Battery diaphragm black spot observation method

By curing the battery separator on the resin material and using grinding technology to reveal the black spot cross-section, combining epoxy resin AB glue and silicone mold, the problems of cumbersome steps and high cost in the existing technology are solved, and the efficiency of the black spot of the battery separator is achieved. Economic and accurate observation to help determine the cause of battery self-discharge.

CN118913851APending Publication Date: 2024-11-08JINGMEN YIWEI CHUANGNENG LITHIUM BATTERY CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411027143.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing battery separator black spot observation methods are cumbersome, costly, and easy to damage the observation cross-section, making it difficult to quickly and economically determine the cause of battery self-discharge.

Method used

The diaphragm with black dots is cured into the resin material, and the black dot cross-section is revealed layer by layer by layer by layer through grinding. The diaphragm is fixed using epoxy resin AB glue and silicone mold. Combined with sandpaper grinding and digital microscope observation, a clearer cross-section of metal foreign matter is achieved. observe.

Benefits of technology

The black spot observation process of battery separator is simplified, the cost is reduced, the observation efficiency and accuracy are improved, and the degree and reason of the battery self-discharge are quickly and economically.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118913851A_ABST
    Figure CN118913851A_ABST
Patent Text Reader

Abstract

The invention provides a method for observing black spots of a battery diaphragm. The method comprises the following steps: taking a diaphragm with black spots; curing the diaphragm in a resin material in a tiled manner to obtain a to-be-polished part; the to-be-polished part is polished, and the polishing condition is observed until it is observed that the sections of the polished black spots have the metal color; and observing the cross sections of the black spots. According to the method, the battery diaphragm with the black spots is cured in the resin material, and then the sections of the black spots are polished in a polishing manner, so that the conditions of the sections of the black spots can be observed more quickly and conveniently, and the color of metal foreign matters and the boundary condition of the diaphragm can be clearer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of batteries, and in particular to a method for observing black spots on battery separators. Background Art

[0002] The phenomenon that the battery automatically loses power when there is no load is called self-discharge. By observing the penetration depth and state of the metal foreign matter deposited on the diaphragm, it is possible to assist in determining the degree of battery self-discharge and the cause of its self-discharge.

[0003] In the related art, the method for observing the penetration depth and state of metal foreign matter deposited on the diaphragm is mostly the scanning electron microscope observation method, including: step 1, take the diaphragm of the abnormal battery and make a pre-cut surface near the black spot of the diaphragm; step 2, make a cut surface along the pre-cut surface by cutting with an ion beam, and spray gold on it; step 3, perform microscopic morphology test on the cut surface by scanning electron microscope to obtain the cross-sectional morphology of the black spot of the diaphragm. The observation method has cumbersome test steps, ion cutting and gold spraying lead to increased costs, and ion cutting is prone to generate local high temperature, thereby destroying the observation section. Summary of the invention

[0004] The embodiments of the present invention provide a method for observing black spots on battery separators, which can improve the technical problems of the existing methods for observing black spots on battery separators, such as complicated steps, high cost, and damage to the observation section.

[0005] An embodiment of the present invention provides a method for observing black spots on a battery separator, comprising:

[0006] Take the diaphragm with black spots;

[0007] Solidifying the diaphragm in a resin material in a flat state to obtain a workpiece to be polished;

[0008] Grinding the workpiece to be polished, and observing the polishing condition until it is observed that the cross section of the polished black spot has a metallic color;

[0009] The cross section of the black spot was observed.

[0010] In the embodiment of the present invention, by curing the battery separator with black spots in the resin material, and then grinding out the black spot cross section by grinding, the black spots can be revealed layer by layer, the black spot cross section can be observed more quickly and conveniently, and the color of the metal foreign matter and the separator boundary can be made clearer. The observation method is simple, economical, efficient and practical.

[0011] In one embodiment, taking out the separator with black spots includes: taking out the separator with black spots from an abnormal battery.

[0012] In the embodiment of the present invention, by observing and analyzing the separator with black spots of the abnormal battery, the degree of self-discharge and the cause of the self-discharge can be assisted in determining.

[0013] In one embodiment, the resin material is epoxy resin AB glue.

