Thin film structure for protecting laser with wavelength of 1064NM and preparation method of thin film structure

By forming SiO2 film on stainless steel foil and adding micro-convex structures, the temperature distribution and protection performance evaluation of laser protection films in the prior art is solved, and the reflectivity and protection time of the laser are improved, which is more effective. Laser protection effect.

CN118915200APending Publication Date: 2024-11-08YANGZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410972228.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The prior art is difficult to effectively protect the potential hazards of a wavelength of 1064NM laser to humans and equipment, and there is a lack of temperature distribution analysis and micro-bulge design for thin film structures to evaluate protective performance.

Method used

Stainless steel foil is used as the substrate to cover the SiO2 film and form a micro-convex structure on its surface. By controlling the thickness of the SiO2 coating and the interval of the micro-convex points, the reflectivity and protection time of the laser are improved, and a thin film with a protective wavelength of 1064NM laser is prepared. structure. The method includes coating the SiO2 suspension on the surface of the substrate, forming a SiO2 coating, and curing it by a CO2 laser to form a SiO2 film, and adding a micro-convex structure thereon.

Benefits of technology

Improve the reflectivity and protection time of the film against high-power density lasers, provide better protection design for space applications, has good economic and social benefits, and ensures parameter stability and micro-convex shape through simulation monitoring and inspection. appearance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118915200A_ABST
    Figure CN118915200A_ABST
Patent Text Reader

Abstract

The invention discloses a thin film structure for protecting laser with the wavelength of 1064NM and a preparation method of the thin film structure, and the preparation method is used for preparing the thin film structure for protecting the laser with the wavelength of 1064NM and comprises the following steps that the surface of a pretreated base material is coated with SiO2 turbid liquid to form a SiO2 coating; drying the base material, and forming a SiO2 film on the base material; micro convex points are added to the SiO2 coating, and a protective film structure is formed on the SiO2 thin film. According to the invention, the reflectivity of the film under the irradiation of laser with the wavelength of 1064nm can be effectively improved, the targeted radiation hardening design can be developed, and the requirements of the space protective film in the fields of spaceflight and nuclear industry can be met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a thin film structure for protecting a laser with a wavelength of 1064 nm and a preparation method thereof, belonging to the technical field of laser protection. Background Art

[0002] Laser protective film is a specially designed material used to absorb, scatter or reflect the radiation generated by the laser, thereby protecting sensitive devices from damage by laser radiation. Laser protective film is usually composed of multiple layers of composite materials with specific optical properties that can selectively absorb or reflect laser beams of specific wavelengths.

[0003] Laser is a high-energy beam with powerful energy and highly concentrated characteristics. Therefore, in the wide application of industrial, medical and scientific research fields, laser radiation may cause damage to human tissues such as eyes and skin, and even cause serious consequences. In order to protect people's health and safety, laser protection technology has been rapidly developed and applied. Laser protection technology mainly includes the design and manufacture of laser protection products and the safety management of laser radiation. Laser protection products such as laser goggles and laser protective clothing use special materials and structures to effectively block laser radiation and reduce its harm to the human body. With the rapid development of lasers, high-energy lasers are often used in scientific research, but these lasers may pose potential dangers to equipment and personnel, which urgently requires the research and development of laser protection technology. Therefore, solving the problem of laser radiation is of great significance to modern society. Summary of the invention

[0004] The technical problem to be solved by the present invention is to overcome the defects of the prior art, provide a thin film structure and a preparation method for protecting the laser of wavelength 1064NM, observe the temperature distribution in the simulation results, find out the places where the film is prone to damage, and focus on them in the subsequent design; on the other hand, since micro-bumps are added to the film, the temperature changes are observed and analyzed by changing the size and gap of the bumps and the time when the protective film is damaged, so as to evaluate the protective performance of the film and provide technical guarantee for its space application protection design.

