Method for manufacturing photomask and photomask

By forming different exposure areas in photomask manufacturing, the problem of photomask overlap error and poor pattern is solved, efficient and fine photomask manufacturing is achieved, and design and production costs are reduced.

CN118915373APending Publication Date: 2024-11-08SK ELECTRONICS CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411261938.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2020-10-14
Filing Date
2021-04-26
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

When existing photomasks form semi-transmissive areas and light-shielding areas with different optical characteristics, overlap errors are prone to occur, resulting in poor patterning and increased manufacturing labor hours. The pattern design needs to consider overlap margins, which increases the designer's work. Burdens and costs.

Method used

A photomask manufacturing method is adopted, in which a semi-transmissive film, an intermediate film and an upper film are formed on a transmissive substrate, and regions with different exposure amounts are formed by exposure, and resist is selectively removed, and an etching process is performed to form a semi-transmissive Areas and shading areas ensure the fineness and freedom of the pattern.

Benefits of technology

It effectively suppresses overlap errors during exposure, shortens manufacturing time, reduces designer work burden and cost, and at the same time realizes the manufacturing of multi-grayscale and phase-shift masks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118915373A_ABST
    Figure CN118915373A_ABST
Patent Text Reader

Abstract

The present invention provides a photomask manufacturing method and a photomask capable of forming patterns having different optical characteristics in a manner of suppressing occurrence of coincidence errors during exposure. In the photomask manufacturing method, a photomask blank having a semi-transmissive film, an intermediate film, and an upper layer film on a transmissive substrate is prepared, a photoresist film formed on the upper layer film is exposed, and a first region, a second region, and a third region having different exposure amounts are formed. Thereafter, the first region is selectively removed, and the upper layer film is etched. Thereafter, the second region is selectively removed, the semi-transmissive film is etched, and the upper layer film and the intermediate film are etched. And then, removing the third region.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for manufacturing a photomask and the photomask. Background Art

[0002] In the process of manufacturing electronic devices such as flat panel displays, photomasks are used. Conventionally, binary masks having a transmission portion and a light-shielding portion are used as photomasks. However, in recent years, in order to form fine patterns, phase-shift masks having, for example, a light-shielding film and a phase-shift film, or multi-grayscale photomasks that can reduce the number of manufacturing steps for electronic devices are sometimes used. Such photomasks have multiple patterns with different optical properties on a transparent substrate, and multiple pattern drawing (exposure) steps are required to form these patterns.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2017-76146

[0006] Patent Document 2: Japanese Patent Application Publication No. 2013-134435 Summary of the invention

[0007] Problems to be solved by the invention

[0008] In the case of forming a semi-transmissive region and a light-shielding region having different optical characteristics, it is necessary to perform exposure (drawing) processing of the photoresist for the formation of each pattern, which increases the number of manufacturing man-hours. Furthermore, each time each pattern is drawn, the photomask substrate is placed on an exposure (drawing) device for exposure processing, so there is a possibility of overlap error (alignment deviation). Therefore, it is necessary to perform pattern configuration taking into account the overlap margin, and it may become impossible to obtain a fine pattern.

[0009] Patent document 1 discloses a method for avoiding the occurrence of superposition errors. Patent document 1 discloses a method of performing a first etching on a first resist pattern formed by preliminary development on a mask, and then performing a second etching after the edge of the first resist pattern is retreated by performing additional development, thereby forming a phase shift film symmetrically on both sides of the light shielding portion. However, in the second etching, although the occurrence of superposition errors in the exposure device can be prevented, the pattern size is naturally limited because of the use of unnecessary light during exposure, which makes it unstable. In addition, the pattern that can be formed is also limited.

[0010] Patent document 2 discloses a method for forming a pattern formed of different materials. Patent document 2 discloses a method of forming a resist pattern on a stack of a lower film and an upper film formed of different materials, selectively wet-etching the upper film and the lower film using the resist pattern as a mask, and then side-etching the upper film using the resist pattern as a mask. Patent document 2 uses a resist pattern formed by a single drawing process, and although it can prevent the occurrence of overlap errors, it becomes unstable due to the use of unnecessary light during exposure, and the pattern size is naturally limited.

[0011] In view of the above-mentioned problems, an object of the present invention is to provide a method for manufacturing a photomask capable of forming a pattern having different optical characteristics so as to suppress the occurrence of overlay errors during exposure.

[0012] Technical solutions to the problem

[0013] A. First method

[0014] The method for manufacturing a photomask of the present invention is characterized by comprising:

[0015] A step of preparing a photomask blank, wherein the photomask blank has a semi-transmissive film on a transmissive substrate, an intermediate film on the semi-transmissive film, and an upper film on the intermediate film;

[0016] forming a resist film on the upper film;

[0017] An exposure process of exposing the resist film to form a first region, a second region, and a third region with different exposure amounts;

[0018] a first resist removal step of selectively removing the first region;

[0019] A first etching step of etching the upper film;

[0020] a second resist removal step of selectively removing the second region;

[0021] A second etching step of etching the semi-transmissive film, the upper film, and the intermediate film; and

[0022] A step of removing the third area.

[0023] Furthermore, the method for manufacturing a photomask of the present invention is characterized in that:

[0024] The semi-transmissive film and the upper film are formed of the same material.

[0025] Furthermore, the method for manufacturing a photomask of the present invention is characterized in that:

[0026] In the exposure step, the exposure amount of the first region is greater than the exposure amount of the second region, and the exposure amount of the third region is zero.

[0027] By adopting such a photomask manufacturing method, a pattern composed of a semi-transparent film and a pattern composed of a semi-transparent film, an intermediate film and an upper film can be formed in a manner that suppresses the occurrence of overlay errors during exposure, which can help shorten the photomask manufacturing process.

[0028] Furthermore, pattern design can be performed without considering the overlap margin, fine patterning can be performed, and the workload of the designer can be reduced.

[0029] Furthermore, it can contribute to cost reduction in the manufacturing process.

[0030] Furthermore, the method for manufacturing a photomask of the present invention is characterized in that:

[0031] The semi-transmissive film is a half-tone film.

[0032] By adopting such a method for manufacturing a photomask, a halftone mask as a multi-tone mask can be manufactured.

[0033] The method for manufacturing a photomask of the present invention is characterized in that:

[0034] The semi-transmissive film is a phase shift film.

[0035] By adopting such a method for manufacturing a photomask, a phase shift mask can be manufactured.

[0036] B. Second method

[0037] The method for manufacturing a photomask of the present invention is characterized by comprising:

[0038] A step of preparing a photomask blank, wherein the photomask blank has a lower film on a transmissive substrate and an upper film on the lower film;

[0039] forming a resist film on the upper film;

[0040] An exposure process of exposing the resist film to form a first region, a second region, and a third region with different exposure amounts;

[0041] a first resist removal step of selectively removing the first region;

[0042] A first etching step of etching the upper film and the lower film;

[0043] a second resist removal step of selectively removing the second region;

[0044] A second etching step of etching the upper film; and

[0045] A step of removing the third area.

[0046] Furthermore, the method for manufacturing a photomask of the present invention is characterized in that:

[0047] The lower film and the upper film are formed of different materials.

[0048] Furthermore, the method for manufacturing a photomask of the present invention is characterized in that:

[0049] In the exposure step, the exposure amount of the first region is greater than the exposure amount of the second region, and the exposure amount of the third region is zero.

[0050] By adopting such a method for manufacturing a photomask, a pattern composed of a lower film and a pattern composed of a lower film and an upper film can be formed in a manner that suppresses the occurrence of an overlap error during exposure. Pattern design can be performed without considering the overlap margin, fine patterning can be performed, and the workload of the designer can be reduced.