[0014] In an embodiment of the present invention, epoxy resin AB glue has the characteristics of high definition, high hardness and high transparency. Using it to cure the diaphragm can make the cured model more transparent, and has high toughness and high hardness, so that the diaphragm can be effectively fixed and the position of the black spots on the diaphragm can be observed conveniently. At the same time, epoxy resin AB glue has strong defoaming ability, fast solidification, and is easy to operate.

[0015] In one embodiment, the epoxy resin AB glue includes A glue and B glue, and the mass ratio of the A glue to the B glue is (2.5-3.5):1.

[0016] In the embodiment of the present invention, by controlling the mass ratio of A glue and B glue, the curing time of epoxy resin AB glue can be shortened and the curing hardness can be increased, thereby facilitating operation and observation.

[0017] In one embodiment, curing the diaphragm in a flat state in a resin material to obtain a workpiece to be polished includes:

[0018] Providing a mold with an opening, and adding the resin material in a fluid state into the mold through the opening;

[0019] After the resin material is semi-cured, the diaphragm is added into the mold from the opening in a flat state, and the resin material in a fluid state is continuously added into the mold from the opening until the diaphragm is wrapped;

[0020] The resin material wrapped with the diaphragm is cured to obtain the workpiece to be polished.

[0021] In the embodiment of the present invention, the diaphragm can be effectively fixed in the cured resin material by adding the fluid resin material twice. After the resin material previously added to the mold is semi-cured, the diaphragm is added to the mold, which can prevent the diaphragm from sliding on the resin material, thereby facilitating the curing of the diaphragm in the resin material and preventing the interface from being skewed due to the sliding of the diaphragm, thereby facilitating polishing and observation.

[0022] In one embodiment, the membrane having black spots comprises:

[0023] Provide a full diaphragm with black spots;

[0024] The area of ​​the diaphragm containing the black spots is cut to obtain a diaphragm section, and the area of ​​the diaphragm section is made smaller than the cross-sectional area of ​​the inner cavity of the mold.

[0025] In the embodiment of the present invention, by cutting off the diaphragm segment, the area of ​​the diaphragm segment can be reduced, thereby reducing the cross-sectional area of ​​the inner cavity of the mold, and further reducing the workload of grinding. By making the area of ​​the diaphragm segment smaller than the cross-sectional area of ​​the inner cavity of the mold, the diaphragm segment can be easily added to the mold in a flat state, which is beneficial to the fixation of the diaphragm.

[0026] In one embodiment, the mold is made of silicone.

[0027] In the embodiment of the present invention, a mold made of silicone material is used to facilitate demolding of the workpiece to be polished in the mold.

[0028] In one embodiment, the grinding of the workpiece to be grinded comprises: grinding the workpiece to be grinded along the thickness direction of the diaphragm; and / or

[0029] The polishing method is sandpaper polishing.

[0030] In the embodiment of the present invention, by grinding the part to be polished along the thickness direction of the diaphragm, the presentation effect of the black spot cross section can be improved. The fineness of sandpaper grinding is high, and the grinding accuracy can be effectively controlled, so that the black spot cross section with metallic color can be polished more accurately.

[0031] In one embodiment, the step of grinding the workpiece to be ground and observing the grinding condition until the cross section of the ground black spot is observed to have a metallic color comprises:

[0032] Performing a first grinding on the workpiece to be polished with a first sandpaper, and observing the grinding condition until the polished cross section is observed to reveal the color of the black spot;

[0033] The workpiece to be polished is subjected to a second polishing with a second sandpaper until it is observed that the cross section of the polished black spot has a metallic color, and the mesh number of the second sandpaper is greater than the mesh number of the first sandpaper.

[0034] In an embodiment of the present invention, the first grinding can quickly grind to a cross section where the color of the black spots is exposed, which serves as a sign that the cross section of the black spots with a metallic color is about to be polished out. At this time, replacing the second sandpaper with a larger mesh number for the second grinding can achieve finer grinding, thereby avoiding grinding away the black spots.

[0035] In one embodiment, the mesh number of the first sandpaper is 400-600 mesh.

[0036] In an embodiment of the present invention, by controlling the mesh size of the first sandpaper, excess solidified material can be quickly polished off, while controlling the polishing accuracy so that the color cross section with black spots exposed is effectively polished out, making it easier to observe the cross section of the diaphragm.

