Method for improving photoetching exposure uniformity
By chamfering the mercury cadmium tellurium chip substrate and photoresist curing, the problem of photoresist stacking at the edges of the four corners is solved, the close fit between the photolithography and the photoresist is achieved, and the resolution of the exposure pattern is improved and graphic effects.
Patent Information
- Application Number
- CN202410952132.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-08
AI Technical Summary
The photoresist coated on the surface of the mercury cadmium tellurium chip is thicker at the edges of the four corners, while the photoresist in the middle is thinner, resulting in a gap between the photolithography plate and the photoresist, affecting the resolution of the exposure pattern. .
Provide a method for improving the exposure uniformity of photolithography, by chamfering the first end of the substrate, forming a chamfered portion, and curing and exposing the chamfered portion after applying photoresist to avoid photolithography gap between the plate and the photoresist. The chamfering treatment can be achieved through grinding, corrosion liquid or oxygen etching, etc., forming an arc or step structure to improve the distribution of the photoresist.
Through chamfering treatment, photoresist is avoided at the edges of the four corners, ensuring that the photolithography plate is closely fitted with the photoresist, and improving the resolution and graphic effect of the exposed graphics.
Smart Images

Figure CN118915392A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of refrigerated infrared detectors, and in particular to a method for improving photolithography exposure uniformity. Background Art
[0002] Infrared focal plane detection technology has significant advantages such as wide spectral response band, more ground target information, and day and night operation. It is widely used in early warning detection, intelligence reconnaissance, damage effect assessment, and agriculture, animal husbandry, forest resource investigation, development and management, weather forecasting, geothermal distribution, earthquakes, volcanic activities, space astronomical detection, etc. Mercury cadmium telluride infrared detector is one of the representative products of infrared detection technology.
[0003] The single crystal rate of the material of the mercury cadmium telluride chip is low, resulting in the mercury cadmium telluride material being cut into squares of inconsistent sizes and small sizes, making it impossible to use automated equipment for mass production. Similarly, photolithography processes such as coating, exposure, and development are all manually or semi-automatically operated. Because the chip is square and the chip size is inconsistent, it is impossible to use edge removal equipment to remove the corners of the chip after coating, resulting in thick photoresist on the four sides of the chip. In addition, due to the contact exposure used in photolithography, during the rotation of the machine, due to the centrifugal force, the photoresist coated on the surface of the mercury cadmium telluride chip accumulates thicker at the edges of the four corners, while the thickness of the photoresist in the middle of the mercury cadmium telluride chip surface is relatively thin, resulting in a gap between the photomask and the photoresist during exposure, affecting the resolution of the exposure pattern, and the resulting pattern is very poor.
[0004] It should be noted that the information disclosed in the background technology section of the invention is only intended to deepen the understanding of the general background technology of the invention, and should not be regarded as an admission or suggestion in any form that the information constitutes prior art already known to those skilled in the art. Summary of the invention
[0005] The purpose of the present invention is to provide a method for improving the uniformity of photolithography exposure, so as to solve the problem that the photoresist coated on the surface of a mercury cadmium telluride chip is thicker at the four corners, while the thickness of the photoresist in the middle of the surface of the mercury cadmium telluride chip is thinner, resulting in a gap between the photomask and the photoresist during exposure, thereby affecting the resolution of the exposure pattern.
[0006] In order to solve the above technical problems, the present invention provides a method for improving photolithography exposure uniformity, comprising:
[0007] Providing a substrate, the substrate having a first end and a second end, and performing chamfering on the first end of the substrate to form a chamfered portion at the first end;
[0008] Coating a photoresist on a substrate having a chamfered portion, and curing the photoresist;
[0009] The cured photoresist is exposed to light to obtain a target pattern.
[0010] Preferably, the chamfering the first end of the substrate to form a chamfered portion at the first end comprises:
[0011] Applying a first photoresist to a first end of the substrate;
[0012] Chamfering the first end of the substrate coated with the first photoresist by grinding to form a chamfered portion at the first end;
[0013] The first photoresist is removed.
[0014] Preferably, the chamfering the first end of the substrate to form a chamfered portion at the first end comprises:
[0015] The first end portion of the substrate is etched by using an etching solution to perform a chamfering process, thereby forming a chamfered portion at the first end portion.
[0016] Preferably, the etching liquid is an etching liquid that can corrode mercury cadmium telluride materials.
[0017] Preferably, the etching solution is an HBr solution, and the concentration of the HBr solution is 68%.
[0018] Preferably, the chamfering the first end of the substrate to form a chamfered portion at the first end comprises:
[0019] coating the substrate with a first photoresist;
[0020] Performing a first etching on the first photoresist by using oxygen to perform a chamfering process on the first photoresist;
[0021] The substrate is subjected to a second etching process using a mixed gas of CH4, H2 and Ar to chamfer the first end of the substrate and form a chamfered portion at the first end.