[0051] Furthermore, it can contribute to cost reduction in the manufacturing process.

[0052] Furthermore, the method for manufacturing a photomask of the present invention is characterized in that:

[0053] The lower film is a halftone film.

[0054] By adopting such a method for manufacturing a photomask, a halftone mask as a multi-tone mask can be manufactured.

[0055] Furthermore, the method for manufacturing a photomask of the present invention is characterized in that:

[0056] The lower film is a phase shift film.

[0057] By adopting such a method for manufacturing a photomask, a phase shift mask can be manufactured.

[0058] Effects of the Invention

[0059] According to the first and second aspects, in any case, it is possible to provide a method for manufacturing a photomask capable of forming a pattern having different optical characteristics while suppressing occurrence of overlay errors during exposure. BRIEF DESCRIPTION OF THE DRAWINGS

[0060] Figure 1 It is a cross-sectional view showing the main manufacturing steps of a photomask.

[0061] Figure 2 It is a cross-sectional view showing the main manufacturing steps of a photomask.

[0062] Figure 3This is a SEM photograph showing a cross section of a photoresist film.

[0063] Figure 4 It is a cross-sectional view showing the main manufacturing steps of a photomask.

[0064] Figure 5 It is a cross-sectional view showing the main manufacturing steps of the photomask according to the second embodiment.

[0065] Figure 6 It is a cross-sectional view showing the main manufacturing steps of the photomask according to the second embodiment.

[0066] Figure 7 It is a cross-sectional view showing the main manufacturing steps of the photomask according to the first embodiment.

[0067] Figure 8 It is a cross-sectional view showing the main manufacturing steps of the photomask according to the first embodiment.

[0068] Fig. 9 This is a SEM photograph showing a cross section of a photoresist film.

[0069] Fig.10 It is a cross-sectional view showing the main manufacturing steps of the photomask according to the first embodiment.

[0070] Fig.11 It is a cross-sectional view showing the main manufacturing steps of the photomask according to the second embodiment.

[0071] Fig.12 It is a cross-sectional view showing the main manufacturing steps of the photomask according to the second embodiment. DETAILED DESCRIPTION

[0072] Hereinafter, the embodiments of the present invention will be described with reference to the accompanying drawings. However, the following embodiments are not to be interpreted restrictively in the determination of the gist of the present invention. In addition, the same reference numerals are given to the same or similar components, and the description is omitted.

[0073] (Implementation Method 1)

[0074] Figure 1 , Figure 2 1 and 2 are cross-sectional views showing main manufacturing steps of the photomask 100 according to the first embodiment.

[0075] Hereinafter, a method for manufacturing the photomask 100 will be described with reference to the drawings.

[0076] (Film forming process: photomask blank preparation process)

[0077] like Figure 1As shown in (a), a transmissive substrate 1 such as synthetic quartz glass is prepared, and a semi-transmissive functional film 2 (semi-transmissive film) formed of a known material such as a Cr-based metal compound, a Si-based compound, or a metal silicide is formed on the transmissive substrate 1 by, for example, sputtering or evaporation.

[0078] Here, the transmissive substrate 1 has a transmittance of 90 to 100% (90%≤transmittance≤100%) with respect to representative wavelengths (eg, i-line, h-line, g-line) included in exposure light used in a photolithography process using the photomask 100 .

[0079] Furthermore, semi-transmissive means that the transmittance at a representative wavelength included in the exposure light is lower than the transmittance of the transmissive substrate 1 and higher than the transmittance of the laminated structure film described later.

[0080] The exposure light may be, for example, an i-line, an h-line, or a g-line, or may be a mixed light containing at least two of these. The exposure light is not limited to these lights.

[0081] The functional film 2 can be used as a halftone film or a phase shift film.

[0082] For example, when the functional film 2 is used as a halftone film, the transmittance of the functional film 2 is set to 10 to 70% (10% ≤ transmittance ≤ 70%) for the representative wavelength. In addition, the phase shift amount may be set small (approximately 0[°], for example, 0 to 20[°]).

[0083] In addition, for example, when the functional film 2 is used as a phase shift film, the transmittance of the functional film 2 is set to 3 to 15% (3% ≤ transmittance ≤ 15%) with respect to the representative wavelength contained in the exposure light, and the phase shift amount is set to 180° (160° ≤ phase shift amount ≤ 200°), and it is further preferably set to 170° ≤ phase shift amount ≤ 190°.

[0084] The optical properties of the functional film 2 as a halftone film and a phase shift film can be realized by adjusting the composition and the film thickness, for example.

[0085] Next, the etching stopper film 3 (intermediate film 3 ) is formed (for example, with a film thickness of 1 [nm] to 20 [nm]) by sputtering, vapor deposition or the like.

[0086] Next, the light shielding film 4 (upper layer film 4 ) is formed (for example, with a film thickness of 50 [nm] to 100 [nm]) by sputtering, vapor deposition or the like.

[0087] As described later, the etching stopper film 3 is formed of a material having etching characteristics different from those of the light shielding film 4 (upper layer film 4 ) and the functional film 2 (having resistance).

[0088] In addition, if the laminated film composed of the functional film 2, the etching stopper film 3 and the light shielding film 4 has a light shielding property, it is not necessary to make the light shielding film 4 (upper film 4) a single layer of the light shielding film having a light shielding property. From this point of view, the material (component) and the film thickness of the light shielding film 4 can be adjusted. The transmittance of the representative wavelength of this laminated film is, for example, 1% or less. In other words, by adjusting the material (component) and the film thickness of the light shielding film 4 in the laminated region of the functional film 2, the etching stopper film 3 and the light shielding film 4, the optical density OD value can be 3.0 or more.

[0089] Hereinafter, a stacked structure in which the functional film 2, the etching stopper film 3, and the light shielding film 4 are formed on the transmissive substrate 1 is referred to as a photomask blank.

[0090] A plurality of photomask blanks having the above structure may be prepared in advance and stored. When a customer places an order, the photomask blanks having the above structure prepared in advance can be used to shorten the production period.

[0091] (Photoresist Formation Process)

[0092] Then, if Figure 1 As shown in (b) of FIG. 8 , a (photo) resist film 5 is formed on the light shielding film 4 by coating, spraying or the like.

[0093] (Exposure process)

[0094] Then, if Figure 1 As shown in (c), the photomask blank is placed on an exposure (drawing) device such as a laser drawing device (placed on an exposure stage in the exposure device), and the resist film 5 is exposed.

[0095] At this time, three regions with different exposure doses, namely, a high-dose region 5 c (first region), a low-dose region 5 b (second region), and an unexposed region 5 a (third region) are formed in the resist film 5 .

[0096] Here, the unexposed area 5a is an unexposed area, that is, an area with an exposure amount of 0, the low-dose area 5b is an area exposed with a relatively lower exposure amount than the high-dose area, and the high-dose area 5c is an area exposed with a relatively higher exposure amount than the low-dose area.

[0097] The drawing method using the exposure device is not limited to laser drawing, and exposure using, for example, an electron beam may be used.

[0098] More specifically, the high dose in the high dose region is an exposure amount that is greater than the exposure amount required to dissolve the resist when the resist is removed by the first development step described later. In contrast, the low dose in the low dose region is an exposure amount that is such that the resist is not removed by the first development step described later and remains, but is removed by the second development step. For example, based on the high dose required in the first development step, the exposure amount is in the range of 5% to 90% of the high dose.

