Manufacturing process of lacquer silk

Through the production process of lacquer silk, using alkaline buffer and rinsing and dyeing, the problem of ordinary silk fabrics lacking waterproofing and other functions is solved, and soft and durable lacquer silk is realized, suitable for use in clothing and other products, and the Wearing functions of traditional lacquerware.

CN118910905APending Publication Date: 2024-11-08CHONGQING FUTURE KEQI CLOTHING DESIGN CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411134674.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the prior art, ordinary silk fabrics lack the functions of waterproof, wrinkle-proof, static-resistant, oil-resistant, acid-alkali-resistant and insect-proof bite-proof. At the same time, the lacquer fabric has a hard texture and is not suitable for contact with the skin. Traditional lacquerware lacks the wearable function.

Method used

A lacquered silk production process consists of soaking white silk in alkaline buffer and diluting the paint for dyeing, followed by rinsing dyeing, acidic soaking and softening treatment, retaining soft properties while enhancing waterproofing. , anti-pleasure and electrostatic resistance, and finally the process is completed by printing silk pattern.

Benefits of technology

It realizes the soft and skin-friendly effect of lacquer silk, and has the tough characteristics of waterproof, wrinkle-proof and static resistance, making this material suitable for use in clothing and other products, expanding the wearable function of traditional lacquerware.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a manufacturing process of lacquer silk. The method comprises the following steps: S1, washing; s2, soaking in an alkaline buffer solution; s3, preparing a dyeing accelerating solution; s4, the silk treated in the step S2 is added into the dyeing accelerating liquid in the step S3 to be soaked; s5, rinsing and dyeing the silk treated in the step S4; s6, repeating the step S5; s7, soaking the silk treated in the step S6 into an acidic soaking solution; s8, softening is carried out; and S9, printing silk patterns, and then drying in the shade to obtain a lacquer silk finished product. According to the manufacturing process of the lacquer silk, provided by the invention, the lacquer coating still keeps the soft characteristic when being attached to the silk, that is, the soft and skin-friendly effects of the silk can be kept at the same time, so that the manufactured lacquer silk can be used for manufacturing products such as clothes and the like. The lacquer silk manufacturing process provided by the invention can retain the characteristics of lacquer, so that the manufactured lacquer silk cloth has the tough characteristics of water resistance, wrinkle resistance and static resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of silk production technology, and in particular to a production technology of lacquer silk. Background Art

[0002] Raw lacquer, commonly known as "earth lacquer", also known as "national lacquer" or "lacquer", is a milky white pure natural liquid paint harvested from lacquer trees. It gradually turns brown after contact with air, and the surface dries and hardens in about 4 hours to form a paint film. Raw lacquer has high economic value. It has the characteristics of corrosion resistance, wear resistance, acid resistance, solvent resistance, heat resistance, good water and insulation properties, and rich gloss. It is a high-quality paint for military industry, industrial equipment, agricultural machinery, infrastructure, handicrafts and high-end furniture.

[0003] Silk is a kind of textile, woven with silk or synthetic fibers, artificial fibers, short silk, etc.; it is a general term for fabrics made of pure or interwoven silk or artificial silk. Silk is also widely used, such as silk clothing, silk scarves, silk paintings, silk books, silk bags, silk craft ornaments, etc. Silk is the most common as clothing.

[0004] The applicant has found that the prior art has at least the following technical problems:

[0005] 1. Ordinary silk fabrics in the prior art do not have the functions of being waterproof, wrinkle-proof, anti-static, oil-resistant, acid-resistant, alkali-resistant, and insect-resistant;

[0006] 2. The lacquer fabrics in the prior art lack the softness and are hard in texture, making them unsuitable for contact with the skin.

[0007] 3. In the existing technology, most of the lacquer art products are currently made into utensils. Now making them into clothing expands the wearable functionality of traditional lacquerware. Summary of the invention

[0008] The purpose of the present invention is to provide a production process of lacquer silk to solve the technical problem that ordinary silk cloth in the prior art does not have the functions of waterproof, wrinkle-proof and anti-static. The preferred technical solutions among the many technical solutions provided by the present invention can produce many technical effects as described below.

