Method for improving fuel combustion efficiency under high-dust working condition of rotary kiln

By adjusting the oxygen-rich air content and coal fineness moisture of primary fans and coal conveyor fans in the rotary kiln, the problem of low fuel combustion efficiency under high dust concentration is solved, and the kiln head temperature is stabilized and the fuel is efficiently burned, which is improved. Productivity and quality.

CN118912899APending Publication Date: 2024-11-08TAIYUAN IRON & STEEL (GRP) CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411125647.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The high dust concentration in the rotary kiln leads to a decrease in fuel combustion efficiency, and the contact between the fuel and the combustion-supporting air in the kiln decreases, resulting in incomplete combustion of the fuel, affecting production efficiency and quality.

Method used

By adjusting the oxygen-rich air content in primary fans and coal transport fans, combining coal fineness and moisture control, the kiln head temperature is maintained at 850±50℃, ensuring that the fuel is fully burned under high-temperature oxygen-rich conditions and improving combustion efficiency.

Benefits of technology

The fuel combustion efficiency is improved, coal consumption is reduced, and the production efficiency and quality of the rotary kiln is improved. The daily output of a single kiln is increased by 12.6%, the quality is increased by 1.2%, and the coal saving rate is 5.1%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a method for improving fuel combustion efficiency of a rotary kiln under a high-dust working condition, and belongs to the technical field of rotary kiln production and calcination. The method comprises the steps of adjusting the oxygen-enriched content in the air volume of a primary fan and a coal conveying fan, controlling the fineness of pulverized coal and the moisture of the pulverized coal, keeping the temperature of the kiln head of the rotary kiln stable, controlling the combustion condition of fuel to be in the optimal state all the time, stabilizing the thermal regulation of the production process of the rotary kiln, improving the combustion efficiency of the fuel, reducing the production coal consumption and improving the production efficiency of the rotary kiln. By the adoption of the method, the combustion effect of fuel of the rotary kiln under the high-dust working condition is obviously improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for improving fuel combustion efficiency under high-dust working conditions of a rotary kiln, and belongs to the technical field of rotary kiln production calcination. Background Art

[0002] The first condition for calcining active lime in a rotary kiln is the selection and use of raw materials. The raw materials are mainly carbonate rocks, with the main component being CaCO3. Common ones include: granular crystalline limestone, dense limestone, porous limestone, earthy limestone, marly limestone, chalk, dolomite, shell-limestone river pebbles, etc. The raw materials are mostly dense limestone, which has the characteristics of dense fine-grained crystal structure and low texture hardness, making it an ideal raw material. At the same time, the selection of limestone particle size ratio, mineral structure, hardness, wear resistance and other physical properties are also important factors in the selection of raw materials. The corresponding hardness and wear resistance also vary significantly with the different mineral structures of limestone. Taking the Majiagou Formation ore as an example, the ore has large reserves in my country, but due to its weaknesses of low strength, easy bursting, and poor wear resistance, as well as secondary crushing during transportation, bursting caused by poor thermal stability during the preheating process in the preheater, and tumbling and moving in the kiln during calcination, a high concentration of dust (≦2mm) of more than 20% is generated, which reduces the contact between the fuel and the combustion-supporting air during the calcination process in the rotary kiln, resulting in reduced fuel combustion efficiency and backward movement of the rotary kiln combustion flame; the reducing atmosphere formed by the incomplete combustion of the fuel produces a ring in the area from the combustion zone to the preheating zone of the rotary kiln cylinder, and the material is compacted in the rotary kiln preheater, which destroys the thermal and pressure systems of the rotary kiln production, causes abnormal production of the rotary kiln and reduced quality, and seriously affects the large-scale industrial production and application of the Majiagou Formation ore in the fields of metallurgy and construction.

[0003] In summary, it is very necessary to adopt a method to improve the fuel combustion efficiency when the rotary kiln has high dust concentration to ensure the high-efficiency operation of the rotary kiln calcining system. Summary of the invention

[0004] The present invention aims to provide a method for improving fuel combustion efficiency under high dust conditions of a rotary kiln. By introducing oxygen-enriched air, the fuel combustion efficiency is improved when the rotary kiln has high dust concentration, the kiln head temperature is increased, the production coal consumption is reduced, and the production efficiency of the rotary kiln is improved.

[0005] The present invention provides a method for improving fuel combustion efficiency under high-dust working conditions of a rotary kiln. The method utilizes the principle that fuel has a violent combustion reaction under high-temperature and oxygen-rich conditions, starts from the core factors affecting fuel combustion conditions, namely, high-temperature environment and oxygen-rich air content, and according to CO concentration in kiln tail exhaust gas and kiln head temperature changes, by reasonably controlling the oxygen-rich air content in the transport air volume of a rotary kiln primary fan and a coal conveying fan, combined with the control of coal powder fineness and coal powder moisture, the kiln head temperature of the rotary kiln is increased, the fuel combustion efficiency is improved, and the purpose of reducing production coal consumption, increasing the production volume of the rotary kiln and stabilizing the quality is achieved.

