, poor reinforcement effect for thick products and other problems; the needle punching reinforcement method has the characteristics of simple process, low cost, good reinforcement effect for thick products, and high production efficiency. At the same time, there are some inherent defects of needle punching reinforcement (such as needle marks on the product, hard feel, and certain loss of fiber strength). For coarser fibers with a monofilament fineness of 3.0 to 6.0 dpf, the situation of the needle punching force breaking the fiber is much smaller than that of fine denier yarns, which is beneficial to improve the strength of the product and increase the air permeability and impregnation performance of the product. Therefore, this project adopts the needle punching reinforcement method as the fiber web consolidation method. Compared with the staple needle punching process, the selection of the needle punching machine is mainly different in the following aspects:
[0063] The structure of the needle loom:
[0064] When using short fibers for needling, the machine can be shut down and started at any time. During the production process, if a large number of broken needles occur, the machine can be stopped at any time to replace the needle plate. However, the spunbond method belongs to continuous production, and the preparation work for starting and shutting down is complicated. The shutdown will cause certain losses to the company's production, but the broken needles and replacement of needle plates of the needle loom are inevitable. At present, the better way is to use a double-axis double-needle plate needle loom, which can realize the replacement of needles without stopping the machine, but the equipment investment is relatively large. From the actual production, balancing the situation of all parties, this project finally chose a double-axis single-needle plate needle loom.
[0065] Needle loom equipment
[0066] When polyester spunbond needle-punched products are used in geotextiles and tarpaulin base fabrics, strength is an important indicator. The strength index, in addition to the performance of the fiber itself, is most importantly affected by the effect of needle punching, including needle structure, needle punching density, needle depth, stepping amount, etc. If the needle punching density is too high, the filament fiber will be severely damaged, resulting in a decrease in its strength; if the needle punching density is too low, the entanglement effect is poor, the product density is poor, the adhesion is not good, and the strength is also reduced. Since the filament needle punching of the spunbond method does not completely rely on the number of needle punches to determine the strength of the product like the staple fiber needle punching, it is not necessary to use more needle punching machines to fully reach and far exceed the quality level of staple fiber needle punching. If too many needle punching machines are used, not only will the product quality not be improved, but it will be reduced. Therefore, when preparing the needle punching production line, the present invention is equipped with a main needle punching machine and a pre-needling machine, and the parameters are shown in (Table 6).
[0067] Table 6 Needle loom parameters
[0068] Pre-needling (upper needling) Main acupuncture (downward needling) Needle width (mm) 7400 7400 Acupuncture frequency (times / min) 900 900 Needle density (pieces / m) 4000 4000 Needling depth (mm) 6~10 6~10
[0069] Choice of needle
[0070] Compared with staple fiber needling, staple fiber needling is easier to penetrate due to its fluffy web and shorter fibers, and the needle has little tension and low resistance when penetrating. However, for continuous filaments produced by spunbond, the tension and resistance are greater when the needle penetrates the web. If you simply use staple fiber needles, it will be difficult to penetrate and the chance of needle breakage will increase greatly. Therefore, this project uses special needles for producing spunbond needle products.
[0071] Ensure the dipping effect and achieve low-cost green production
[0072] When it is subsequently processed into asphalt felt, the tire base cloth must undergo high-temperature processes such as impregnation and drying. Therefore, the tire base cloth must also undergo high-temperature heat setting first. The thermal stability of the heat-set product is greatly improved, but the strength and stiffness still do not meet the requirements of the tire base cloth. In the subsequent asphalt impregnation process, the structure will change due to the force, affecting the quality of the final product. The conventional approach to solving this problem is to use adhesives to improve the strength and stiffness of the product. The present invention compares the differences between acrylic esters and modified starches as dipping finishing agents, and studies the effects of drying process, glue amount, etc. on product performance.
[0073] Selection of impregnation finishing agent (adhesive)
[0074] At present, the adhesives used in the domestic market mainly include casein glue, chemical glue, starch glue and their improved glue. It can be seen from the performance comparison in (Table 7) that casein glue performs better in various properties, but casein glue raw materials are rare and expensive, so it is difficult to become a large-scale glue; chemical glue is also limited in use due to its toxicity and high pollution: starch raw materials are cheap, easy to obtain, non-toxic and pollution-free, but starch glue has defects in viscosity and generally needs to be modified before use.
[0075] Table 7 Comparison of performance of casein glue, chemical glue and starch glue
[0076] Chemical glue Starch glue Casein glue Initial adhesion middle high high Quick drying slow slow Medium-Fast Anti-condensation performance Difference Difference good Machine performance good good good Suitable for machine speed slow slow quick Stable performance excellent generally good
[0077] Compared with other types of adhesives, adhesives prepared with starch as raw material have defects in performance such as poor machine performance, poor waterproof performance, and short storage time. However, in recent years, with the improvement of people's environmental awareness and the tight supply of petrochemical raw materials, the advantages of starch as a raw material have become prominent. Since starch raw materials are cheap, easy to obtain, non-toxic and environmentally friendly, and a sustainable renewable resource, more and more modified starch adhesives are also used in industrial production and daily life. Traditional polyester staple needle-punched felt base cloth uses acrylic adhesives. The monomers required for this kind of emulsion copolymerization are all petrochemical raw materials, and the cost of use is relatively high. It will cause environmental pollution during the synthesis and use process, and there are problems such as the difficulty in cleaning the production equipment. In the present invention, modified starch is used as a dipping finishing agent, which can reduce production costs on the basis of green environmental protection and the product meeting the requirements of subsequent asphalt impregnation.