[0037] In one embodiment, the mesh number of the second sandpaper is ≥2000 meshes.

[0038] In the embodiment of the present invention, by controlling the mesh size of the second sandpaper, fine grinding of the black spots can be achieved, so that the cross section of the black spots with a metallic color can be effectively polished out, thereby avoiding grinding away the black spots.

[0039] In one embodiment, observing the grinding condition comprises: observing the grinding condition by a first observation device; and / or

[0040] The observing the cross section of the black spot includes: observing the cross section of the black spot by using a second observation device.

[0041] In one embodiment,

[0042] The first observation device is a digital microscope; and / or

[0043] The second observation device is a digital microscope.

[0044] In an embodiment of the present invention, observation through a digital microscope can make the cross-section of the black spots clearer, making it easier to observe the polishing conditions. The digital microscope can intuitively observe whether the black spots have passed through the diaphragm and the size and color of the black spots. From the color, it can be intuitively determined what kind of metal foreign matter has precipitated and caused the black spots to pass through the diaphragm. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative work.

[0046] Figure 1 1 is a schematic flow chart of a method for observing black spots on a battery separator provided by an embodiment of the present invention;

[0047] Figure 2 is a structural schematic diagram of a mold provided by an embodiment of the present invention;

[0048] Figure 3 This is a model diagram of an epoxy resin AB glue after curing provided by an embodiment of the present invention;

[0049] Figure 4This is an observation diagram of a cross section of a diaphragm provided by an embodiment of the present invention under a digital microscope. DETAILED DESCRIPTION

[0050] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present invention. In addition, it should be understood that the specific implementation methods described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention. In the present invention, unless otherwise specified, the directional words used, such as "upper" and "lower", generally refer to the upper and lower parts of the device in actual use or working state, specifically the drawing direction in the drawings; while "inside" and "outside" refer to the outline of the device.

[0051] See also Figure 1-4 , an embodiment of the present invention provides a method for observing black spots on a battery separator, comprising:

[0052] Take the diaphragm with black spots;

[0053] Solidifying the diaphragm in a resin material in a flat state to obtain a workpiece to be polished;

[0054] Grinding the workpiece to be polished, and observing the polishing condition until it is observed that the cross section of the polished black spot has a metallic color;

[0055] The cross section of the black spot was observed.

[0056] It can be understood that the diaphragm with black spots can be a whole diaphragm with black spots, or a diaphragm with black spots in a cut battery, which can be selected according to the size of the battery diaphragm and observation needs. The area of ​​the battery diaphragm cured in the resin material can be selected according to observation needs. The resin material can be selected with high definition, high hardness, high transparency, strong defoaming ability, and fast solidification, so as to facilitate the curing and observation of the diaphragm. The tool used for grinding can be selected according to needs, as long as it can not wear out the black spots and can remove the black spot cross-section with a metallic color (such as Figure 4 As shown) can be effectively polished out. Figure 4 As shown, the metal color on the cross section of the black spot has metallic luster and reflection under a microscope. The metal color on the cross section of the black spot presents different colors due to different precipitated metal elements, such as Figure 4 The metallic color is reddish brown.

[0057] In one embodiment, taking out the separator with black spots includes: taking out the separator with black spots from an abnormal battery.

[0058] It can be understood that black spots are generally produced in batteries with abnormal K values. Such batteries are usually at low voltage, and the reason is generally caused by the precipitation of metal foreign matter and the short circuit caused by contact with the positive and negative electrodes.

[0059] In one embodiment, before the diaphragm is solidified in the resin material in a flat state, the method further includes: physically cleaning the diaphragm. For example, anhydrous ethanol can be used to clean the diaphragm.

[0060] It can be understood that cleaning the diaphragm with anhydrous ethanol can remove the residual electrolyte on the diaphragm, thereby avoiding affecting the curing effect of the resin material.

[0061] In one embodiment, the resin material is epoxy resin AB glue.

[0062] In one embodiment, the epoxy resin AB glue includes glue A and glue B, and the mass ratio of glue A to glue B is (2.5-3.5): 1. For example, it can be 2.5: 1, 2.6: 1, 2.7: 1, 2.8: 1, 2.9: 1, 3.0: 1, 3.1: 1, 3.2: 1, 3.3: 1, 3.4: 1, 3.5: 1, etc.