[0006] The present invention provides a method for improving fuel combustion efficiency under high dust conditions of a rotary kiln, which mainly includes: adjusting the oxygen-enriched content in the air volume of a primary fan and a coal conveying fan, combining the control of coal powder fineness and coal powder moisture, maintaining the temperature of the rotary kiln head stable, always controlling the fuel combustion condition in the best state, stabilizing the thermal system of the rotary kiln production process, improving fuel combustion efficiency, reducing production coal consumption, and improving the production efficiency of the rotary kiln. By adopting the above method, the coal powder combustion effect is significantly improved when the rotary kiln is roasting easy-to-powder limestone.

[0007] The method for improving the fuel combustion efficiency of a rotary kiln with high dust concentration provided by the present invention comprises the following contents: 1. Operation adjustment basis 1) Adjustments are made based on the CO content in the exhaust gas at the kiln tail and the temperature changes at the kiln head, with the coal powder fineness and moisture content as reference.

[0008] 2) CO content in kiln tail exhaust gas: 5000±1000ppm; kiln head temperature standard: 850±50℃; coal powder fineness according to the percentage of passing rate of 200 mesh sieve is 96±2%; coal powder moisture standard (i.e. coal powder moisture content) is 2±0.5% (mass percentage); air-coal ratio standard is 7~9:1.

[0009] 3) Adjustments should be made when the CO content in the exhaust gas at the kiln tail fluctuates by more than ±1000ppm or changes continuously, or the temperature at the kiln head fluctuates by more than ±50℃ or changes continuously.

[0010] 2. Operation adjustment method 1) When the dust concentration of the rotary kiln is high and causes the CO content in the tail gas to be higher than 6000ppm, increase the oxygen enrichment content of the air supplied by the primary fan and the coal conveying fan by 4%~6% (volume percentage); when the CO content in the kiln tail gas has a downward trend and is lower than 4000ppm, reduce the oxygen enrichment content of the air supplied by the primary fan and the coal conveying fan by 4%~6% to restore to the standard parameters, that is, the CO content in the kiln tail gas is 5000±1000ppm.

[0011] 2) When the dust concentration of the rotary kiln is high and the kiln head temperature is lower than 800℃, increase the oxygen enrichment content of the primary fan and coal conveying fan by 5%; when the kiln head temperature is higher than 900℃, reduce the oxygen enrichment content of the primary fan and coal conveying fan by 5% and restore to the standard parameters, that is, maintain the kiln head temperature at 850±50℃.

[0012] 3) When the passing rate of coal powder fineness through 200 mesh sieve reaches more than 98%, reduce the speed of powder concentrator by 1%; when the passing rate of coal powder fineness through 200 mesh sieve is less than 94%, increase the speed of powder concentrator by 1% to restore to the standard parameters of coal grinding, and maintain the passing rate of coal powder fineness through 200 mesh sieve at 96±2%.

[0013] 4) When the moisture content of coal powder is higher than 2.5% (mass percentage), reduce the coal grinding rate by 2t / h and stabilize the mill outlet temperature; when the moisture content of coal powder is lower than 1.5%, increase the coal grinding rate by 2t / h, restore to the standard parameters of coal grinding, and maintain the air-coal ratio at 7~9:1.

[0014] Beneficial effects of the present invention: (1) By introducing oxygen-enriched air, the combustion efficiency of fuel is improved when the dust concentration of the rotary kiln is high, the kiln head temperature is increased, the production coal consumption is reduced, and the production efficiency of the rotary kiln is improved; (2) This operation adjustment method was applied to the actual production of the rotary kiln. The temperature at the kiln head of the rotary kiln was stabilized at 850±50℃, the CO content in the exhaust gas at the kiln tail was maintained at 5000±1000ppm, the daily output of a single rotary kiln increased by 12.6%, the quality improved by about 1.2%, and the coal saving rate of the rotary kiln was 5.1%. DETAILED DESCRIPTION

[0015] Comparative Example: First, a method for adjusting the combustion efficiency of a rotary kiln roasting pulverizable limestone fuel according to an existing process is provided, and the specific steps are as follows: (1) Stable process parameters: CO content in kiln exhaust gas: 5000±1000ppm; kiln head temperature standard: 850±50℃; coal powder fineness standard: 96±2%; coal powder moisture standard: 2±0.5%; air-coal ratio: 8:1.