[0009] To achieve the above object, the present invention provides the following technical solutions:

[0010] A production process of lacquer silk, characterized by comprising the following steps:

[0011] S1. Wash the white silk with clean water;

[0012] S2, soaking the cleaned silk in an alkaline buffer solution, first at a temperature of 18-25°C for 2-4 hours, then at a temperature of 55-65°C for 0.8-1.2 hours, and drying the silk after soaking;

[0013] S3, diluting the lacquer with alcohol, and then mixing the diluted lacquer with an alkaline buffer solution to obtain a dye-accelerating solution;

[0014] S4, adding the silk treated in step S2 to the dyeing accelerator in step S3 and soaking for 8-20 minutes until the surface of the silk changes from white to brown;

[0015] S5, rinsing and dyeing the silk processed in step S4, and then taking it out and drying it in the shade;

[0016] S6, drying the silk treated in step S5 in the shade until it is half dry, repeating step S5 at least 6 times, and ironing the silk until the silk stops fading;

[0017] S7, soaking the silk treated in step S6 in an acidic soaking liquid to remove excess alkaline substances on the surface of the silk, and then drying in the shade;

[0018] S8, soaking the silk processed in step S7 in a softening liquid to soften the silk, and then drying in the shade and ironing the silk;

[0019] S9, printing silk patterns on the silk processed in step S8, and then drying in the shade to obtain a finished lacquer silk product.

[0020] Furthermore, in step S2, the alkaline buffer solution contains sodium carbonate and sodium bicarbonate, the mass fraction of sodium carbonate is 0.5%-0.6%, and the mass fraction of sodium bicarbonate is 0.4%-0.5%.

[0021] Furthermore, in step S2, the alkaline buffer solution contains sodium carbonate and sodium bicarbonate, the mass fraction of sodium carbonate is 0.55%, and the mass fraction of sodium bicarbonate is 0.45%;

[0022] In step S2, the pH of the alkaline buffer solution is 9.2-10.3.

[0023] Furthermore, in step S5, the rinsing liquid used for rinsing and dyeing is prepared according to the following raw materials in parts by weight: 0.3-0.8 parts of water, 0.3-0.8 parts of alcohol, and 5-7 parts of sodium carbonate; during rinsing and dyeing, the temperature of the rinsing liquid is 55-65°C, and during rinsing, the silk is continuously rubbed, and the rinsing and dyeing time is 8-20 minutes.

[0024] Furthermore, in step S7, the acidic soaking liquid is an acetic acid solution, which is prepared by distilled water and acetic acid powder, and the mass ratio of distilled water to acetic acid powder is 1000:20-30.

[0025] Furthermore, in step S7, the acidic soaking solution is used for 3-4 times, each soaking is at room temperature for 15-20 minutes, and after each soaking, it is dried before the next soaking.

[0026] Furthermore, in step S8, the softening liquid is prepared by using alcohol, clean water and glycerol, and the volume ratio of alcohol, clean water and glycerol is 1:1:1.

[0027] Furthermore, in step S8, the soaking is performed 3-4 times with the softening liquid, each soaking is performed at a temperature of 55-65° C. for 15-20 minutes, and after each soaking, it is dried before the next soaking.

[0028] Furthermore, in step S9, when printing the silk pattern, the lacquer silk pattern is first made, and then the prepared color lacquer is printed on the surface of the lacquer silk by screen printing, and finally the printed lacquer silk is dried in the shade to obtain the lacquer silk finished product.

[0029] Based on the above technical solution, the embodiments of the present invention can at least produce the following technical effects:

[0030] (1) The production process of lacquer silk provided by the present invention allows the lacquer coating to remain soft when attached to silk, that is, the soft and skin-friendly effect of silk can be retained at the same time. Therefore, the lacquer silk produced can be used to make clothing and other products.

[0031] (2) The production process of lacquer silk provided by the present invention can retain the characteristics of lacquer, so that the lacquer silk fabric produced has the tough characteristics of being waterproof, wrinkle-proof, and anti-static. DETAILED DESCRIPTION

[0032] To make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be described in detail below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other implementation methods obtained by ordinary technicians in this field without creative work belong to the scope of protection of the present invention.

[0033] Embodiment 1:

[0034] A production process of lacquer silk, characterized by comprising the following steps:

[0035] S1. Wash the white silk with clean water;

[0036] S2, soaking the cleaned silk in an alkaline buffer solution, first at 20°C for 3 hours, then at 50°C for 1 hour, and drying the silk after soaking;

[0037] The alkaline buffer solution contains sodium carbonate and sodium bicarbonate, wherein the mass fraction of sodium carbonate is 0.55% and the mass fraction of sodium bicarbonate is 0.45%. Sodium hydroxide is used to adjust the pH value of the alkaline buffer solution to 9.5.