[0099] The low dose can be appropriately set within the above range, but of course, the processing time of the second development step needs to be considered.

[0100] In addition, for the sake of simplicity, the high-dose area 5c of the resist film 5 is sometimes referred to as the "high-dose area 5c", the low-dose area 5b of the resist film 5 is sometimes referred to as the "low-dose area 5b", and the unexposed area 5a of the resist film 5 is sometimes referred to as the "unexposed area 5a".

[0101] The low-dose region 5b and the high-dose region 5c can be formed without removing (taking out) the transmissive substrate 1 from the exposure device. For example, the regions corresponding to the low-dose region 5b and the regions corresponding to the high-dose region 5c can be formed by exposing them by scanning the laser beam in a manner to obtain a first exposure amount and a second exposure amount, respectively.

[0102] In addition, the area corresponding to the low-dose area 5b and the high-dose area 5c may be exposed by scanning the laser in a manner to obtain the first exposure amount, and then, the area corresponding to the high-dose area 5c may be exposed by additionally scanning the laser in a manner to obtain the second exposure amount. The exposure amount is averaged by multiple laser irradiations, thereby improving the uniformity of the exposure amount of the high-dose area 5c. In addition, when the low-dose area 5b and the high-dose area 5c are connected, the uniformity of the exposure amount of the boundary area can also be improved.

[0103] Since the exposure process of the low-dose region 5 b and the high-dose region 5 c is performed without removing the photomask blank from the exposure apparatus, it is possible to suppress the occurrence of overlay errors (deviations) between these regions (patterns).

[0104] (First Development (Resist Removal) Step)

[0105] Then, if Figure 1 As shown in (d) of FIG. 8 , in the first development step, only the resist film 5 in the high-dose region 5 c is selectively removed by a developer, and the resist film 5 is patterned.

[0106] As described later, since the dissolution characteristics of the developer of the resist film 5 depend on the exposure amount (dose), the exposed resist film 5 can be selectively removed in sequence according to the exposure amount. In the first development step, by performing development (using dissolution of the developer) under development conditions where the dissolution rate of the high-dose region 5c is very high (for example, several times or even more than one order of magnitude) compared to the dissolution rate of the unexposed region 5a and the low-dose region 5b, only the high-dose region 5c is selectively removed.

[0107] In addition, if Figure 1 As shown in (d), the resist film thickness of the low-dose region 5b is thinner than the resist film thickness of the unexposed region 5a.

[0108] (First Etching Step)

[0109] Then, if Figure 2 As shown in (a), the light shielding film 4 is etched by wet etching or dry etching using the patterned resist film 5, i.e., the unexposed area 5a and the low-dose area 5b, as an etching mask. By making the light shielding film 4 and the etching stopper film 3 use different materials, the light shielding film 4 on the etching stopper film 3 can be selectively etched using an etchant (chemical solution or gas) that does not etch the etching stopper film 3. As a result, the etching stopper film 3 and the functional film 2 thereunder are not etched, but remain on the transmissive substrate 1.

[0110] In this step, since the functional film 2 whose surface is covered with the etching stopper film 3 is not etched, the functional film 2 and the light shielding film 4 can be formed using the same material.

[0111] In this case, the same film forming device or the same film forming material (sputtering target, vapor deposition material) can be used in the film forming process of the functional film 2 and the light-shielding film 4. In addition, the same etching device or the same etching agent can be used in the etching process of the functional film 2 and the light-shielding film 4. Therefore, production management becomes easy, which helps to reduce manufacturing costs.

[0112] Then, if Figure 2 As shown in (b), the etching stopper film 3 is etched by wet etching or dry etching using the resist film 5 in the unexposed area 5a and the low-dose area 5b as an etching mask. By making the functional film 2 and the etching stopper film 3 use different materials, the etching stopper film 3 on the functional film 2 can be selectively etched using an etchant (chemical solution or gas) that does not etch the functional film 2. As a result, the functional film 2 is not etched but remains on the transmissive substrate 1.

[0113] (Second Development (Resist Removal) Step)

[0114] Then, if Figure 2 As shown in (c), in the second development step, the resist film 5 is selectively removed only in the low-dose region 5b by a developer, and the resist film 5 is patterned. In this step, only the unexposed region 5a remains on the light shielding film 4.

[0115] The reason why the resist film 5 with different exposure amounts can be removed sequentially according to the exposure amount as shown in the first development step and the second development step is that the dissolution rate depends nonlinearly on the development conditions (time, etc.) The area with different exposure amounts can be selectively removed sequentially by utilizing the characteristic that the change point of the dissolution rate change (increase) depends on the exposure amount.

[0116] In the second development step, development (dissolution) can be performed under development conditions where the dissolution rate of the low-dose region 5 b is much higher than the dissolution rate of the unexposed region 5 a , and only the low-dose region 5 b can be selectively removed.

[0117] Furthermore, by using this method, three or more different patterns of the resist film 5 can be obtained.

[0118] (Second Etching Process)

[0119] Then, if Figure 2 As shown in (d), the functional film 2 is etched away by wet etching or dry etching, and the light shielding film 4 is etched away by wet etching or dry etching using the resist film 5 in the unexposed area 5a as an etching mask. In the area where the functional film 2 is etched, the transmissive substrate 1 is exposed.

[0120] Since the functional film 2 and the light shielding film 4 are formed of the same material, the functional film 2 and the light shielding film 4 can be etched simultaneously using the same etchant.

[0121] Thereafter, the etching stopper film 3 is removed by etching using a wet etching method or a dry etching method.

[0122] Thereafter, the resist film 5 in the unexposed region 5 a is removed by an ashing method or immersion in a resist stripping solution (third resist removal step).

[0123] Through the above process, a photomask 100 can be obtained, which includes a semi-transmissive area 6 formed by a functional film 2, a shading area 7 formed by a stack of layers including the functional film 2 as a lower film, an etching stop film 3 as an intermediate film, and a shading film 4 as an upper film, and a transmissive area 8 exposing the transmissive substrate 1.

[0124] The photomask 100 functions as a multi-tone halftone mask when the above-mentioned halftone film is used as the functional film 2 , and functions as a phase shift mask when the above-mentioned phase shift film is used as the functional film 2 .

[0125] In addition, you can also Figure 2 In the step (b), after the etching stopper film 3 on the functional film 2 is selectively etched, the functional film 2 is further etched.

[0126] However, in this case, if Figure 2 In the second etching step shown in (d), if the light shielding film 4 is etched by isotropic etching such as wet etching, the functional film 2 is also etched, and the amount of side etching of the functional film 2 increases.

[0127] exist Figure 2 In the step (b) shown in FIG. 1 , by etching only the light shielding film 4 and the etching stopper film 3 and leaving the functional film 2, the Figure 2 As a result, the patterning controllability of the functional film 2 can be improved.

[0128] Figure 3 This is a SEM photograph showing the cross-sectional shape of the photoresist. Figure 3 (a) shows the cross-sectional shape of the resist film 5 after the first development step. Figure 3 (b) shows the cross-sectional shape of the resist film 5 after the second development step.

[0129] like Figure 3 As shown in (a) of FIG. 5 , in the boundary portion where the unexposed region 5 a and the low-dose region 5 b meet, the cross section of the resist film 5 may have a gently tapered shape.

[0130] However, if Figure 3 As shown in (b), after the second development step, the cross section of the resist film 5 in the unexposed area 5a has a steep shape. Figure 1 The resist film 5 in the low-dose region 5 b determined in the exposure step shown in (c) is selectively removed in the second development step.