[0016] (2) Detection of important parameters: real-time detection of air volume and oxygen enrichment content of primary fan and coal conveying fan; real-time detection of operating air volume of primary fan, coal conveying fan and secondary fan, real-time detection of CO content in exhaust gas at kiln tail; real-time detection of kiln head temperature.

[0017] (3) Adjustment of oxygen-enriched air supply content of primary fan and coal conveying fan: During the production process, the control is based on whether the CO concentration of the exhaust gas at the kiln tail exceeds 5000±1000ppm, whether the temperature at the kiln head exceeds 850±50℃, and whether the air-coal ratio exceeds 8:1. Operational adjustments are made based on changes (the original process operation includes on-site increase of secondary air volume, etc.).

[0018] (4) After the adjustment, verify whether the adjustment range and direction are correct based on the CO concentration of the kiln tail exhaust gas, the kiln head temperature, the real-time detection curve, and the kiln head sample roasting rate in the next hour or several hours. The experiment found that after increasing the secondary air volume on site, the secondary air temperature and the kiln head temperature decreased, and the dust concentration in the kiln head hood increased, which made the coal powder combustion conditions worse.

[0019] The above benchmark example shows that in the continuous production process of the rotary kiln system, when the dust concentration at the kiln head is high, improving the fuel combustion effect through existing operating means lags behind the actual production situation by four hours, and the effect is not good, resulting in invalid operation adjustments or deviations in direction, which is not conducive to stable production.

[0020] The specific embodiments of the present invention are further described below by way of examples, but the specific embodiments of the present invention are not limited to the following examples. Example

[0021] In this embodiment, the CO concentration of the exhaust gas at the kiln tail and the temperature at the kiln head are first used as the main basis for operation, and then the oxygen enrichment content of the air supplied by the primary fan and the coal conveying fan and the changes in the fuel input amount are adjusted to make advance operation adjustments.

[0022] The specific steps are as follows: (1) Operation adjustment basis: Adjustment is made based on the CO content in the exhaust gas at the kiln tail and the temperature change at the kiln head, with the coal powder fineness and moisture content as reference.

[0023] Stable parameters: Stable process parameters: CO content in kiln tail exhaust gas: 5000±1000ppm; kiln head temperature standard: 850±50℃; coal powder fineness standard 96±2%; coal powder moisture standard 2±0.5%; air-coal ratio standard 7~9:1.

[0024] (2) Detection of important parameters: real-time detection of air volume and oxygen enrichment content of primary fan and coal conveying fan; real-time detection of operating air volume of primary fan, coal conveying fan and secondary fan, real-time detection of CO content in exhaust gas at kiln tail; real-time detection of kiln head temperature.

[0025] When the CO content in the exhaust gas at the kiln tail fluctuates by more than ±1000PPm or changes continuously, or the temperature at the kiln head fluctuates by more than ±50℃ or changes continuously, follow the steps below.

[0026] (3) Adjustment of oxygen-enriched air supply and secondary air volume of primary fan and coal conveying fan: During the production process, the control system calculates the theoretical change of secondary air consumption based on the CO concentration of exhaust gas at the kiln tail and the real-time detection results of kiln head temperature and the amount of fuel input, and makes corresponding operational adjustments during operation. The specific adjustment methods are as follows: ① When the dust concentration of the rotary kiln is high and causes the CO content in the tail gas to be higher than 6000ppm, increase the oxygen enrichment content of the primary fan and coal conveying fan by 4~6% (volume percentage); when the CO content in the kiln tail gas shows a downward trend and is lower than 4000ppm, reduce the primary fan and coal conveying fan air supply content by 5% to restore to the standard parameters, that is, the CO content in the kiln tail gas is 5000±1000ppm.

[0027] ② When the dust concentration of the rotary kiln is high and causes the kiln head temperature to be lower than 800℃, increase the oxygen-enriched air content of the primary fan and the coal conveying fan by 5%; when the kiln head temperature is higher than 900℃, reduce the oxygen-enriched air content of the primary fan and the coal conveying fan by 5% and restore to the standard parameters, that is, maintain the kiln head temperature at 850±50℃.

[0028] ③ When the passing rate of coal powder fineness through 200 mesh sieve reaches more than 98%, reduce the speed of powder concentrator by 1%; when the passing rate of coal powder fineness through 200 mesh sieve is less than 94%, increase the speed of powder concentrator by 1%, restore to the standard parameters of coal grinding, and maintain the passing rate of coal powder fineness through 200 mesh sieve at 96±2%.

