Super-hydrophobic porous radiation refrigeration film as well as preparation method and application thereof

By using a superhydrophobic porous radiation refrigeration film made of polydimethylsiloxane and tetra-like zinc oxide whiskers, the problem of reducing radiation refrigeration efficiency caused by dust accumulation on the surface of the film is solved, and high-efficiency radiation cooling and self-cleaning performance are achieved , suitable for building materials and other scenarios.

CN118994711APending Publication Date: 2024-11-22CHINA THREE GORGES UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410952837.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The thin film surface of early radiation refrigeration technology is prone to accumulation of dust, resulting in a decrease in radiation refrigeration efficiency and limited application scenarios.

Method used

Superhydrophobic porous radiation refrigeration film composed of polydimethylsiloxane and tetra-shaped zinc oxide whiskers is made by a simple preparation method, with high whiteness, good radiation cooling effect and self-cleaning performance, suitable for scale .

Benefits of technology

It achieves efficient radiation cooling effect under various conditions, improves the reflectivity and emissivity of the film, and has self-cleaning ability, and is suitable for building materials and other scenarios.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994711A_ABST
    Figure CN118994711A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of materials, and particularly discloses a super-hydrophobic porous radiation refrigeration film and a preparation method and application thereof.The preparation method comprises the following steps that S1, polydimethylsiloxane and n-hexane are evenly mixed to prepare a solution, tetrapod-like zinc oxide whiskers are added into the solution to be evenly mixed to prepare dispersion liquid; adding a curing agent into the dispersion, and uniformly mixing to obtain a blade coating stock solution; and S2, blade-coating the blade-coating stock solution obtained in the step S1 on a substrate, and drying to obtain the super-hydrophobic porous radiation refrigeration film. The preparation method is simple, and the prepared film is high in whiteness, good in radiation cooling effect and low in cost, has self-cleaning performance and can be applied on a large scale.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of material technology, relates to the problems of self-cleaning and radiation cooling, and specifically relates to a super-hydrophobic porous radiation cooling film and a preparation method and application thereof. Background Art

[0002] Passive daytime radiation cooling technology is an energy-free autonomous cooling technology proposed in recent years. This technology relies on high reflectivity in the sunlight (0-2.5μm) band and high emissivity in the atmospheric window (8-13μm) band, so that as much sunlight and heat as possible can be radiated out of the space to be cooled to achieve the purpose of cooling.

[0003] In the early development of radiation cooling technology, many radiation cooling technologies were relatively simple, with only the function of cooling and cooling. The surface cleanliness of the radiation cooling film was required to be high. Once used for a long time, a lot of dust would accumulate, which greatly reduced the efficiency of radiation cooling. Therefore, its application scenarios were relatively narrow. In order to solve such problems, we need to find solutions. Summary of the invention

[0004] The invention provides a super-hydrophobic porous radiation refrigeration film and a preparation method and application thereof. The preparation method is simple, the prepared film has high whiteness, good radiation cooling effect, low cost, self-cleaning performance, and can be applied on a large scale.

[0005] The technical solution of the present invention is to provide a method for preparing a super-hydrophobic porous radiative refrigeration film, comprising the following steps: S1: polydimethylsiloxane and n-hexane are mixed evenly to form a solution, and tetrapod-shaped zinc oxide whiskers are added to the solution and mixed evenly to form a dispersion; a curing agent is added to the dispersion and mixed evenly to obtain a scraping stock solution; S2, applying the coating solution obtained in S1 onto the substrate by scraping, and obtaining a super-hydrophobic porous radiative cooling film after drying.

[0006] Furthermore, the mass ratio of polydimethylsiloxane, n-hexane, tetrapod-shaped zinc oxide whiskers and curing agent in S1 is 10:8~12:6.67~23.33:0.8~1.2.

[0007] Furthermore, the mass ratio of polydimethylsiloxane to tetrapod-shaped zinc oxide whiskers is 10:15.

[0008] Furthermore, the four-needle zinc oxide whisker in S1 has a core, from which four needle-like crystals extend radially, each needle-like body is a single crystal microfiber, the angle between any two needle-like bodies is 109°, the central body diameter of the whisker is 0.7~1.4μm, and the length is 10~50μm.

[0009] Furthermore, the curing agent is Sylgard 184 silicone rubber curing agent.

[0010] Furthermore, the polydimethylsiloxane in S1 is added dropwise to n-hexane and stirred and mixed for 15 to 20 minutes; the tetrapod-shaped zinc oxide whisker is added to the solution and stirred and mixed for 10 to 15 minutes; and the curing agent is added and stirred and mixed for 10 to 15 minutes.