[0131] If the resist film 5 is uniformly dissolved in the second developing step, the cross section of the resist film 5 in the unexposed area 5a cannot be obtained. Figure 3 A steep shape as shown in (b).

[0132] When the side wall of the resist film 5 in the thick unexposed region 5 a is tapered, the pattern width varies, making it difficult to form a fine pattern.

[0133] In particular, the film thickness of the resist film 5 in the unexposed region 5a is thicker than that in the low-dose region 5b, so the taper angle of the cross section of the unexposed region 5a has a greater influence on the pattern accuracy formed on the photomask 100. However, by controlling the exposure amount to optically determine the boundary between the low-dose region 5b and the unexposed region 5a, the side shape of the resist film 5 in the unexposed region 5a after the second development step is as follows: Figure 3 As a result, fine patterning can be achieved by photolithography using the present photomask 100 .

[0134] In addition, Figure 1 , Figure 2 , an example is shown in which the semi-transmissive region 6 and the light-shielding region 7 are in contact with each other. However, since the shape of the photoresist film 5 can be optically determined in the exposure step, the photoresist film 5 can be patterned into a desired shape.

[0135] For example, it is also possible to Figure 4 As shown in (c) of FIG. 1 , the semi-transmissive region 6 and the light-shielding region 7 are formed to be spaced apart from each other. Figure 4 As shown in (a), the resist film 5 is exposed by an exposure (drawing) device so that the unexposed area 5a and the low-dose area 5b are spaced apart from each other, and then as shown in Figure 4 As shown in (b) of FIG. 1 , by the first development step, the resist film 5 of the unexposed region 5 a and the resist film 5 of the low-dose region 5 b which are spaced apart from each other are obtained.

[0136] Afterwards, you can also Figure 2 In the process shown, the semi-transmissive region 6 and the light shielding region 7 are formed at a distance from each other. Therefore, the degree of freedom in pattern design of the photomask 100 is greatly improved compared with the method disclosed in Patent Document 1.

[0137] Furthermore, a pattern arrangement in which a pattern in which the semi-transmissive region 6 and the light-shielding region 7 are spaced apart from each other and a pattern in which the semi-transmissive region 6 and the light-shielding region 7 are adjacent to each other may be performed.

[0138] (Implementation Method 2)

[0139] The photomask 100 can also be viewed by referring to Figure 5 and Figure 6 The following manufacturing process is described.

[0140] like Figure 5 As shown in (a) of FIG. 1 , a semi-transmissive functional film 2 (semi-transmissive film) made of a metal compound, for example, a Cr compound, is formed on a transmissive substrate 1 by sputtering, vapor deposition or the like.

[0141] As described above, the functional film 2 can be used as a halftone film or a phase shift film.

[0142] Next, the light shielding film 41 is formed on the functional film 2 by sputtering, vapor deposition or the like.

[0143] The light shielding film 41 is formed of a metal (or a compound thereof) of a different type from the metal of the metal compound constituting the functional film 2. For example, the functional film 2 may be a Cr compound and the light shielding film 41 may be a Ni film.

[0144] The film thickness of the formed light shielding film 41 is set so that the optical density (OD value) can be equal to or greater than 3. For example, when Ni is used as the light shielding film 41, the film thickness can be set to, for example, 100 [nm].

[0145] Next, an anti-reflection film 9 formed of a metal compound is formed on the light-shielding film 41 by a sputtering method, an evaporation method, or the like. The film thickness of the anti-reflection film 9 can be, for example, 2 to 5 [nm]. The anti-reflection film 9 is formed of a metal compound, such as a metal oxide, a metal nitride, or a metal oxynitride. The metal of the metal compound forming the anti-reflection film 9 and the metal of the metal compound forming the functional film 2 are the same type of metal. That is, the metal component forming the functional film 2 and the metal component forming the anti-reflection film 9 are composed of the same metal element. For example, when the functional film 2 is composed of a compound containing Cr, the anti-reflection film 9 is also formed of a compound containing Cr.

[0146] In addition, as the Cr compound, for example, Cr oxide, Cr nitride, or Cr oxynitride can be used.

[0147] Next, a (photo) resist film 5 is formed on the antireflection film 9 by a coating method, a spray coating method, or the like.

[0148] Thus, on the transmissive substrate 1, the functional film 2, the light shielding film 41, the antireflection film 9, and the resist film 5 are formed in this order.

[0149] Then, if Figure 5 As shown in (b), by Figure 1 In the same process as the process shown in (c) and (d), the resist film 5 is patterned to form two regions with different exposure doses, namely, a low-dose region 5b (second region) and an unexposed region 5a (third region).

[0150] The anti-reflection film 9 can reduce unnecessary reflection (halation, etc.) of exposure light during exposure of the resist film 5 , thereby improving the patterning accuracy of the resist film 5 .

[0151] Then, if Figure 5As shown in (c), the anti-reflection film 9 is selectively etched relative to the light shielding film 41 by wet etching or dry etching using the low-dose region 5b (second region) and the unexposed region 5a (third region) of the resist film 5 as masks.

[0152] As described above, the shading film 41 is formed of a metal of a different type from the metal of the metal compound forming the anti-reflection film 9. Therefore, by adopting an etchant (liquid or gas) having a low etching rate for the shading film 41 and a high selectivity ratio for etching the anti-reflection film 9 relative to etching the shading film 41, it is possible to selectively etch only the anti-reflection film 9 without etching the shading film 41.

[0153] In this step, the functional film 2 is not etched because its surface is covered with the light shielding film 41 .

[0154] In addition, as the etching device and the etching agent, a known etching device and the etching agent capable of performing selective etching can be used as appropriate. The same shall apply to the following.

[0155] Then, if Figure 5 As shown in (d), the low-dose region 5b (second region) and the unexposed region 5a (third region) of the resist film 5 are used as masks, and the light-shielding film 41 is selectively etched relative to the anti-reflection film 9 and the functional film 2 by wet etching or dry etching. The anti-reflection film 9 and the functional film 2 are formed of a compound of a metal different from the metal forming the light-shielding film 41. Therefore, by using an etchant (chemical solution or gas) having a low etching rate for the anti-reflection film 9 and the functional film 2 and a high selectivity ratio for etching the light-shielding film 41 relative to etching the anti-reflection film 9 and the functional film 2, the etching rate of the anti-reflection film 9 and the functional film 2 can be suppressed to a low level, and only the light-shielding film 41 can be selectively etched.

[0156] Generally, in the case of wet etching, when the upper light shielding film 41 is selectively etched, there is a tendency to reduce damage (film loss and ion impact caused by dry etching, etc.) to the underlying functional film 2. Therefore, in terms of avoiding damage to the functional film 2, wet etching can be preferably used.

[0157] Then, if Figure 5 As shown in (e), the low-dose region 5b (second region) and the unexposed region 5a (third region) of the resist film 5 are used as masks, and the functional film 2 is selectively etched relative to the light-shielding film 41 by wet etching or dry etching. As with the selective etching of the anti-reflection film 9 described above, the light-shielding film 41 is formed of a metal different from the metal of the metal compound forming the functional film 2, and an etchant (chemical solution or gas) having a high selectivity ratio for etching the functional film 2 relative to etching the light-shielding film 41 can be used. Therefore, by using an etchant that does not etch the light-shielding film 41, only the functional film 2 can be selectively etched.

[0158] However, the antireflection film 9 and the functional film 2 are metal compounds composed of the same metal. When isotropic etching, particularly wet etching, is performed, the antireflection film 9 may be undercut depending on the etchant used to etch the functional film 2 .