[0022] Preferably, in the first etching, the oxygen flow rate is 200 sccm to 400 sccm.
[0023] Preferably, in the second etching, the volume ratio of CH4, H2, and Ar is 1:2:6.
[0024] Preferably, the chamfered portion is an arc-shaped structure.
[0025] Preferably, before the first end of the substrate is chamfered, the method for improving photolithography exposure uniformity further comprises:
[0026] The surface of the substrate is cleaned with a cleaning liquid.
[0027] Compared with the prior art, the method for improving photolithography exposure uniformity of the present invention has the following advantages:
[0028] The present invention provides a substrate, performs chamfering on the corners of the substrate; applies photoresist to the substrate after the chamfering, and solidifies the photoresist; and exposes the solidified photoresist to obtain a target pattern. Therefore, the method for improving the uniformity of photolithography exposure provided by the present invention forms a chamfered portion at the first end portion because the first end portion of the substrate is chamfered. When the substrate is subsequently coated with photoresist and solidified, and then exposed by contact exposure, a gap between the photoresist plate and the photoresist can be avoided, so that the photoresist plate and the photoresist are closely attached. The uniformity of photolithography exposure is improved, the resolution of the exposed pattern is improved, and the pattern effect is also improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 is a schematic diagram of a photolithography exposure process in one embodiment;
[0030] Figure 2 is a flow chart of a method for improving photolithography exposure uniformity provided in one embodiment of the present invention;
[0031] Figure 3 is a schematic diagram of a photolithography exposure process in one embodiment of the present invention;
[0032] Figure 4 is a schematic diagram of a process of photolithography exposure in another embodiment of the present invention;
[0033] Figure 5 is a schematic diagram of the photolithography exposure process in the third embodiment of the present invention;
[0034] Figure 6 is a schematic diagram of the photolithography exposure process in the fourth embodiment of the present invention;
[0035] In the figure,
[0036] 100-substrate; 200-photoresist;
[0037] 300-photolithography plate; 400-mercury cadmium telluride chip;
[0038] 110-chamfered portion; 111-photoresist chamfered portion;
[0039] 120 - step; 130 - first end. DETAILED DESCRIPTION
[0040] In order to make the purpose, advantages and features of the present invention clearer, the method for improving the uniformity of lithography exposure proposed by the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. It should be noted that the drawings are all in a very simplified form and are all in an inaccurate proportion, which is only used to conveniently and clearly assist in explaining the purpose of the embodiments of the present invention. It should be understood that the drawings in the specification do not necessarily show the specific structure of the present invention in proportion, and the illustrative features used to illustrate certain principles of the present invention in the drawings in the specification will also adopt a slightly simplified drawing method. The specific design features of the present invention disclosed herein include, for example, specific dimensions, directions, positions and shapes, which will be determined in part by the specific application and use environment. And, in the embodiments described below, sometimes the same figure mark is used in common between different drawings to represent the same part or a part with the same function, and its repeated description is omitted. In this specification, similar numbers and letters are used to represent similar items, so once an item is defined in one drawing, it does not need to be further discussed in subsequent drawings.
[0041] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of the present invention, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.
[0042] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0043] Ginseng Figure 1As shown, in the prior art, when the HgCdTe chip 400 is subjected to photolithographic exposure, a layer of photoresist 200 is first coated on the surface of the HgCdTe chip 400 by a coating machine. Because the HgCdTe chip 400 is square and the sizes of the HgCdTe chip 400 are inconsistent, it is impossible to use an edge removal device to remove the edges and corners of the chip coated with the photoresist 200, resulting in the photoresist 200 on the four sides of the HgCdTe chip 400 being thicker than the photoresist 200 in the middle. And after the photoresist 200 is cured, a contact exposure method is usually adopted. During the rotation of the machine, due to the action of centrifugal force, the photoresist 200 coated on the surface of the HgCdTe chip 400 is relatively thick at the edges of the four sides, while the thickness of the photoresist 200 in the middle of the surface of the HgCdTe chip is relatively thin, resulting in a gap between the photomask 300 and the photoresist 200 during exposure. Figure 1 The gap shown at a in the middle causes the photomask 300 and the photoresist 200 to not fit together, affecting the resolution of the exposed pattern, so that the resulting pattern is very poor.