[0011] Furthermore, the base material in S2 is an acrylic board; the drying temperature is 70-90° C., and the drying time is 90 min-150 min.

[0012] Furthermore, the film thickness is 300-600 μm, preferably 400 μm.

[0013] The invention also relates to a super-hydrophobic porous radiation refrigeration film obtained by the preparation method.

[0014] The present invention also relates to the application of the super-hydrophobic porous radiation cooling film in building materials, such as building exterior walls, container houses, etc.

[0015] The present invention has the following beneficial effects: The super-hydrophobic porous radiative cooling film of the present invention is composed of polydimethylsiloxane and tetrapod-shaped zinc oxide whiskers. The super-hydrophobic porous radiative cooling film has high reflectivity in the visible light band, high emissivity in the atmospheric window band, and self-cleaning ability, and can be used under various conditions. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 This is a real picture of the super-hydrophobic porous radiative cooling film doped with different mass ratios of four-needle zinc oxide whiskers in Example 1. Figure 1 AD are white porous refrigeration films of the same thickness doped with tetrapod-shaped zinc oxide whiskers in a mass ratio of 40 wt %, 50 wt %, 60 wt %, and 70 wt %, respectively.

[0017] Figure 2 This is a reflectivity curve of the super-hydrophobic porous radiative cooling film doped with different mass proportions of four-needle zinc oxide whiskers in Example 1.

[0018] Figure 3 This is a graph showing the emissivity of the super-hydrophobic porous radiative cooling film doped with different mass proportions of four-needle zinc oxide whiskers in Example 1.

[0019] Figure 4 This is a comparative film reflectivity curve of 60wt%, 400μm common crystalline zinc oxide and polydimethylsiloxane in Example 1.

[0020] Figure 5This is a comparative film emissivity curve of 60wt%, 400μm common crystalline zinc oxide and polydimethylsiloxane in Example 1.

[0021] Figure 6 This is a reflectivity curve of the super-hydrophobic porous radiative cooling film of four-needle zinc oxide whiskers and polydimethylsiloxane of different thicknesses in Example 2.

[0022] Figure 7 This is an emissivity curve of a super-hydrophobic porous radiative cooling film of four-needle zinc oxide whiskers and polydimethylsiloxane of different thicknesses in Example 2.

[0023] Figure 8 This is a measurement diagram of the hydrophobic angle of different tetrapod-shaped zinc oxide whisker mass ratios doped in Example 3. Figure 8 AD are the hydrophobic angles of the film surfaces of the same thickness with the tetrapod-shaped ZnO whiskers incorporated in the amounts of 40 wt %, 50 wt %, 60 wt %, and 70 wt %, respectively.

[0024] Fig. 9 This is the hydrophobic angle measurement diagram of 60wt% ordinary crystalline zinc oxide in Example 3.

[0025] Fig.10 This is a self-cleaning test diagram of a super-hydrophobic porous radiative cooling film doped with 60 wt % of tetrapod-shaped zinc oxide whiskers and having a thickness of 400 μm in Example 3. Fig.10 AD is the self-cleaning test of polydimethylsiloxane and tetrapod-shaped zinc oxide whisker film. Fig.10 Medium EH is a self-cleaning test of pure polydimethylsiloxane.

[0026] Fig.11 This is an electron microscope image of a super-hydrophobic porous radiation cooling film of Example 4 doped with four-needle zinc oxide whiskers in a mass ratio of 60 wt % and a thickness of 400 μm.

[0027] Fig.12 The temperature drop test device for the outdoor super-hydrophobic porous radiative cooling film of Example 5 is as follows: Fig.12 A is the test site for the test box. Fig.12 B is a schematic diagram of the temperature drop test box.

[0028] Fig.13 This is the temperature drop test curve and solar irradiance of the super-hydrophobic porous radiative cooling film of Example 5 placed outdoors.

[0029] Fig.14 This is a temperature difference test curve of the super-hydrophobic porous radiative cooling film of Example 5 placed outdoors.

[0030] Fig.15For Example 6, the application study of super-hydrophobic porous radiative cooling film in simulated architecture, Fig.15 A is a simulated building test site. Fig.15 B is the temperature drop test curve and solar irradiance.

[0031] Fig.16 This is the temperature difference test curve of Example 6 when the super-hydrophobic porous radiative cooling film is placed in a simulated building. DETAILED DESCRIPTION

[0032] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to the following embodiments.