[0159] However, the film thickness of the anti-reflection film 9 is thinner than the film thickness of the functional film 2. For example, the film thickness of the anti-reflection film 9 can be set to (but not limited to) one-fifth of the film thickness of the functional film 2 to a film thickness that is one order of magnitude thinner than the film thickness of the functional film 2. Therefore, compared with the functional film 2, the height of the side wall surface exposed by the anti-reflection film 9 is low and the exposed area is small, and the side erosion amount of the anti-reflection film 9 is small.

[0160] Therefore, even if Figure 5 The etchant used in the etching step of the antireflection film 9 in (c) is the same as the etchant used for the functional film 2 in this step, and the amount of side etching of the antireflection film 9 (the amount of retreat due to side etching) is also small.

[0161] Therefore, the same etching agent (chemical solution) can be used in the same etching device (wet etching device).

[0162] In this process, there is no obstacle to using an etchant (chemical solution or gas) that does not etch the anti-reflection film 9 to etch the functional film 2. However, as described above, in the etching process of the anti-reflection film 9 and the etching process of the functional film 2, by using the same etchant in the same etching device, the running cost of the etching device and / or the etchant can be reduced.

[0163] Then, if Figure 6 As shown in (a), Figure 2 In the step (c) shown in FIG. 1 , only the resist film 5 in the low-dose region 5 b is selectively removed, and only the unexposed region 5 a is left on the anti-reflection film 9 .

[0164] Then, if Figure 6 As shown in (b), the unexposed area 5a of the resist film 5 is used as a mask. Figure 5 In the step (c) shown in FIG. 9 , the anti-reflection film is selectively etched with respect to the light shielding film 41 .

[0165] When etching the anti-reflection film 9, the functional film 2 may be etched sideways. However, since the film thickness of the anti-reflection film 9 is much thinner than that of the functional film 2, the etching amount of the anti-reflection film 9 is small. Therefore, in this step of etching the anti-reflection film 9, even if an etchant capable of etching both the anti-reflection film 9 and the functional film 2 is used, the etched amount of the functional film 2 is small, and the reduction in the pattern width of the functional film 2 can be reduced.

[0166] In addition, in this process, it is not a problem to etch the anti-reflection film 9 using an etchant (chemical solution or gas) that does not etch both the light shielding film 41 and the functional film 2. However, as described above, the side etching of the functional film 2 during the etching of the anti-reflection film 9 has a slight effect on the pattern size, and it is possible to prevent the degradation of the dimensional accuracy. Therefore, by etching the anti-reflection film 9 in the etching process ( Figure 5 (c) and Figure 6 The process (b) shown in FIG. 1 and the etching process ( Figure 5 Using the same etchant in the step (shown in (e)) can help reduce the running cost of the etching process (for example, including the management cost of the etchant).

[0167] In addition, as an etching method, there is no obstacle to using a dry etching method. However, compared with a dry etching device, a wet etching device does not require a vacuum chamber, exhaust equipment, etc., so it is easy to cope with the manufacture of a large-area photomask 100, and it is generally low-priced. According to this embodiment, the wet etching method, which is an etching method with strong isotropy, can also easily ensure the pattern size accuracy of the functional film 2, so by using a wet etching device as an etching device, the effect of reducing manufacturing costs is large.

[0168] Then, if Figure 6 As shown in (c), Figure 5 In the step (d) of FIG. 1 , the light shielding film 41 is etched selectively with respect to the antireflection film 9 and the functional film 2 using the unexposed region 5 a of the resist film 5 as a mask.

[0169] Then, if Figure 6 As shown in (d) of FIG. 1 , the resist film 5 in the unexposed region 5 a is removed by ashing or immersion in a resist stripping solution, thereby obtaining a photomask 100 .

[0170] In this embodiment, the shading film 41 is composed of a film having etching characteristics different from those of the functional film 2 and the anti-reflection film 9, and the film thickness of the anti-reflection film 9 is set to be thinner than the film thickness of the functional film 2, thereby easily reducing the side etching of the functional film 2 and ensuring the dimensional accuracy of the functional film 2.

[0171] Therefore, it is possible to easily ensure the required dimensional accuracy for a final product manufactured using the present photomask 100 in a photolithography process.

[0172] Furthermore, by using the same etching device to etch the anti-reflection film 9 and the functional film 2, good processing accuracy can be achieved. As a result, it is possible to obtain an effect such as contributing to a reduction in manufacturing costs. In particular, when a wet etching device is used as the etching device, the effect is greater.

[0173] In addition, the above embodiment is described by taking the case of using a positive resist as the resist film 5 as an example, and the same is true when a negative resist is used. In the case of a negative resist, the relationship of the exposure amount is opposite to that of a positive resist. The unexposed area of ​​the positive resist corresponds to the high-dose area of ​​the negative resist, and the high-dose area of ​​the positive resist corresponds to the unexposed area of ​​the negative resist.

[0174] (Implementation 3)

[0175] Figure 7 , Figure 8 It is a cross-sectional view showing the main manufacturing process of the photomask 100 according to Embodiment 3. Hereinafter, the manufacturing method of the photomask 100 is described with reference to the drawings.

[0176] (Film forming process: photomask blank preparation process)

[0177] like Figure 7 As shown in (a), a transmissive substrate 11 such as synthetic quartz glass is prepared, and a semi-transmissive lower layer film 12 (e.g., film thickness 5 [nm] to 20 [nm]) formed of a well-known material such as a Cr-based metal compound, a Si-based compound, or a metal silicide is formed on the transmissive substrate 11 by sputtering, evaporation, or the like.

[0178] Here, the transmissive substrate 11 has a transmittance of 90 to 100% (90%≤transmittance≤100%) with respect to representative wavelengths (eg, i-line, h-line, g-line) included in exposure light used in a photolithography process using the photomask 100 .

[0179] Furthermore, semi-transmissive means that the transmittance with respect to a representative wavelength included in the exposure light is lower than the transmittance of the transmissive substrate 11 and higher than the transmittance of the laminated structure film described later.

[0180] The exposure light may be, for example, an i-line, an h-line, or a g-line, or may be a mixed light containing at least two of these. The exposure light is not limited to these lights.

[0181] The lower layer film 12 can be used as a halftone film or a phase shift film.

[0182] For example, when the lower film 12 is used as a halftone film, the transmittance of the lower film 12 is set to 10 to 70% (10% ≤ transmittance ≤ 70%) with respect to the representative wavelength. The phase shift amount may be set small (approximately 0°, for example, 0 to 20°).

[0183] In addition, for example, when the lower layer film 12 is used as a phase shift film, the transmittance of the lower layer film 12 is set to 3 to 15% (3% ≤ transmittance ≤ 15%) with respect to the representative wavelength contained in the exposure light, and the phase shift amount is set to 180° (160° ≤ phase shift amount ≤ 200°), and it is further preferably set to 170° ≤ phase shift amount ≤ 190°.

[0184] The optical properties of the lower layer film 12 as a halftone film and a phase shift film can be realized by adjusting the composition and the film thickness, for example.

[0185] Next, an upper film 13 made of a known material such as a Cr-based metal compound, a Si-based compound, or a metal silicide is formed on the lower film 12 by, for example, sputtering or vapor deposition (e.g., a film thickness of 50 [nm] to 100 [nm]). However, the upper film 13 is formed of a material having different etching characteristics from the lower film 12. For example, a combination of using a Cr-based compound as the lower film 12 and a metal-based compound other than Cr, such as a Ti-based compound or a Ni-based compound, is selected as the upper film 13. In addition, the metal-based compound such as the Cr-based compound may also be composed of only metal.