[0063] like Figure 2 and Figure 3 As shown, in one embodiment, curing the diaphragm in a flat state in a resin material to obtain a workpiece to be polished includes:

[0064] Providing a mold with an opening, and adding the resin material in a fluid state into the mold through the opening;

[0065] After the resin material is semi-cured, the diaphragm is added into the mold from the opening in a flat state, and the resin material in a fluid state is continuously added into the mold from the opening until the diaphragm is wrapped;

[0066] The resin material wrapped with the diaphragm is cured to obtain the workpiece to be polished.

[0067] It can be understood that the amount of the fluid resin material added twice can be adjusted according to the size of the mold, as long as the diaphragm can be fixed in the solidified resin material. Semi-solidification of the resin material means that when the mold is picked up and gently shaken, it is observed that the resin material has no obvious flow phenomenon. For example, the resin material uses epoxy resin AB glue, and the semi-curing time is 4-6 minutes. The curing of the resin material means that the resin material has no fluidity and is completely solidified. For example, the resin material uses epoxy resin AB glue, and the curing time at room temperature is 22-26 hours. The shape of the mold cavity can be a regular geometric shape, such as a cuboid, a cube, a cylinder, or an irregular geometric shape.

[0068] In one embodiment, before adding the fluid resin material into the mold, the method further includes: cleaning the mold. For example, anhydrous ethanol may be used to clean the mold.

[0069] It can be understood that cleaning the mold with anhydrous ethanol can remove impurities on the mold, thereby avoiding affecting the curing effect of the resin material.

[0070] In one embodiment, the membrane having black spots comprises:

[0071] Provide a full diaphragm with black spots;

[0072] The area of ​​the diaphragm containing the black spots is cut to obtain a diaphragm section, and the area of ​​the diaphragm section is made smaller than the cross-sectional area of ​​the inner cavity of the mold.

[0073] It can be understood that when the area of ​​the entire diaphragm of the battery is large, the area of ​​the diaphragm containing black spots can be cut off for curing observation. When cutting off the area of ​​the diaphragm containing black spots from the entire diaphragm, cutting, pressing, etc. can be used, which is simple to operate. The size of the inner cavity cross-sectional area of ​​the mold can be selected according to the size of the black spot area, and the inner cavity cross-sectional area of ​​the mold needs to be larger than the area of ​​the black spot.

[0074] In one embodiment, the mold is made of silicone.

[0075] Understandably, silicone molds are softer and easier to demould.

[0076] In one embodiment, the polishing of the workpiece includes: polishing the workpiece along a thickness direction of the diaphragm.

[0077] It can be understood that the thickness direction of the diaphragm is the direction of metal precipitation. Grinding along the thickness direction can prevent the black spots from being worn away, and it is also beneficial to the presentation of the cross-section of the black spots for easy observation.

[0078] In one embodiment, the polishing method is sandpaper polishing.

[0079] It is understandable that grinding fluid can be added during grinding to improve the grinding effect.

[0080] In one embodiment, the step of grinding the workpiece to be ground and observing the grinding condition until the cross section of the ground black spot is observed to have a metallic color comprises:

[0081] Performing a first grinding on the workpiece to be polished with a first sandpaper, and observing the grinding condition until the polished cross section is observed to reveal the color of the black spot;

[0082] The workpiece to be polished is subjected to a second polishing with a second sandpaper until it is observed that the cross section of the polished black spot has a metallic color, and the mesh number of the second sandpaper is greater than the mesh number of the first sandpaper.

[0083] It can be understood that the color of the black spots revealed in the polished cross-section represents the surface polished to the black spots. Since the thickness of the diaphragm is relatively small, it means that the cross-section of the black spots will be polished to a metallic color, and more fine polishing is required at this time.

[0084] In one embodiment, the mesh number of the first sandpaper is 400-600 mesh.

[0085] In one embodiment, the mesh number of the second sandpaper is ≥2000 meshes.

[0086] In one embodiment, observing the grinding condition includes: observing the grinding condition through a first observation device.