[0033] Example 1 The present invention conducts experiments on super-hydrophobic porous radiative cooling films of polydimethylsiloxane doped with different mass ratios of tetrapod-shaped zinc oxide whiskers. The specific preparation method is as follows: (1) According to the mass ratio of polydimethylsiloxane to n-hexane of 10:10, weigh 4 g of polydimethylsiloxane and 4 g of n-hexane into a weighing bottle and stir magnetically for 15 min to fully mix them.

[0034] (2) According to the mass ratio of tetrapod-shaped zinc oxide whisker to polydimethylsiloxane of 6.67-23.33:10, weigh 2.7 g (40 wt %), 4 g (50 wt %), 6 g (60 wt %) and 9.4 g (70 wt %) of tetrapod-shaped zinc oxide whisker, respectively, add them to the mixed solution in step (1), continue magnetic stirring for 10 min to make it evenly stirred, and obtain a white scraping stock solution.

[0035] (3) According to the mass ratio of Sylgard 184 curing agent to polydimethylsiloxane being 1:10, 0.4 g of Sylgard 184 curing agent was weighed and added to the mixed solution in step (2), and magnetic stirring was continued for 10 min to make it uniform, thereby obtaining a white scraping stock solution.

[0036] (4) The white coating solution in step (3) was dripped onto the acrylic substrate using a rubber-tipped dropper to obtain a smooth coating by coating, and finally placed in an oven at 80°C for 2 hours to obtain a super-hydrophobic porous radiative cooling film with different doping ratios of four-needle zinc oxide whiskers. Figure 1 The surface conditions of the cooling films with different doping ratios are different. When the doping ratio of the four-needle zinc oxide whiskers is 40 wt% ( Figure 1When the doping ratio is 60 wt % ( Figure 1 C) when the film surface is flat, white, and no obvious agglomeration occurs. The doping ratio is 70wt% ( Figure 1 D) of the film does not change much. Figure 2 , 3 It can be found that the reflectivity and emissivity will also have corresponding differences with different doping ratios. The higher the doping ratio, the higher the reflectivity and emissivity will be. When the doping ratio is 60 wt%, the film has a low average reflectivity in the solar spectrum band: 0.3-0.5μ m because it absorbs ultraviolet light. The average reflectivity of 0.5-1.5μ m is 0.95, which is about 633 times that of pure polydimethylsiloxane (0.0015). In the mid-infrared band: the average emissivity of 2.5-22μ m is 0.98, which is about 1.1 times that of pure polydimethylsiloxane (0.9). Continuing to increase the doping ratio, the average reflectivity and emissivity will also increase relatively slowly, and the flexibility of the film will deteriorate. Considering the cost factor, 60wt% is preferred. In order to verify the effect of needle-shaped zinc oxide on the radiation cooling effect, we also measured the reflection and emissivity of 60wt% of ordinary crystalline zinc oxide (Aladdin, 98%, 500g) ( Figure 4 , 5), the average reflectance and emissivity in the 0.5-1.5μm and 2.5-22μm bands are 0.85 and 0.96, respectively, which are lower than those of the four-needle zinc oxide whisker doped.

[0037] Example 2 The present invention experiments on super-hydrophobic porous radiative cooling films of tetrapod-shaped zinc oxide whiskers of different thicknesses and polydimethylsiloxane. The specific preparation method is as follows: (1) According to the mass ratio of polydimethylsiloxane to n-hexane of 10:10, weigh 4 g of polydimethylsiloxane and 4 g of n-hexane into a weighing bottle and stir magnetically for 15 min to fully mix them.

[0038] (2) Based on the ratio of tetrapod-shaped zinc oxide whiskers to the total weight of polydimethylsiloxane and tetrapod-shaped zinc oxide whiskers, 6 g of tetrapod-shaped zinc oxide whiskers were weighed and added to the mixed solution in step (1), and magnetically stirred for 10 min to fully disperse the mixture.

[0039] (3) According to the mass ratio of Sylgard 184 curing agent to polydimethylsiloxane being 1:10, 0.4 g of Sylgard 184 curing agent was weighed and added to the mixed solution in step (2), and magnetic stirring was continued for 10 min to make it uniform, thereby obtaining a white scraping stock solution.

[0040] (4) The white coating solution in step (3) was dripped onto the acrylic substrate using a rubber-tipped dropper, and the thickness of the scraper was adjusted to 300, 400, 500, and 600 μm, respectively. The coating was applied at a uniform speed to obtain a smooth coating, and finally placed in an oven at 80°C for 2 h to obtain a super-hydrophobic porous radiative cooling film of four-needle zinc oxide whiskers and polydimethylsiloxane of different thicknesses. Figure 6 , 7 The reflectivity and emissivity of radiation cooling films of different thicknesses are inconsistent. The thicker the thickness, the higher the corresponding reflectivity and emissivity. The average reflectivity and emissivity of 400μm in the 0.5-1.5μm and 2.5-22μm bands are both over 0.9. Considering the cost issue, the preferred film thickness is 400μm, which is more suitable for large-scale industrial production.