[0186] The material (component) and film thickness of the upper film 13 may be adjusted so that the laminated film of the upper film 13 and the lower film 12 has light-shielding properties with respect to the transmittance of the representative wavelength of the upper film 13. The transmittance with respect to the representative wavelength of the laminated film is, for example, 1% or less (0% ≤ transmittance ≤ 1%). In other words, the optical density OD value may be 3.0 or more by adjusting the material (component) and film thickness of the light-shielding film 4 in the laminated region of the functional film 2, the etching stopper film 3, and the light-shielding film 4.

[0187] Hereinafter, a stacked structure in which the lower layer film 12 and the upper layer film 13 are formed on the transmissive substrate 11 is referred to as a photomask blank.

[0188] A plurality of photomask blanks having the above structure may be prepared in advance and stored. When a customer places an order, the photomask blanks having the above structure prepared in advance can be used to shorten the production period.

[0189] (Photoresist Formation Process)

[0190] Then, if Figure 7 As shown in (b) of FIG. 1 , a (photo) resist film 14 is formed on the upper film 13 by coating, spraying or the like.

[0191] (Exposure process)

[0192] Then, if Figure 7As shown in (c) of FIG. 1 , the photomask blank is placed on an exposure (drawing) device (eg, a laser drawing device) (placed on an exposure stage in the exposure device), and the resist film 14 is exposed.

[0193] At this time, three regions with different exposure doses are formed in the resist film 14 , namely, a high-dose region 14 c (first region), a low-dose region 14 b (second region), and an unexposed region 14 a (third region).

[0194] Here, the unexposed region 14a is a region that is not exposed, that is, a region with an exposure amount of 0, the low-dose region 14b is a region exposed with a relatively low exposure amount, and the high-dose region 14c is a region exposed with a relatively high exposure amount.

[0195] The drawing method using the exposure device is not limited to laser drawing, and exposure using, for example, an electron beam may be used.

[0196] More specifically, the high dose in the high dose region is an exposure amount that is greater than the exposure amount required to dissolve the resist when the resist is removed by the first development step described later. In contrast, the low dose in the low dose region is an exposure amount that is such that the resist is not removed by the first development step described later and remains, but is removed by the second development step. For example, based on the high dose required in the first development step, the exposure amount is in the range of 5% to 90% of the high dose.

[0197] The low dose can be appropriately set within the above range, but of course, the processing time of the second development step needs to be considered.

[0198] In addition, for the sake of simplicity, the high-dose region 14c of the resist film 14 is sometimes referred to as the "high-dose region 14c", the low-dose region 14b of the resist film 14 is sometimes referred to as the "low-dose region 14b", and the unexposed region 14a of the resist film 14 is sometimes referred to as the "unexposed region 14a".

[0199] The low-dose region 14b and the high-dose region 14c can be formed without removing (taking out) the transmissive substrate 11 from the exposure device. For example, these regions can be formed by exposing the region corresponding to the low-dose region 14b and the region corresponding to the high-dose region 14c by scanning the laser beam in a manner to obtain a first exposure amount and a second exposure amount, respectively.

[0200] In addition, the area corresponding to the low-dose area 14b and the high-dose area 14c may be exposed by scanning the laser in a manner to obtain a first exposure amount, and then additionally scanning the laser only in the area corresponding to the high-dose area 14c in a manner to obtain a second exposure amount. The exposure amount is averaged by multiple laser irradiations, and the uniformity of the exposure amount of the high-dose area 14c can be improved. In addition, when the low-dose area 14b and the high-dose area 14c are connected, the uniformity of the exposure amount of the boundary area can also be improved.

[0201] As described above, since the exposure process of the low-dose region 14 b and the high-dose region 14 c is performed without removing the photomask blank from the exposure apparatus, it is possible to suppress the occurrence of overlay errors (deviations) between these regions (patterns).

[0202] (First Development (Resist Removal) Step)

[0203] Then, if Figure 7 As shown in (d) of FIG. 8 , in the first development step, only the resist film 14 in the high-dose region 14 c is selectively removed using a developer, and the resist film 14 is patterned.

[0204] As described later, since the dissolution characteristics of the developer of the resist film 14 depend on the exposure amount (dose), the exposed resist film 14 can be selectively removed in sequence according to the exposure amount. In the first development step, by performing development (using dissolution of the developer) under development conditions where the dissolution rate of the high-dose region 14c is very high (for example, several times or even more than one order of magnitude) relative to the dissolution rate of the unexposed region 14a and the low-dose region 14b, only the high-dose region 14c is selectively removed.

[0205] In addition, if Figure 7 As shown in (d), the resist film thickness of the low-dose region 14b is thinner than the resist film thickness of the unexposed region 14a.

[0206] (First Etching Step)

[0207] Then, if Figure 8 As shown in (a), the patterned resist film 14, i.e., the resist film 14 in the unexposed area 14a and the low-dose area 14b, is used as an etching mask, and the upper film 13 is etched by wet etching or dry etching, and then the lower film 12 is etched by wet etching or dry etching to expose the transmissive substrate 11.

[0208] By making the upper film 13 and the lower film 12 using different materials, the upper film 13 can be selectively etched using an etchant (chemical solution or gas) that does not etch the lower film 12. Thereafter, the lower film 12 can be selectively etched using an etchant (chemical solution or gas) that does not etch the upper film 13.

[0209] (Second Development (Resist Removal) Step)

[0210] Then, if Figure 8 As shown in (b) of FIG. 1 , in the second development step, only the resist film 14 in the low-dose region 14b is selectively removed by a developer to pattern the resist film 14. In this step, only the unexposed region 14a remains on the upper film 13.

[0211] The reason why the resist film 14 with different exposure amounts can be removed sequentially according to the exposure amount as shown in the first development step and the second development step is that the dissolution rate depends nonlinearly on the development conditions (time, etc.). By utilizing the characteristic that the change point of the dissolution rate change (increase) depends on the exposure amount, the areas with different exposure amounts can be selectively removed sequentially.

[0212] In the second development step, development (dissolution) can be performed under development conditions where the dissolution rate of the low-dose region 14 b is much higher than the dissolution rate of the unexposed region 14 a , and only the low-dose region 14 b can be selectively removed.

[0213] Furthermore, by using this method, three or more different patterns of the resist film 14 can be obtained.

[0214] (Second Etching Process)

[0215] Then, if Figure 8 As shown in (c), the unexposed region 14a is used as an etching mask, and an etchant (chemical solution or gas) that does not etch the lower film 12 is used to selectively etch the upper film 13 by wet etching or dry etching.

[0216] exist Figure 8 In (c), a pattern consisting of only the lower film 12 is formed on both sides of a pattern consisting of a stack of the lower film 12 and the upper film 13 .

[0217] The pattern consisting only of the lower film 12 is determined by the low-dose region 14b, so that Figure 7 It is optically set in the exposure step shown in (c).

[0218] (Third Resist Removal Step)

[0219] Then, if Figure 8As shown in (d) of FIG. 8 , the resist film 14 in the unexposed region 14 a is removed by ashing or immersion in a resist stripping solution.

[0220] Through the above steps, a photomask 100 including a light shielding region 15 formed of a stack of lower film 12 and upper film 13, a semi-transmissive region 16 formed of the lower film 12, and a transmissive region 17 where the transmissive substrate 11 is exposed can be obtained.

[0221] The photomask 100 can function as a multi-grayscale halftone mask by adopting the above-mentioned halftone film as the lower film 12. In addition, the photomask 100 can function as a phase shift mask by adopting the above-mentioned phase shift film as the lower film 12. In this case, since the occurrence of the overlay error in the exposure process can be suppressed, the rims of the semi-transmissive region 16 can be symmetrically provided on both sides of the light shielding region 15, and a phase shift mask capable of fine patterning can be obtained.