[0005] Preferably, the present invention provides a thin film structure for protecting lasers of wavelength 1064NM, including a substrate, a SiO2 thin film, a protective film structure and a micro-bump structure, wherein the substrate is covered with a SiO2 thin film, and the SiO2 thin film is covered with a protective film structure or a micro-bump structure.

[0006] Preferably, the substrate is a stainless steel foil.

[0007] Preferably, a thin film structure for protecting a laser with a wavelength of 1064 nm and a preparation method thereof, used to prepare the thin film structure for protecting a laser with a wavelength of 1064 nm, comprises the following steps:

[0008] Coating a SiO2 suspension on the surface of the pretreated substrate to form a SiO2 coating;

[0009] Drying the substrate to form a SiO2 film on the substrate;

[0010] Micro bumps are added to the SiO2 coating to form a protective film structure on the SiO2 film.

[0011] Preferably, coating the pretreated substrate surface with a SiO2 suspension to form a SiO2 coating comprises:

[0012] The SiO2 content in the SiO2 suspension coated on the surface of the pretreated substrate is 8-12 wt %, and the solvent of the SiO2 suspension is ethanol;

[0013] Dropping the SiO2 suspension on the center of the substrate, and rotating the substrate at a speed of 100-200 rpm for a first preset time after the SiO2 suspension completely infiltrates the surface of the substrate, so that the SiO2 suspension is evenly distributed on the surface of the substrate;

[0014] The substrate is rotated at 400-600 rpm for a second preset time to shake off excess SiO2 suspension on the substrate to form a SiO2 coating.

[0015] Preferably, the substrate is dried to form a SiO2 film on the substrate, comprising:

[0016] The CO2 laser is repeatedly used to scan the entire surface of the SiO2 coating of the substrate, and the temperature at the SiO2 coating is controlled to be 400-450° C., so that the SiO2 coating is solidified to form a SiO2 film of a first thickness threshold;

[0017] Preferably, micro-bumps are added to the SiO2 coating to form a protective film structure on the SiO2 film, comprising:

[0018] Laminating a SiO2 wafer on the surface of the SiO2 film, or placing the SiO2 wafer in a reaction chamber so that the SiO2 film grows on the surface of the SiO2 wafer;

[0019] Applying photoresist on the SiO2 coating or SiO2 wafer surface, covering the micro-bump template on the photoresist, and irradiating the photoresist with ultraviolet light according to a preset time;

[0020] The photoresist which is not exposed to the ultraviolet light is removed by a developer to expose the surface of the SiO2 film;

[0021] Etching is performed on the exposed surface of the SiO2 film to form a micro-bump structure;

[0022] Clean the SiO2 film surface and micro-bump structure, remove residual photoresist and etching products, and form a protective film structure.

[0023] Preferably, the substrate is pretreated, comprising:

[0024] Clean the substrate surface using an ethanol solution;

[0025] Use deionized water and dry gas to dry the substrate;

[0026] Check the substrate for defects, if not obtain the treated substrate.

[0027] The beneficial effects achieved by the present invention are:

[0028] The present invention proposes a thin film structure for protecting lasers with a wavelength of 1064nm. The reflectivity of the protective film to the laser is improved by optimizing the bump spacing, and the protection time of the film to high-power density lasers is increased, thereby protecting the internal sensitive devices and providing technical guarantee for the protection design of its space application, which has good economic and social benefits.

[0029] The invention effectively controls the thickness of the SiO2 film layer and uniformly coats SiO2 to form a SiO2 film with good quality by controlling the rotation speed when coating SiO2.

[0030] The present invention ensures the stability and consistency of parameters during the preparation process and monitors and checks the morphology of the micro-convex point structure in real time, thereby improving the shape of the micro-convex points on the surface of the film. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly illustrate the technical solution of the present application, the drawings required for use in the embodiments are briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without any creative work.