[0041] Example 3 Effect of superhydrophobic porous radiative cooling films doped with polydimethylsiloxane with different mass ratios of tetrapod-shaped zinc oxide whiskers on their self-cleaning properties.

[0042] The preparation method is the same as that of Example 1. The doping ratios of the four-needle zinc oxide whiskers in step (2) are selected as 40 wt %, 50 wt %, 60 wt %, and 70 wt %, respectively. The super-hydrophobic porous radiative cooling films with different doping ratios are placed in an instrument for measuring the hydrophobic angle to measure their hydrophobic angles, such as Figure 8 As shown. The hydrophobic angle of 40 wt % is 124.75°, the hydrophobic angle of 50 wt % is 147.75°, the hydrophobic angle of 60 wt % is 153.25°, and the hydrophobic angle of 70 wt % is 154°. At the same time, we also measured the hydrophobic angle of ordinary crystalline zinc oxide ( Fig. 9 ) is 105.5°, and there is no super-hydrophobic property. According to Examples 1 and 2, 60 wt% of the super-hydrophobic porous radiative cooling film was selected for self-cleaning test. Fig.10 AD, using mud and water to mix and stir to get muddy water, using a rubber-tipped dropper to absorb the muddy water, and dropping about 0.05 ml of the muddy water onto the film each time (a drop of rainwater is about 0.05 ml), it can be found that the 60wt% super-hydrophobic porous radiation cooling film can bounce the muddy water into the culture dish without causing pollution, and has good self-cleaning performance. Fig.10 EH, 0wt% pure polydimethylsiloxane film cannot bounce the muddy water into the culture dish, but adheres to the film, and does not have good self-cleaning performance.

[0043] Example 4 The surface morphology of the super-hydrophobic porous radiative cooling film was studied when the mass ratio of the doped tetrapod-shaped zinc oxide whiskers was 60 wt% and the thickness was 400 μm. The specific preparation method is as follows: (1) According to the mass ratio of polydimethylsiloxane to n-hexane of 10:10, weigh 3 g of polydimethylsiloxane and 3 g of n-hexane into a weighing bottle and stir magnetically for 15 min to fully mix them.

[0044] (2) Based on the ratio of tetrapod-shaped zinc oxide whiskers to the total weight of polydimethylsiloxane and tetrapod-shaped zinc oxide whiskers, 4.5 g of tetrapod-shaped zinc oxide whiskers were weighed and added to the mixed solution in step (1), and magnetically stirred for 10 min to fully disperse the mixture.

[0045] (3) According to the mass ratio of Sylgard 184 curing agent to polydimethylsiloxane being 1:10, 0.3 g of Sylgard 184 curing agent was weighed and added to the mixed solution in step (2), and magnetic stirring was continued for 10 min to make it uniform, thereby obtaining a white scraping stock solution.

[0046] (4) The white coating solution in step (3) is applied to the acrylic substrate using a rubber-tipped dropper, the thickness of the scraper is adjusted to 400 μm, and a smooth coating is obtained by coating at a uniform speed. Finally, the coating is placed in an oven at 80°C and dried for 2 h to obtain a super-hydrophobic porous radiative cooling film of tetrapod-shaped zinc oxide whiskers and polydimethylsiloxane. Fig.11 A, it can be clearly observed that the surface microstructure of the radiation cooling film is composed of a large number of micro-nano pores and needles, and the distribution is relatively uniform. Fig.11 B. The same is true for the side, and it can also be inferred that its porous structure is connected.

[0047] Example 5 The outdoor cooling performance of the superhydrophobic porous radiative cooling film was studied when the mass ratio of doped tetrapod-shaped zinc oxide whiskers was 60 wt% and the thickness was 400 μm.