[0038] S3, diluting the lacquer with alcohol at a volume ratio of 1:1, and then uniformly mixing the diluted lacquer with an alkaline buffer at a volume ratio of 1:1 to obtain a dyeing accelerator;

[0039] S4, adding the silk processed in step S2 into the dyeing accelerator solution in step S3 and soaking it until the surface of the silk changes from white to brown;

[0040] S5, rinsing and dyeing the silk processed in step S4, and then taking it out and drying it in the shade;

[0041] The rinsing liquid used for rinsing and dyeing is prepared according to the following raw materials in parts by weight: 0.5 parts of water, 0.5 parts of alcohol, and 6 parts of sodium carbonate; during rinsing and dyeing, the temperature of the rinsing liquid is 60°C, and during rinsing, the silk is continuously rubbed, and the rinsing and dyeing time is 15 minutes;

[0042] S6, drying the silk treated in step S5 in the shade until it is half dry, repeating step S5 six times, until the silk no longer fades, drying in the shade, and steam ironing or steam ironing until it is smooth;

[0043] S7, soaking the silk treated in step S6 in an acidic soaking liquid to remove excess alkaline substances on the surface of the silk, and then drying in the shade;

[0044] The acidic soaking solution is an acetic acid solution, which is prepared with distilled water and acetic acid powder, and the mass ratio of distilled water to acetic acid powder is 1000:25; the number of soakings with the acidic soaking solution is 3 times, each soaking is at room temperature for 18 minutes, and after each soaking, it is dried before the next soaking.

[0045] S8, soaking the silk processed in step S7 in a softening liquid to soften the silk, then drying it in the shade and steam ironing or steam ironing it until it is smooth;

[0046] The softening liquid is prepared with alcohol, water and glycerol, and the volume ratio of alcohol, water and glycerol is 1:1:1. The softening liquid is used for immersion 3 times, each immersion is at a temperature of 60°C for 18 minutes, and after each immersion, it is dried before the next immersion.

[0047] S9, printing silk patterns on the silk processed in step S8. When printing the silk patterns, first make the lacquer art silk patterns, then print the prepared color lacquer on the surface of the lacquer art silk by screen printing, and finally dry the printed lacquer art silk in the shade to obtain the finished lacquer silk product.

[0048] Embodiment 2:

[0049] A production process of lacquer silk, characterized by comprising the following steps:

[0050] S1. Wash the white silk with clean water;

[0051] S2, soaking the cleaned silk in an alkaline buffer solution, first at 25°C for 2 hours, then at 65°C for 0.8 hours, and drying the silk after soaking;

[0052] The alkaline buffer solution contains sodium carbonate and sodium bicarbonate, wherein the mass fraction of sodium carbonate is 0.6% and the mass fraction of sodium bicarbonate is 0.4%. Sodium hydroxide is used to adjust the pH value of the alkaline buffer solution to 9.2.

[0053] S3, diluting the lacquer with alcohol at a volume ratio of 1:1, and then mixing the diluted lacquer with an alkaline buffer at a volume ratio of 1:1 to obtain a dyeing accelerator;

[0054] S4, adding the silk treated in step S2 to the dyeing accelerator in step S3 and soaking for 20 minutes until the surface of the silk changes from white to brown;

[0055] S5, rinsing and dyeing the silk processed in step S4, and then taking it out and drying it in the shade;

[0056] The rinsing liquid used for rinsing and dyeing is prepared according to the following raw materials in parts by weight: 0.8 parts of water, 0.3 parts of alcohol, and 7 parts of sodium carbonate; during rinsing and dyeing, the temperature of the rinsing liquid is 65°C, and during rinsing, the silk is continuously rubbed, and the rinsing and dyeing time is 8 minutes;

[0057] S6, drying the silk treated in step S5 in the shade until it is half dry, repeating step S5 seven times, until the silk no longer fades, drying in the shade, and steam ironing or steam ironing until it is smooth;

[0058] S7, soaking the silk treated in step S6 in an acidic soaking liquid to remove excess alkaline substances on the surface of the silk, and then drying in the shade;

[0059] The acidic soaking liquid is an acetic acid solution, prepared by distilled water and acetic acid powder, and the mass ratio of distilled water to acetic acid powder is 1000: 30. The acidic soaking liquid is used for soaking 3 times, each soaking is soaked at room temperature for 20 minutes, and after each soaking, it is dried before the next soaking.