[0032] Figure 1 is a flow chart of some embodiments of the present application;

[0033] Figure 2 is a simulation diagram of the protective film structure in some embodiments of the present application;

[0034] Figure 3 is a simulation diagram of the protective film structure in some embodiments of the present application;

[0035] Figure 4 is a graph showing the variation of reflectivity with the number of convex points in some embodiments of the present application; DETAILED DESCRIPTION

[0036] To facilitate the technical solution of the application, some concepts involved in the application are first explained below.

[0037] It should be noted that if there are directional indications (such as up, down, left, right, front, back, etc.) in the embodiments of the present invention, they are only used to explain the relative position relationship and movement status of the various components under a certain specific posture. If the specific posture changes, the directional indication will also change accordingly.

[0038] In addition, if the descriptions of "first" and "second" etc. are involved in the present invention, they are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the ability of ordinary technicians in the field to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such a combination of technical solutions does not exist and is not within the scope of protection required by the present invention.

[0039] See also Figure 1 The present application provides a thin film structure for protecting a laser with a wavelength of 1064 nm, and the preparation process steps thereof are as follows:

[0040] Step 1: Prepare the substrate stainless steel foil: Select a stainless steel foil with a diameter of 40mm and a thickness of 0.7mm as the substrate and ensure that the substrate size meets the requirements and the surface flatness is good; use an ethanol solution with a concentration of 70% to 90% to clean the surface of the stainless steel foil, and ensure that there is no dust, grease or other impurities on the surface. Apply the ethanol solution evenly on the surface of the stainless steel foil, and then wipe it gently with a clean cloth to ensure that it can fully contact and clean the surface. Then use deionized water and dry gas (nitrogen) to blow dry the surface of the stainless steel foil. Deionized water can remove detergent residues and any impurities on the surface, while dry gas can accelerate the drying process of the surface and avoid water stains; visually inspect the surface of the stainless steel foil to ensure that there are no obvious scratches, dents or other defects on the surface;

[0041] The reason for selecting an ethanol solution with a concentration of 70% to 90% in step 1 is that ethanol is a universal cleaning agent with good compatibility with stainless steel surfaces, will not introduce new pollutants, and will not damage the surface, so an ethanol solution with a concentration of 70% to 90% is selected.

[0042] Step 2: Prepare SiO2 coating: Coat the surface of stainless steel foil with SiO2 suspension to form SiO2 coating. The specific operation is as follows: select SiO2 suspension with a content of 8-12wt% and ethanol as the solvent of SiO2 suspension; drop SiO2 suspension on the center of stainless steel foil, wait for the SiO2 suspension to completely soak the surface of stainless steel foil, rotate the stainless steel foil at a speed of 100-200rpm for about 60s (first preset time), and then rotate the stainless steel foil at 400-600rpm for about 90s (second preset time). Evenly distribute the SiO2 suspension on the surface at a low speed during spin coating, and then throw out the excess SiO2 suspension at a high speed;

[0043] Step 3: Dry the stainless steel foil; the specific operation is: use a CO2 laser to scan the entire SiO2 coating surface of the stainless steel foil, control the temperature of the SiO2 coating to 400-450°C, and solidify the SiO2 coating to form a SiO2 film with a thickness of 200nm. Since SiO2 absorbs lasers with a wavelength of 10064nm well, a CO2 laser is used to scan the entire surface with a laser. When scanning the entire piece, the scanning is performed in a galvanometer manner. The output power of the CO2 laser is 60-100W. By controlling the output power of the CO2 laser, the temperature of the SiO2 coating during scanning can be effectively controlled to 400-450°C. The parameters of CO2 laser scanning are: spot width 0.15-0.25mm; line filling spacing 0.04-0.06mm. Repeat the above steps to make the thickness of the SiO2 coating 0.3mm (first thickness threshold);