[0048] The preparation method of the super-hydrophobic porous radiative cooling film is the same as that of Example 4. Pure polydimethylsiloxane film (preparation method is the same as that of Example 1, except that tetrapod-shaped zinc oxide whiskers are not added) and commercial white paint (Muyaju Sanitary Ware Co., Ltd., 350g of metal anti-rust white paint) were selected as the control group. The specifications of the experimental temperature measuring box are as follows Fig.12 B, the length and width of the box are the same, 16×16cm, the size of the cavity is 5×5cm, the interior is polyethylene foam, and the outer wall is wrapped with thin aluminum paper to play a role in insulation and reduce the impact of heat convection. On March 11, 2024, a temperature drop experiment was conducted on the roof of the simulated building of the Three Gorges University in Yichang City. The experimental site is as follows Fig.12As shown in A. The experimental film is placed at the cavity opening and sealed with PE film to reduce the influence of external wind, humidity and heat flow. The thermal couple is connected to the bottom of the base to measure and record the temperature data. The solar irradiance meter is placed next to the experimental box to record the solar irradiance intensity during the measurement period of the day. The average solar irradiance during the period of 11:00-14:00 on that day was 677W / m 2 The average temperature in the target sample cavity is about 28°C, and the average temperature of the acrylic substrate is 38°C. Compared with the temperature of the acrylic substrate, the target sample temperature can reach a maximum temperature drop of 11.9°C, and the average temperature drop is about 10°C, which is higher than the temperature difference of commercial white paint and pure polydimethylsiloxane film. Fig.13 , 14 shown.

[0049] Example 6 When the super-hydrophobic porous radiative cooling film is doped with four-needle zinc oxide whiskers at a mass ratio of 60 wt% and its thickness is 400 μm, the cooling and cooling performance of outdoor buildings is simulated.

[0050] The preparation method of the super-hydrophobic porous radiative cooling film is the same as that of Example 4. The size of the simulated house building is set to be 10 cm long, 8 cm wide, and 8-15 cm high. The target coating is a white house (the outer surface of the house is wrapped with a super-hydrophobic porous radiative cooling film with a thickness of 400 μm), and the other is a bare house. On March 20, 2024, a temperature drop experiment was conducted on the simulated roof of the Three Gorges University in Yichang City. The experimental site is as follows Fig.15 As shown in A. The average solar irradiance during the period from 11:30 to 14:30 on that day was 693W / m 2 , the average temperature of the target coating room is 31.9℃, and the average temperature of the bare room is about 40.6℃. Compared with the temperature of the target coating room and the bare room, the maximum temperature difference can reach 9.9℃, and the average temperature difference is about 8.7℃. Fig.15 B, as shown in 16. In summary, the radiant cooling film has a good radiant cooling effect in the simulated building.

[0051] The above embodiments describe the preferred implementation of the present invention, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for preparing a super-hydrophobic porous radiative cooling film, characterized in that: The following steps are involved: S1: polydimethylsiloxane and n-hexane are mixed evenly to form a solution, tetrapod-shaped zinc oxide whiskers are added to the solution and mixed evenly to form a dispersion; a curing agent is added to the dispersion and mixed evenly to obtain a scraping stock solution; S2, applying the coating solution obtained in S1 onto the substrate by scraping, and obtaining a super-hydrophobic porous radiative cooling film after drying.

2. The preparation method according to claim 1, characterized in that: The mass ratio of polydimethylsiloxane, n-hexane, tetrapod-shaped zinc oxide whiskers and curing agent in S1 is 10:8~12:6.67~23.33:0.8~1.

2.

3. The preparation method according to claim 2, characterized in that: The mass ratio of polydimethylsiloxane to tetrapod-shaped zinc oxide whiskers is 10:

15.

4. The preparation method according to claim 1, characterized in that: The four-needle zinc oxide whisker in S1 has a core, from which four needle-like crystals extend radially. Each needle-like body is a single crystal microfiber. The angle between any two needle-like bodies is 109°. The diameter of the central body of the whisker is 0.7 ~ 1.4μm, and the length is 10 ~ 50μm.

5. The preparation method according to claim 1, characterized in that: The curing agent is Sylgard 184 silicone rubber curing agent.

6. The preparation method according to claim 1, characterized in that: The polydimethylsiloxane in S1 was added dropwise to n-hexane and stirred for 15-20 min; Add the tetrapod-shaped zinc oxide whiskers to the solution and stir and mix for 10 to 15 minutes; add the curing agent and stir and mix for 10 to 15 minutes.

7. The preparation method according to claim 1, characterized in that: The base material in S2 is acrylic board; the drying temperature is 70~90℃, and the drying time is 90min~150min.

8. The preparation method according to any one of claims 1 to 7, characterized in that: The film thickness is 300-600 μm; preferably 400 μm.

9. A super-hydrophobic porous radiative cooling film obtained according to the preparation method according to any one of claims 1 to 8.

10. Use of the super-hydrophobic porous radiative cooling film according to claim 9 in building materials.

Citation Information

Cited By

  • Cross-linked network structure radiation refrigeration film and preparation method and application thereof

    CN119931141A

  • Application of calcium sulfate whisker in radiation refrigeration material

    CN122563382A