[0060] S8, soaking the silk processed in step S7 in a softening liquid to soften the silk, then drying it in the shade and steam ironing or steam ironing it until it is smooth;

[0061] The softening liquid is prepared with alcohol, water and glycerol, and the volume ratio of alcohol, water and glycerol is 1:1:1. The softening liquid is used for immersion for 3 times, and each immersion is at a temperature of 65°C for 20 minutes. After each immersion, it is dried before the next immersion.

[0062] S9, printing silk patterns on the silk processed in step S8. When printing the silk patterns, first make the lacquer art silk patterns, then print the prepared color lacquer on the surface of the lacquer art silk by screen printing, and finally dry the printed lacquer art silk in the shade to obtain the finished lacquer silk product.

[0063] Embodiment 3:

[0064] A production process of lacquer silk, characterized by comprising the following steps:

[0065] S1. Wash the white silk with clean water;

[0066] S2, soaking the cleaned silk in an alkaline buffer solution, first at 18°C ​​for 4 hours, then at 55°C for 1.2 hours, and drying the silk after soaking;

[0067] The alkaline buffer solution contains sodium carbonate and sodium bicarbonate, wherein the mass fraction of sodium carbonate is 0.5% and the mass fraction of sodium bicarbonate is 0.5%. Sodium hydroxide is used to adjust the pH value of the alkaline buffer solution to 9.2.

[0068] S3, diluting the lacquer with alcohol at a volume ratio of 1:1, and then mixing the diluted lacquer with an alkaline buffer at a volume ratio of 1:1 to obtain a dyeing accelerator;

[0069] S4, adding the silk treated in step S2 to the dyeing accelerator in step S3 and soaking for 8-20 minutes until the surface of the silk changes from white to brown;

[0070] S5, rinsing and dyeing the silk processed in step S4, and then taking it out and drying it in the shade;

[0071] The rinsing liquid used for rinsing and dyeing is prepared according to the following raw materials in parts by weight: 0.3 parts of water, 0.8 parts of alcohol, and 5 parts of sodium carbonate; during rinsing and dyeing, the temperature of the rinsing liquid is 55°C, and during rinsing, the silk is continuously rubbed, and the rinsing and dyeing time is 20 minutes;

[0072] S6, drying the silk treated in step S5 in the shade until it is half dry, repeating step S5 six times, and drying in the shade and steam ironing or steam ironing until the silk stops fading;

[0073] S7, soaking the silk treated in step S6 in an acidic soaking liquid to remove excess alkaline substances on the surface of the silk, and then drying in the shade;

[0074] The acidic soaking liquid is an acetic acid solution, prepared by distilled water and acetic acid powder, and the mass ratio of distilled water to acetic acid powder is 1000: 20. The acidic soaking liquid is used for 4 times, each soaking is at room temperature for 15 minutes, and after each soaking, it is dried before the next soaking.

[0075] S8, soaking the silk processed in step S7 in a softening liquid to soften the silk, then drying it in the shade and steam ironing or steam ironing it until it is smooth;

[0076] The softening liquid is prepared with alcohol, water and glycerol, and the volume ratio of alcohol, water and glycerol is 1:1:1. The number of soaking times with the softening liquid is 4 times, and each soaking is soaked at a temperature of 55°C for 15 minutes. After each soaking, dry it first before the next soaking.

[0077] S9, printing silk patterns on the silk processed in step S8. When printing the silk patterns, first make the lacquer art silk patterns, then print the prepared color lacquer on the surface of the lacquer art silk by screen printing, and finally dry the printed lacquer art silk in the shade to obtain the finished lacquer silk product.

[0078] Embodiment 4:

[0079] A production process of lacquer silk, characterized by comprising the following steps:

[0080] S1. Wash the white silk with clean water;

[0081] S2, soaking the cleaned silk in an alkaline buffer solution, first at 20°C for 2.5 hours, then at 58°C for 1.2 hours, and drying the silk after soaking;

[0082] The alkaline buffer solution contains sodium carbonate and sodium bicarbonate, wherein the mass fraction of sodium carbonate is 0.52% and the mass fraction of sodium bicarbonate is 0.48%. Sodium hydroxide is used to adjust the pH value of the alkaline buffer solution to 10.3.