[0044] Step 4: Add micro-bumps; the specific operation is: a SiO2 wafer with the same size as the SiO2 film is bonded to the surface of the SiO2 film by chemical vapor deposition (CVD) technology. This can be achieved by placing the SiO2 wafer in a reaction chamber, controlling the flow rate and temperature of the gas mixture, and growing the SiO2 wafer on the surface of the SiO2 film; then a photoresist is applied on the SiO2 coating or the surface of the SiO2 wafer, and a micro-bump template is prepared according to the desired micro-bump structure and covered on the photoresist. The photoresist is irradiated with ultraviolet light, and the photoresist is exposed to the area of ​​the template pattern through optical reaction to form the desired structure. A suitable developer is used to remove the photoresist that is not exposed to ultraviolet light, exposing the surface of the SiO2 film. The exposed SiO2 film surface is etched to form a micro-bump structure; the SiO2 film surface and the micro-bump structure are cleaned, and the residual photoresist and etching products are removed, and finally a protective film structure is formed.

[0045] Step 5: Use the built-in modeling tools in COMSOL software to construct a 3D geometric structure, such as Figure 2As shown in the figure, the simulated model size is a film with a diameter of 40mm and a thickness of 1mm. There are two layers, made of stainless steel and SiO2. The lowest layer of the film is a 0.7mm stainless steel foil, followed by a 0.3mm SiO2 layer on top, and the environment is vacuum. According to the simulation model, the three-dimensional geometric structure, regional material and geometric body material are determined to build a simulation model.

[0046] Step 6: Next, perform optical simulation. The specific simulation process is as follows: first, select the geometric optics module in the physical field; then, according to the given laser parameters, set the laser point and power and other parameters to simulate the laser beam; then, after the settings are completed, perform research and calculations, extract the ray power gop.Q and the initial ray power gop.relg1.Q0 in the equation view, and calculate the protective film reflectivity α according to the laser reflectivity formula (1-1):

[0047] α=(gop.relg1.Q0-gop.Q) / gop.relg1.Q0#(1-1)

[0048] Step 7: Further thermal simulation is performed. The specific simulation process is as follows: first, since the energy distribution of the laser is Gaussian, the laser can be equivalent to a Gaussian heat source, and the equivalent is performed according to the given laser power and spot size using formula (1-2);

[0049]

[0050] where p laser is the laser power, r spot is the spot size, r focus is the focal length; then, according to the optical calculation of the absorptivity of the protective film, the heat absorbed by the irradiated surface of the protective film can be equivalent to (1-α)*Flux; secondly, in space, there is no thermal convection phenomenon, only the surface radiates to the environment, so the radiation coefficient of the surface to the environment is set in the boundary conditions; finally, after the settings are completed, simulation is performed to obtain the thermal field distribution of the protective film;

[0051] Step 8: Optimization of the simulation model of the protective film: First, change the thickness and radius of the initial model, and obtain the optical properties and thermal field distribution after laser radiation through the above steps to determine the protective performance of the film. Then add micro-bumps to the surface of the initial model. Its material parameters are SiO2, and its size is a semicircle with a radius of 0.5mm. Arrange 2 linear arrays at a spacing of 10mm, and array 360° in a circle at a spacing of 10°. Through the above steps, compare the difference in protective performance with the initial model. Secondly, change the spacing of the micro-bumps, linear array 20 at a spacing of 1um, and array 360° in a circle at a spacing of 10°. Compare the difference in protective performance between the two models and the initial model, thereby proving that the optimized model has improved laser protection.

[0052] The various embodiments in this specification are described in a progressive manner, and the same or similar parts between the various embodiments can be referenced to each other, and each embodiment focuses on the differences from other embodiments.

[0053] Those skilled in the art will readily appreciate other embodiments of the present invention after considering the specification and practicing the invention invented herein. This application is intended to cover any variations, uses or adaptations of the present invention that follow the general principles of the present invention and include common knowledge or customary techniques in the art that are not invented by the present invention. The specification and examples are to be considered exemplary only, and the true scope and spirit of the present invention are indicated by the following claims.