[0029] ④ When the moisture content of coal powder is higher than 2.5%, reduce the coal grinding capacity by 2t / h and stabilize the mill outlet temperature; when the moisture content of coal powder is lower than 1.5%, increase the coal grinding capacity by 2t / h, restore to the standard parameters of coal grinding, and maintain the air-coal ratio at 7~9:1.

[0030] (4) After the adjustment, verify whether the adjustment range and direction are correct based on the CO concentration of the kiln tail exhaust gas, the kiln head temperature, the real-time detection curve, and the kiln head sample roasting rate in the next hour or several hours.

[0031] For different CO concentrations in kiln tail exhaust gas and kiln head temperatures, the main parameter control operation standards are shown in Table 1 below.

[0032] Table 1 Process parameter values ​​of different embodiments

[0033] The operation adjustment method provided by the present invention is used in the actual production of the rotary kiln. The data of the above embodiments 1 to 7 show that the method of the present invention can adjust the combustion effect of the fuel under high dust conditions. Generally, after 2 to 3 hours of adjustment operation, the standard parameters can be met, so that the temperature of the kiln head of the rotary kiln is stabilized at 850±50°C, and the CO content in the exhaust gas at the kiln tail can be maintained at 5000±1000ppm; according to the above implementation effects, the daily output of a single rotary kiln is increased by 12.6%, the quality is improved by about 1.2%, and the coal saving rate of the rotary kiln is 5.1%.

[0034] When the kiln head temperature is higher than 900°C, the kiln head temperature is generally increased. When the designed capacity is reached, the parameters of Example 1 are gradually restored; under high dust conditions, the kiln head temperature will hardly increase due to poor combustion. This can also be seen in the working conditions of the above embodiment.

[0035] The above embodiments show that this operation method replaces the original on-site operation of increasing the secondary air volume, resulting in lower secondary air temperature and kiln head temperature, increased kiln head hood dust concentration, and greatly improved coal powder combustion conditions, and significantly improved the rotary kiln thermal system and calcination effect.

Claims

1. A method for improving fuel combustion efficiency under high dust conditions of a rotary kiln, characterized in that: By adjusting the oxygen-enriched content in the air volume of the primary fan and the coal conveying fan, combined with the control of coal powder fineness and coal powder moisture, the temperature at the kiln head of the rotary kiln is kept stable, the fuel combustion condition is always controlled in the best state, and the thermal system of the rotary kiln production process is stabilized; the state parameters controlled in this method are as follows: the CO content in the exhaust gas at the kiln tail is 5000±1000ppm, the kiln head temperature is 850±50℃; the percentage of coal powder fineness passing the 200-mesh sieve is 96±2%; the coal powder moisture content is 2±0.5%; the air-coal ratio standard is 7~9:

1.

2. The method for improving fuel combustion efficiency under high dust conditions of a rotary kiln according to claim 1, characterized in that: Includes the following: When the dust concentration of the rotary kiln is high and causes the CO content in the tail gas to be higher than 6000ppm, the oxygen enrichment content of the air supplied by the primary fan and the coal conveying fan shall be increased by 4%~6%; when the CO content in the kiln tail gas shows a downward trend and is lower than 4000ppm, the oxygen enrichment content of the air supplied by the primary fan and the coal conveying fan shall be reduced by 4%~6% to restore to the standard parameters, that is, the CO content in the kiln tail gas is 5000±1000ppm.

3. The method for improving fuel combustion efficiency under high dust conditions of a rotary kiln according to claim 1, characterized in that: Includes the following: When the dust concentration of the rotary kiln is high and causes the kiln head temperature to be lower than 800℃, increase the oxygen enrichment content of the primary fan and coal conveying fan by 5%; when the kiln head temperature is higher than 900℃, reduce the oxygen enrichment content of the primary fan and coal conveying fan by 5% to restore to the standard parameters, that is, maintain the kiln head temperature at 850±50℃.

4. The method for improving fuel combustion efficiency under high dust conditions of a rotary kiln according to claim 1, characterized in that: Includes the following: When the passing rate of coal powder fineness through 200 mesh sieve reaches more than 98%, reduce the speed of powder concentrator by 1%; when the passing rate of coal powder fineness through 200 mesh sieve is less than 94%, increase the speed of powder concentrator by 1% to restore to the standard parameters of coal grinding, and maintain the passing rate of coal powder fineness through 200 mesh sieve at 96±2%.

5. The method for improving fuel combustion efficiency under high dust conditions of a rotary kiln according to claim 1, characterized in that: Includes the following: When the moisture content of coal powder is higher than 2.5%, reduce the coal grinding rate by 2t / h and stabilize the mill outlet temperature; when the moisture content of coal powder is lower than 1.5%, increase the coal grinding rate by 2t / h and restore to the standard parameters of coal grinding, maintaining the air-coal ratio at 7~9:1.