[0083] S3, diluting the lacquer with alcohol at a volume ratio of 1:1, and then mixing the diluted lacquer with an alkaline buffer at a volume ratio of 1:1 to obtain a dyeing accelerator;

[0084] S4, adding the silk treated in step S2 to the dyeing accelerator in step S3 and soaking for 8-20 minutes until the surface of the silk changes from white to brown;

[0085] S5, rinsing and dyeing the silk processed in step S4, and then taking it out and drying it in the shade;

[0086] The rinsing liquid used for rinsing and dyeing is prepared according to the following raw materials in parts by weight: 0.7 parts of water, 0.4 parts of alcohol, and 5 parts of sodium carbonate; during rinsing and dyeing, the temperature of the rinsing liquid is 65°C, and during rinsing, the silk is continuously rubbed, and the rinsing and dyeing time is 20 minutes;

[0087] S6, drying the silk treated in step S5 in the shade until it is half dry, repeating step S5 six times, and drying in the shade and steam ironing or steam ironing until the silk stops fading;

[0088] S7, soaking the silk treated in step S6 in an acidic soaking liquid to remove excess alkaline substances on the surface of the silk, and then drying in the shade;

[0089] The acidic soaking liquid is an acetic acid solution, prepared by distilled water and acetic acid powder, and the mass ratio of distilled water to acetic acid powder is 1000: 22. The acidic soaking liquid is used for soaking 3 times, each soaking is soaked at room temperature for 20 minutes, and after each soaking, it is dried before the next soaking.

[0090] S8, soaking the silk processed in step S7 in a softening liquid to soften the silk, then drying it in the shade and steam ironing or steam ironing it until it is smooth;

[0091] The softening liquid is prepared with alcohol, water and glycerol, and the volume ratio of alcohol, water and glycerol is 1:1:1. The softening liquid is used for immersion 3 times, each immersion is at 60℃ for 20min, and after each immersion, it is dried before the next immersion.

[0092] S9, printing silk patterns on the silk processed in step S8. When printing the silk patterns, first make the lacquer art silk patterns, then print the prepared color lacquer on the surface of the lacquer art silk by screen printing, and finally dry the printed lacquer art silk in the shade to obtain the finished lacquer silk product.

[0093] Embodiment 5:

[0094] A production process of lacquer silk, characterized by comprising the following steps:

[0095] S1. Wash the white silk with clean water;

[0096] S2, soaking the cleaned silk in an alkaline buffer solution, first at 22°C for 3.5 hours, then at 62°C for 1 hour, and drying the silk after soaking;

[0097] The alkaline buffer solution contains sodium carbonate and sodium bicarbonate, wherein the mass fraction of sodium carbonate is 0.58% and the mass fraction of sodium bicarbonate is 0.43%. Sodium hydroxide is used to adjust the pH value of the alkaline buffer solution to 9.5.

[0098] S3, diluting the lacquer with alcohol at a volume ratio of 1:1, and then mixing the diluted lacquer with an alkaline buffer at a volume ratio of 1:1 to obtain a dyeing accelerator;

[0099] S4, adding the silk treated in step S2 to the dyeing accelerator in step S3 and soaking for 8-20 minutes until the surface of the silk changes from white to brown;

[0100] S5, rinsing and dyeing the silk processed in step S4, and then taking it out and drying it in the shade;

[0101] The rinsing liquid used for rinsing and dyeing is prepared according to the following raw materials in parts by weight: 0.6 parts of water, 0.6 parts of alcohol, and 6 parts of sodium carbonate; during rinsing and dyeing, the temperature of the rinsing liquid is 60°C, and during rinsing, the silk is continuously rubbed, and the rinsing and dyeing time is 10 minutes;

[0102] S6, drying the silk treated in step S5 in the shade until it is half dry, repeating step S5 seven times, and drying in the shade and steam ironing or steam ironing until the silk stops fading;

[0103] S7, soaking the silk treated in step S6 in an acidic soaking liquid to remove excess alkaline substances on the surface of the silk, and then drying in the shade;

[0104] The acidic soaking liquid is an acetic acid solution, prepared by distilled water and acetic acid powder, and the mass ratio of distilled water to acetic acid powder is 1000: 28. The acidic soaking liquid is used for 4 times, each time for 15 minutes at room temperature, and after each soaking, it is dried before the next soaking.