[0087] It is understandable that due to the small size of the black spots, the first observation device needs to be a device with sufficient accuracy to clearly observe the black spots, so as to facilitate the judgment of the grinding condition.

[0088] In one embodiment, observing the cross section of the black spot includes: observing the cross section of the black spot by using a second observation device.

[0089] It is understandable that due to the small size of the black spots, the second observation device needs to be selected with sufficient accuracy to clearly observe the black spots, so as to facilitate the judgment of the penetration depth and state of the metal foreign matter on the diaphragm. In one embodiment, the first observation device is a digital microscope; and / or

[0090] The second observation device is a digital microscope.

[0091] It is understood that the second observation device and the first observation device can be the same device or different devices. Since the black spot size is small, it is necessary to use a high-precision device to observe and observe in order to judge the polishing condition.

[0092] The embodiments of the present invention are described in detail above. Specific examples are used herein to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core idea. At the same time, for those skilled in the art, according to the idea of ​​the present invention, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as a limitation on the present invention.

Claims

1. A method for observing black spots on battery separators. It is characterized in that include: Take the diaphragm with black spots; Solidifying the diaphragm in a resin material in a flat state to obtain a workpiece to be polished; Grinding the workpiece to be polished, and observing the polishing condition until it is observed that the cross section of the polished black spot has a metallic color; The cross section of the black spot was observed.

2. The method for observing black spots on battery separators according to claim 1, It is characterized in that Taking out the separator with black spots includes: taking out the separator with black spots from an abnormal battery; and / or The resin material is epoxy resin AB glue.

3. The method for observing black spots on battery separators according to claim 2, It is characterized in that The epoxy resin AB glue includes A glue and B glue, and the mass ratio of the A glue to the B glue is (2.5-3.5):

1.

4. The method for observing black spots on battery separators according to claim 2 or 3, It is characterized in that The step of curing the diaphragm in a flat state in a resin material to obtain a workpiece to be polished comprises: Providing a mold with an opening, and adding the resin material in a fluid state into the mold through the opening; After the resin material is semi-cured, the diaphragm is added into the mold from the opening in a flat state, and the resin material in a fluid state is continuously added into the mold from the opening until the diaphragm is wrapped; The resin material wrapped with the diaphragm is cured to obtain the workpiece to be polished.

5. The method for observing black spots on battery separators according to claim 4, It is characterized in that The diaphragm with black spots comprises: Provide a full diaphragm with black spots; The area of ​​the diaphragm containing the black spots is cut to obtain a diaphragm section, and the area of ​​the diaphragm section is made smaller than the cross-sectional area of ​​the inner cavity of the mold.

6. The method for observing black spots on battery separators according to claim 4 or 5, It is characterized in that The material of the mold is silicone.

7. The method for observing black spots on battery separators according to claim 1, It is characterized in that The grinding of the workpiece to be polished includes: grinding the workpiece to be polished along the thickness direction of the diaphragm; and / or The polishing method is sandpaper polishing.

8. The method for observing black spots on battery separators according to claim 7, It is characterized in that The step of grinding the workpiece to be ground and observing the grinding condition until the cross section of the ground black spot is observed to have a metallic color includes: Performing a first grinding on the workpiece to be polished with a first sandpaper, and observing the grinding condition until the polished cross section is observed to reveal the color of the black spot; The workpiece to be polished is subjected to a second polishing with a second sandpaper until it is observed that the cross section of the polished black spot has a metallic color, and the mesh number of the second sandpaper is greater than the mesh number of the first sandpaper.

9. The method for observing black spots on battery separators according to claim 7, It is characterized in that The mesh number of the first sandpaper is 400-600 mesh; and / or The mesh number of the second sandpaper is ≥2000 meshes.

10. The method for observing black spots on battery separators according to claim 1, It is characterized in that The observing the grinding condition includes: observing the grinding condition by a first observing device; and / or The observing the cross section of the black spot includes: observing the cross section of the black spot by using a second observation device.

11. The method for observing black spots on battery separators according to claim 10, It is characterized in that The first observation device is a digital microscope; and / or The second observation device is a digital microscope.

Citation Information

Cited By

  • Method for detecting corrosion defect points in lithium battery

    CN120778779A