[0222] Fig. 9 This is a SEM photograph showing the cross-sectional shape of the photoresist. Fig. 9 (a) shows the cross-sectional shape of the resist film 14 after the first development step. Fig. 9 (b) shows the cross-sectional shape of the resist film 14 after the second development step.

[0223] like Fig. 9 As shown in (a), the cross section of the resist film 14 has a gently tapered shape at the boundary portion where the unexposed region 14a and the low-dose region 14b meet.

[0224] However, if Fig. 9 As shown in (b), after the second development step, the cross section of the resist film 14 in the unexposed area 14a presents a steep shape. Figure 7 The resist film 14 in the low-dose region 14 b defined in the exposure step shown in (c) is selectively removed in the second development step, and the unexposed region 14 a is accurately defined optically.

[0225] In addition, it is also possible to Fig.10 As shown in (c) of FIG. 1 , the semi-transmissive region 16 and the light-shielding region 15 are formed to be spaced apart from each other. Fig.10 As shown in (a), the resist film 14 is exposed to light by using an exposure (drawing) device, with the unexposed area 14a and the low-dose area 14b spaced apart from each other, and then as shown in Fig.10 As shown in (b), in the first development step, unexposed regions 14a and low-dose regions 14b spaced apart from each other are obtained.

[0226] Afterwards, in Figure 8In the steps shown, the semi-transmissive region 16 and the light shielding region 15 can be formed with a gap therebetween.

[0227] Therefore, the light shielding region 15 and the semi-transmissive region 16 can be optically set to a desired pattern, and the degree of freedom in pattern design of the photomask 100 is greatly improved compared to the methods disclosed in Patent Documents 1 and 2.

[0228] In addition, a pattern arrangement in which a pattern in which the semi-transmissive region 16 and the light-shielding region 15 are spaced apart from each other and a pattern in which the semi-transmissive region 16 and the light-shielding region 15 are adjacent to each other can be realized.

[0229] Regarding the pattern arrangement of the semi-transmissive region 16 and the light shielding region 15 , various arrangements can be made as described above, and this also applies to other embodiments.

[0230] (Implementation 4)

[0231] In Embodiment 3, it is illustrated that three regions, namely, unexposed region 14a, low-dose region 14b, and high-dose region 14c, are formed in the resist film 14 through one exposure process, and a photomask having three grayscales, namely, a transmissive region, a semi-transmissive region, and a light-shielding region, can be manufactured.

[0232] According to the fourth embodiment, a photomask 100 having more grayscales can be provided.

[0233] like Fig.11 As shown in (a), the resist film 14 is exposed in one exposure step to form a first region 14d, a second region 14e, a third region 14f, and a fourth region 14g (exposure amount 0) in descending order of exposure amount.

[0234] Then, if Fig.11 As shown in (b), after the first area 14d with the largest exposure amount is selectively removed, the upper film 13 and the lower film 12 are etched using the resist film 14 of the second area 14e, the third area 14f, and the fourth area 14g as a mask to expose the transmissive substrate 11.

[0235] Then, if Fig.11 As shown in (c), after the second area 14e with the second largest exposure amount is selectively removed, the upper film 13 is etched away using the anti-etching film 14 of the third area 14f and the fourth area 14g as a mask, and the lower film 12 is further partially etched to form a first lower film 12a with a relatively thin film thickness (thin film lower film 12a) and a second lower film 12b with a relatively thick film thickness (thick film lower film 12b).

[0236] Then, if Fig.11As shown in (d), after the third region 14f having the third largest exposure amount is selectively removed, the upper film 13 is etched away using the resist film 14 in the fourth region 14g as a mask to expose the surface of the second lower film 12b.

[0237] Then, if Fig.11 As shown in (e), the resist film 14 in the fourth region 14g is removed by ashing or immersion in a resist stripping solution.

[0238] A shading area 15 is formed as a stack of a lower film 12 and an upper film 13, a transmissive area 17 exposing the transmissive substrate 11, a first semi-transmissive area 161 composed of a first lower film 12a with a relatively thin film thickness, and a second semi-transmissive area 162 composed of a second lower film 12b with a relatively thick film thickness is formed.

[0239] Therefore, it is possible to obtain the photomask 100 having four grayscales, namely, the transmissive region 17 and the light shielding region 15 , and the first semi-transmissive region 161 and the second semi-transmissive region 162 having different transmittances.

[0240] Alternatively, a semi-transmissive region may be formed by partially etching a portion of the upper layer film 13 to reduce the film thickness.

[0241] exist Fig.11 In the process shown in (c), after the second region 14e with the second largest exposure amount is selectively removed, the resist film 14 of the third region 14f and the fourth region 14g is used as a mask. Figure 8 In the same manner as in the step (c) shown in FIG. 1 , only the upper film 13 is selectively etched away to expose the surface of the lower film 12. (See FIG. 1 ) Fig.12 (a)

[0242] Then, if Fig.12 As shown in (b), after the third area 14f with the third largest exposure amount is selectively removed, the upper film 13 is partially etched using the resist film 14 of the fourth area 14g as a mask to form a first upper film 13a with a relatively thin film thickness (thin film upper film 13a) and a second upper film 13b with a relatively thick film thickness (thick film upper film 13b).

[0243] The thin film upper layer film 13 a obtained by reducing the film thickness of the upper layer film 13 has a high transmittance with respect to the representative wavelength, and becomes a semi-transmissive film.

[0244] Then, if Fig.12 As shown in (c), the resist film 14 in the fourth region 14g is removed by ashing or immersion in a resist stripping solution.

[0245] The transmissive region 17 in which the transmissive substrate 11 is exposed, the first semi-transmissive region 161 composed of the lower film 12, the second semi-transmissive region 162 composed of a stack of the lower film 12 and the first upper film 13a with a relatively thin film thickness, and the light-shielding region 15 which is a stack of the lower film 12 and the second upper film 13b with a relatively thick film thickness are formed. Since the second semi-transmissive region 162 includes the first upper film 13a (thin film upper film 13a) on the upper layer of the lower film 12, the transmittance is lower than that of the first semi-transmissive region 161. In addition, since the first upper film 13a is thinner than the upper film 13 and has a higher transmittance, the second semi-transmissive region 162 becomes a semi-transmissive region with a higher transmittance than the light-shielding region 15 (a stack of the lower film 12 and the thick film upper film 13b).

[0246] Therefore, the photomask 100 having four grayscales including the transmissive region 17 , the first semi-transmissive region 161 , the second semi-transmissive region 162 , and the light shielding region 15 , each having a different transmittance, can be obtained.

[0247] In this way, the transmittance can be changed by reducing the film thickness in a part of the lower film 12 or the upper film 13, thereby obtaining a photomask 100 with more grayscales. Fig.11 The manufacturing process shown is similar to Fig.12 The combination of manufacturing steps shown is to obtain a multi-tone photomask 100 by reducing the film thickness in a part of the lower film 12 and the upper film 13 to change the transmittance.

[0248] In addition, the above embodiments describe an example of using a positive resist as the resist film 14, but the same is true when a negative resist is used. In the case of a negative resist, the relationship of exposure amount is opposite to that of a positive resist. For example, the unexposed area of ​​the positive resist corresponds to the high-dose area of ​​the negative resist, and the high-dose area of ​​the positive resist corresponds to the unexposed area of ​​the negative resist.