[0054] Finally, a few points should be explained: First, in the description of this application, it should be noted that, unless otherwise specified and limited, the terms "installed", "connected", "connected", and "matched" should be understood in a broad sense, which may refer to mechanical connection or electrical connection, or internal communication between two elements, or direct connection. "upper", "lower", "left", "right", etc. are only used to indicate relative positional relationships. When the absolute position of the object being described changes, the relative positional relationship may change;

[0055] Secondly: In the drawings of the embodiments of the present invention, only the structures involved in the embodiments of the present invention are involved, and other structures can refer to the general design; the above specific implementation methods further explain the purpose, technical solutions and beneficial effects of the present application in detail. It should be understood that the above are only specific implementation methods of the present application and are not used to limit the protection scope of the present application. Any modifications, equivalent substitutions, improvements, etc. made on the basis of the technical solutions of the present application should be included in the protection scope of the present application.

Claims

1. A thin film structure for protecting lasers with a wavelength of 1064NM, characterized in that: The invention comprises a substrate, a SiO2 film, a protective film structure and a micro-convex point structure. The substrate is covered with a SiO2 film, and the SiO2 film is covered with a protective film structure or a micro-convex point structure.

2. The thin film structure for protecting a laser with a wavelength of 1064 nm according to claim 1, characterized in that: The substrate is stainless steel foil.

3. A thin film structure for protecting lasers with a wavelength of 1064NM and a preparation method thereof, characterized in that: The method for preparing a thin film structure for protecting a laser with a wavelength of 1064 nm as claimed in claim 1 or 2 comprises the following steps: Coating a SiO2 suspension on the surface of the pretreated substrate to form a SiO2 coating; Drying the substrate to form a SiO2 film on the substrate; Micro bumps are added to the SiO2 coating to form a protective film structure on the SiO2 film.

4. The thin film structure for protecting a laser with a wavelength of 1064 nm and the preparation method thereof according to claim 3, characterized in that: Coating the SiO2 suspension on the surface of the pretreated substrate to form a SiO2 coating, including: The content of SiO2 in the SiO2 suspension coated on the surface of the pretreated substrate is 8-12wt%, and the solvent of the SiO2 suspension is ethanol; Dropping the SiO2 suspension on the center of the substrate, and rotating the substrate at a speed of 100-200 rpm for a first preset time after the SiO2 suspension completely infiltrates the surface of the substrate, so that the SiO2 suspension is evenly distributed on the surface of the substrate; The substrate is rotated at 400-600 rpm for a second preset time to shake off excess SiO2 suspension on the substrate to form a SiO2 coating.

5. The thin film structure for protecting laser of wavelength 1064NM and the preparation method thereof according to claim 3, characterized in that: The substrate is dried to form a SiO2 film on the substrate, including: The CO2 laser is repeatedly used to scan the entire surface of the SiO2 coating of the substrate, and the temperature at the SiO2 coating is controlled to be 400-450° C., so that the SiO2 coating is solidified to form a SiO2 film of a first thickness threshold.

6. The thin film structure for protecting a laser with a wavelength of 1064 nm and the preparation method thereof according to claim 3, characterized in that: Add micro bumps to the SiO2 coating to form a protective film structure on the SiO2 film, including: Laminating a SiO2 wafer on the surface of the SiO2 film, or placing the SiO2 wafer in a reaction chamber so that the SiO2 film grows on the surface of the SiO2 wafer; Applying photoresist on the SiO2 coating or SiO2 wafer surface, covering the micro-bump template on the photoresist, and irradiating the photoresist with ultraviolet light according to a preset time; The photoresist which is not exposed to the ultraviolet light is removed by a developer to expose the surface of the SiO2 film; Etching is performed on the exposed surface of the SiO2 film to form a micro-bump structure; Clean the SiO2 film surface and micro-bump structure, remove residual photoresist and etching products, and form a protective film structure.

7. The thin film structure for protecting laser of wavelength 1064NM and the preparation method thereof according to claim 3, characterized in that: Pre-treat the substrate, including: Clean the substrate surface using an ethanol solution; Use deionized water and dry gas to dry the substrate; Check the substrate for defects, if not obtain the treated substrate.