[0078] Drying process
[0079] From the production practice, the drying temperature should be based on the fiber material, adhesive characteristics and energy consumption. The selection of appropriate drying temperature and drying time (production line speed) should match the equipment performance and meet the impregnation requirements, so that the adhesive is completely cured, all indicators are within the specified range, the base tire will not turn yellow, and the fiber net will not be damaged. The drying process mainly includes drying temperature and drying time (production line speed). After continuous production practice, the present invention finally determines that the optimal drying temperature of each zone of starch adhesive in the production of tire base cloth is: 210°C in the first zone (drying barrel), 165°C in the second zone (rotary screen), 180°C in the third zone (rotary screen), and the production speed is 18m / min.
[0080] Glue quantity control
[0081] The amount of glue applied directly affects the quality of the product after dipping and the production cost, and is one of the key parameters in the dipping process. The amount of glue applied can be controlled by adjusting the concentration of the dipping finishing agent (modified corn starch solution), controlling the dipping speed, adjusting the roller spacing, etc.
[0082] For example, 200g / ㎡ polyester filament base fabric is selected, the production line speed is controlled at 18m / min, the drying temperature is 210℃~165℃~180℃, and by adjusting the concentration of the dipping finishing agent (modified corn starch solution) and the roller spacing, products with different amounts of glue can be obtained. The effect of the amount of glue on product performance is studied. The test results are as follows:
[0083] As shown in (Table 8),
[0084]
[0085] From the test results, it can be seen that under the condition of a certain base weight, the polyester long tire base increases in thickness, increases in longitudinal and transverse strength, reduces elongation and shrinkage, and the hand feel changes from soft to hard as the glue content increases. Considering the actual use requirements and cost, the final glue content is 25%. Compared with the commercially available polyester staple needle-punched tire base (base weight of 180 / m'), the high-strength polyester filament tire base fabric product (150g / m" base fabric) of the present invention has better performance, short production process and fast production speed.
[0086] The embodiments of the present invention are described in detail above with reference to the accompanying drawings, but the present invention is not limited to the described embodiments. For those skilled in the art, various changes, modifications, substitutions and variations of these embodiments are made without departing from the principles and spirit of the present invention, and still fall within the scope of protection of the present invention.
Claims
1. A production process for high-strength polyester filament base fabric, characterized in that: First, a high-strength polyester filament tire base cloth semi-finished product is produced through the polyester spunbonding and needle punching reinforcement methods, and then it is treated through a dipping and shaping process to finally obtain a high-strength polyester filament tire base cloth product.
2. The production process of high-strength polyester filament base fabric according to claim 1, characterized in that: The method specifically comprises the following steps: the polyester chips are crystallized and dried, fed into a screw extruder, passed through a filter and a metering pump and entered into a spinning box, the melt is quantitatively passed through a spinneret to form primary fibers, the filaments after being drawn are separated and swung, and evenly laid on a mesh curtain to form a fiber web, the fiber web is reinforced by pre-needling and main needling, and is cut and rolled to obtain a semi-finished product of a high-strength polyester filament tire base cloth, and the semi-finished product of the high-strength polyester filament tire base cloth is heat-set, dipped in glue, dried and then finished to obtain a finished product of the high-strength polyester filament tire base cloth.
3. The production process of the high-strength polyester filament base fabric according to claim 2 is characterized in that: In the above steps, a single screw extruder with a diamond pin mixing head is used as a tool for the spinning process, and the cooling side blowing of the spinning is set. The side blowing air duct is a tapered type with a guide plate, a damping rectifying layer composed of a porous plate and a stainless steel mesh, so that the longitudinal velocity gradient of the side blowing air is completed to complete the spinning process.
4. The production process of the high-strength polyester filament base fabric according to claim 2 is characterized in that: In the above steps, a tubular drafter is used for drafting, and the drafting rate and the drafting ratio are regulated by increasing the number of drafting tubes and controlling the drafting air flow speed / temperature.
5. The production process of high-strength polyester filament base fabric according to claim 2, characterized in that: In the above steps, a reciprocating traverse mechanism is used to perform mechanical wire separation by lateral swinging, and then a web laying machine system is used to lay the web.
6. The production process of high-strength polyester filament base fabric according to claim 1, characterized in that: Needle punching reinforcement method is used as the fiber web consolidation method.
7. The production process of high-strength polyester filament base fabric according to claim 4, characterized in that: The tubular drafter is a HY-II type drafter.
8. The production process of high-strength polyester filament base fabric according to claim 4, characterized in that: The drawing speed of the tractor is 5000-6000m / min.
9. The production process of high-strength polyester filament base fabric according to claim 4, characterized in that: The height of the tractor drawing tube is 1000-1200mm, the inner diameter of the tractor drawing tube is 10mm, and the drawing wind pressure is 0.5MPa.
10. The production process of high-strength polyester filament base fabric according to claim 5, characterized in that: The swing amplitude of the reciprocating traverse mechanism is 50-54 mm.