[0249] Industrial Applicability

[0250] According to the present invention, a photomask including patterns having different optical characteristics can be obtained through a single exposure process, thereby preventing an increase in the number of steps required to manufacture the photomask and realizing a fine pattern.

[0251] By using the present photomask in the production process of products such as display devices, it is possible to contribute to improvement in product performance and the like, and the present photomask has great industrial applicability.

[0252] Description of Reference Numerals

[0253] 100 Photomasks

[0254] 1Transmissive substrate

[0255] 2Functional film (semi-transmissive film)

[0256] 3 Etching stop film (intermediate film)

[0257] 4. Light-shielding film (upper film)

[0258] 5 (Photo)resist film

[0259] 5a Unexposed area

[0260] 5b Low dose area

[0261] 5c High dose area

[0262] 6 Semi-transmissive area

[0263] 7Shading area

[0264] 8 Transmission Area

[0265] 9 Anti-reflective film

[0266] 41 shading film

[0267] 11Transmissive substrate

[0268] 12 Lower membrane

[0269] 12a The first lower film (thin film lower film)

[0270] 12b Second lower film (thick film lower film)

[0271] 13 Upper membrane

[0272] 13a The first upper film (thin film upper film)

[0273] 13b Second upper film (thick upper film)

[0274] 14 (Photo) resist film

[0275] 14a Unexposed area (third area)

[0276] 14b Low dose area (second area)

[0277] 14c High dose area (first area)

[0278] 14d First Area

[0279] 14e Second Area

[0280] 14f Third Area

[0281] 14g Fourth Area

[0282] 15 Shading area

[0283] 16 semi-transmissive areas

[0284] 161 first semi-transmission area

[0285] 162 second semi-transmissive area

[0286] 17 Transmission Area

Claims

1. A method for manufacturing a photomask, characterized in that: Include: A step of preparing a photomask blank, wherein the photomask blank has a lower film on a transmissive substrate and an upper film on the lower film; forming a resist film on the upper film; An exposure process of exposing the resist film to form a first region, a second region, and a third region with different exposure amounts; a first resist removal step of selectively removing the first region; A first etching step of etching the upper film and the lower film; a second resist removal step of selectively removing the second region; a second etching step of selectively etching the upper film relative to the lower film; and A step of removing the third area.

2. The method for manufacturing a photomask according to claim 1, wherein: The lower layer film is a semi-transmissive film having a transmittance of 10% to 70% and a phase shift of 0 degrees to 20 degrees.

3. The method for manufacturing a photomask according to claim 1, wherein: The lower layer film is a phase shift film having a transmittance of 3% to 15% and a phase shift amount of 160 degrees to 200 degrees.

4. The method for manufacturing a photomask according to any one of claims 1 to 3, wherein: The lower film and the upper film are formed of different materials.

5. The method for manufacturing a photomask according to any one of claims 1 to 3, wherein: The transmittance of the stacked region of the lower film and the upper film is adjusted by adjusting the film thickness of the upper film.

6. The method for manufacturing a photomask according to any one of claims 1 to 3, wherein: The upper film is a Cr-based metal compound, a Si-based compound or a metal silicide.

7. The method for manufacturing a photomask according to any one of claims 1 to 3, wherein: The lower layer film is a Cr-based metal compound, a Si-based compound or a metal silicide.

8. The method for manufacturing a photomask according to any one of claims 1 to 3, wherein: The transmittance of the upper film is adjusted by etching the upper film to adjust the film thickness of the upper film.

9. A photomask, characterized in that: include: A pattern formed by an underlying film on a transmissive substrate; and A pattern consisting of a laminated film having an upper film on the lower film, The lower film is a semi-transmissive film having a transmittance of 10% or more and 70% or less and a phase shift of 0 degrees or more and 20 degrees or less. The material of the lower film is selected from any one of Cr-based metal compounds, Si-based compounds and metal silicides, The material of the upper film is selected from any one of Cr-based metal compounds, Si-based compounds, and metal silicides, and is different from the material of the lower film.

10. A photomask, characterized in that: include: A pattern formed by an underlying film on a transmissive substrate; and A pattern consisting of a laminated film having an upper film on the lower film, The lower film is a phase shift film having a transmittance of 3% or more and 15% or less and a phase shift of 160 degrees or more and 200 degrees or less. The material of the lower film is selected from any one of Cr-based metal compounds, Si-based compounds and metal silicides, The material of the upper film is selected from any one of Cr-based metal compounds, Si-based compounds, and metal silicides, and is different from the material of the lower film.

11. A method for manufacturing a photomask, characterized in that: Include: A step of preparing a photomask blank, wherein the photomask blank has a lower film on a transmissive substrate, an intermediate film on the lower film, and an upper film on the intermediate film; forming a resist film on the upper film; An exposure process of exposing the resist film to form a first region, a second region, and a third region with different exposure amounts; a first resist removal step of selectively removing the first region; a first patterning step of selectively etching the upper film relative to the intermediate film; a second patterning step of selectively etching the intermediate film relative to the underlying film; a second resist removal step of selectively removing the second region; a third patterning step of forming a pattern consisting of the lower film and a pattern consisting of a stacked film of the lower film, the intermediate film, and the upper film; and A step of removing the third area.

12. The method for manufacturing a photomask according to claim 11, wherein: The upper film is a light-shielding film, The intermediate film is an etching stopper film, The third patterning step includes a step of etching the intermediate film after etching the lower film and the upper film.

13. The method for manufacturing a photomask according to claim 11, wherein: The upper film is an anti-reflection film, The intermediate film is a light-shielding film, The second patterning step further includes, after the step of etching the intermediate film selectively with respect to the lower film, the step of etching the lower film selectively with respect to the intermediate film. The third patterning step includes a step of, after etching the upper film selectively with respect to the intermediate film, etching the intermediate film selectively with respect to the upper film and the lower film.

14. The method for manufacturing a photomask according to any one of claims 11 to 13, wherein: The upper film and the lower film are made of the same material.

15. The method for manufacturing a photomask according to any one of claims 11 to 13, wherein: The upper film and the lower film are composed of a Cr-based metal compound, a Si-based compound, or a metal silicide compound.

16. The method for manufacturing a photomask according to any one of claims 11 to 13, wherein: The transmittance of the stacked film is adjusted by adjusting the material or film thickness of the upper film.

17. The method for manufacturing a photomask according to any one of claims 11 to 13, wherein: The lower layer film is a semi-transmissive film having a transmittance of 10% to 70% and a phase shift of 0 degrees to 20 degrees.

18. The method for manufacturing a photomask according to any one of claims 11 to 13, wherein: The lower layer film is a phase shift film having a transmittance of 3% to 15% and a phase shift amount of 160 degrees to 200 degrees.

19. A photomask, characterized in that: include: A pattern formed by an underlying film on a transmissive substrate; and A pattern consisting of a laminated film having an intermediate film and an upper film in sequence on the lower film, The material of the lower film is selected from any one of Cr-based metal compounds, Si-based compounds and metal silicides, The material of the upper film is selected from any one of Cr-based metal compounds, Si-based compounds, and metal silicides, and is the same as the material of the lower film.

20. The photomask according to claim 19, wherein: The lower layer film is a semi-transmissive film having a transmittance of 10% to 70% and a phase shift of 0 degrees to 20 degrees.

21. The photomask according to claim 19, wherein: The lower layer film is a phase shift film having a transmittance of 3% to 15% and a phase shift amount of 160 degrees to 200 degrees.

Citation Information

Patent Citations

  • Method for manufacturing photomask, photomask, method for transferring pattern and method for manufacturing display device

    JP2017076146A