[0105] S8, soaking the silk processed in step S7 in a softening liquid to soften the silk, then drying it in the shade and steam ironing or steam ironing it until it is smooth;

[0106] The softening liquid is prepared with alcohol, water and glycerol, and the volume ratio of alcohol, water and glycerol is 1:1:1. The softening liquid is used for immersion 3 times, each immersion is at a temperature of 65°C for 120 minutes, and after each immersion, it is dried before the next immersion.

[0107] S9, printing silk patterns on the silk processed in step S8. When printing the silk patterns, first make the lacquer art silk patterns, then print the prepared color lacquer on the surface of the lacquer art silk by screen printing, and finally dry the printed lacquer art silk in the shade to obtain the finished lacquer silk product.

[0108] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A production process of lacquer silk, It is characterized in that The steps include: S1. Wash the white silk with clean water; S2, soaking the cleaned silk in an alkaline buffer solution, first at a temperature of 18-25°C for 2-4 hours, then at a temperature of 55-65°C for 0.8-1.2 hours, and drying the silk after soaking; S3, diluting the lacquer with alcohol, and then mixing the diluted lacquer with an alkaline buffer solution to obtain a dye-accelerating solution; S4, adding the silk treated in step S2 to the dyeing accelerator in step S3 and soaking for 8-20 minutes until the surface of the silk changes from white to brown; S5, rinsing and dyeing the silk processed in step S4, and then taking it out and drying it in the shade; S6, drying the silk treated in step S5 in the shade until it is half dry, repeating step S5 at least 6 times, and ironing the silk until the silk stops fading; S7, soaking the silk treated in step S6 in an acidic soaking liquid to remove excess alkaline substances on the surface of the silk, and then drying in the shade; S8, soaking the silk processed in step S7 in a softening liquid to soften the silk, and then drying in the shade and ironing the silk; S9, printing silk patterns on the silk processed in step S8, and then drying in the shade to obtain a finished lacquer silk product.

2. The production process of lacquer silk according to claim 1, It is characterized in that In step S2, the alkaline buffer solution contains sodium carbonate and sodium bicarbonate, wherein the mass fraction of sodium carbonate is 0.5%-0.6%, and the mass fraction of sodium bicarbonate is 0.4%-0.5%.

3. The production process of lacquer silk according to claim 1, It is characterized in that In step S2, the alkaline buffer solution contains sodium carbonate and sodium bicarbonate, the mass fraction of sodium carbonate is 0.55%, and the mass fraction of sodium bicarbonate is 0.45%; in step S2, the pH of the alkaline buffer solution is 9.2-10.

3.

4. The process for producing lacquer silk according to claim 1, It is characterized in that In step S5, the rinsing liquid used for rinsing and dyeing is prepared according to the following raw materials in parts by weight: 0.3-0.8 parts of water, 0.3-0.8 parts of alcohol, and 5-7 parts of sodium carbonate; during rinsing and dyeing, the temperature of the rinsing liquid is 55-65° C., and during rinsing, the silk is continuously rubbed, and the rinsing and dyeing time is 8-20 minutes.

5. The process for producing lacquer silk according to claim 1, It is characterized in that In step S7, the acidic soaking liquid is an acetic acid solution prepared by distilled water and acetic acid powder, and the mass ratio of distilled water to acetic acid powder is 1000:20-30.

6. The process for producing lacquer silk according to claim 1, It is characterized in that In step S7, the acidic soaking solution is used for 3-4 times, each soaking is at room temperature for 15-20 minutes, and after each soaking, it is dried before the next soaking.

7. The process for making lacquer silk according to claim 1, It is characterized in that In step S8, the softening liquid is prepared by using alcohol, clean water and glycerol, and the volume ratio of alcohol, clean water and glycerol is 1:1:

1.

8. The process for producing lacquer silk according to claim 1, It is characterized in that In step S8, the soaking is performed 3-4 times with the softening liquid, each soaking is performed at a temperature of 55-65° C. for 15-20 minutes, and after each soaking, it is dried before the next soaking.

9. The process for producing lacquer silk according to claim 1, It is characterized in that In step S9, when printing the silk pattern, the lacquer silk pattern is first made, and then the prepared color lacquer is printed on the surface of the lacquer silk by screen printing, and finally the printed lacquer silk is dried in the shade to obtain the lacquer silk finished product.