[0044] It should be noted that Figure 1 The plane in FIG. 4 is a schematic diagram of the top view of the structure of the mercury cadmium telluride chip 400 during the photolithography exposure process. Figure 1 The cross section corresponding to the arrow in is a schematic diagram of the main cross-sectional structure of the mercury cadmium telluride chip 400 during the photolithography exposure process, and is a schematic diagram of the cross-sectional structure located at the dotted line in the top view. Figures 3 to 5 The plane in FIG. 1 is a schematic diagram of the top structure of the substrate 100 during the photolithography exposure process. Figures 3 to 5 The cross section corresponding to the arrow in is a schematic diagram of the main cross-sectional structure of the substrate 100 during the photolithography exposure process, and is a schematic diagram of the cross-sectional structure located at the dotted line in the top view.
[0045] The core idea of the present invention is to provide a method for improving the uniformity of photolithography exposure, which can avoid the appearance of a gap between the photomask 300 and the photoresist 200 when performing photolithography exposure on a mercury cadmium telluride chip, so that the photomask 300 and the photoresist 200 can fit tightly together to improve the resolution of the exposure pattern.
[0046] In order to realize the above idea, the present invention provides a method for improving the uniformity of photolithography exposure. Figures 2 to 6 A specific implementation of a method for improving photolithography exposure uniformity is disclosed. The method for improving photolithography exposure uniformity includes the following steps S1 to S3.
[0047] Step S1: providing a substrate 100 , wherein the substrate 100 has a first end 130 and a second end (not shown in the figure), and chamfering the first end 130 of the substrate 100 to form a chamfered portion 110 at the first end 130 .
[0048] Specifically, refer to Figures 2 to 5As shown, the substrate 100 can be a mercury cadmium telluride chip 400, or a material plate made of mercury cadmium telluride material. Of course, the substrate 100 can also be any base made of mercury cadmium telluride material. The substrate 100 has two ends, including a first end 130 and a second end (not shown). The first end 110 of the substrate 100 is chamfered to form a chamfered portion at the first end 130. That is, the chamfered portion 110 is formed at the first end 130, and the chamfered portion 110 does not extend to the second end. The substrate 100 can be a quadrilateral structure. When the substrate 100 is a quadrilateral structure, the four sides and four corners of the end of one end of the quadrilateral structure are chamfered, and the chamfered portions 110 are formed at the four sides and four corners of the substrate 100. When the substrate 100 is a circular structure, the chamfering process can be performed along the circumferential direction of the end of one end of the circular structure to form a chamfered portion 110 in the circumferential direction of the substrate 100. Of course, the substrate 100 can also be a triangle, or an irregular structure, or a combination of any structures. In this embodiment, preferably, the substrate 100 is a quadrilateral structure. Below, the substrate 100 is explained as a quadrilateral structure.
[0049] Ginseng Figure 3 As shown, as one embodiment thereof, the first end portion 130 of the substrate 100 is chamfered to form the chamfered portion 110 at the first end portion 130, including: firstly, the first end portion 130 of the substrate 100 is coated with a first photoresist. In order to distinguish the coating of photoresists in different process steps, the photoresist coated for the first time is referred to as the first photoresist. The photoresist coated for the second time is referred to as the second photoresist. In this step, the surface of the substrate 100 can be protected by coating the first photoresist, so that the substrate 100 is prevented from being damaged in the following grinding step.
[0050] Next, the first end portion 130 of the substrate 100 coated with the first photoresist is chamfered by grinding. The substrate 100 is placed on a grinder, and the four corners and four edges of the first end portion 130 coated with the first photoresist are chamfered to form a chamfered portion 110. The chamfered portion 110 may be an arc-shaped structure.
[0051] Finally, the first photoresist is removed. Since the first photoresist has been contaminated and there are impurities such as dust on the surface of the first photoresist, the first photoresist needs to be removed. Then, the substrate 100 having the chamfered portion 110 is subjected to the next process.
[0052] Ginseng Figure 4As shown, as a second embodiment, the first end 130 of the substrate 100 is chamfered to form a chamfered portion 110 at the first end 130, including: the first end 130 of the substrate 100 is corroded by using an etching solution to chamfer the first end 130 of the substrate 100. The etching solution is an etching solution that can corrode the mercury cadmium telluride material. For example, the etching solution can be a potassium dichromate solution, aqua regia, a bromine-based solution, and other solutions that can corrode the mercury cadmium telluride material. Preferably, in this embodiment, the etching solution is an HBr solution, and the concentration of the HBr solution is 68%.
[0053] Ginseng Figure 5 As shown, as a third embodiment, the first end 130 of the substrate 100 is chamfered to form a chamfered portion 110 at the first end 130, including: first, the substrate 100 is coated with a first photoresist. For the same reason as above, in order to distinguish the coated photoresists in different process steps, the photoresist coated for the first time is called the first photoresist. The photoresist coated for the second time is called the second photoresist. In this step, the surface of the substrate 100 can be protected by coating the first photoresist, so that the substrate 100 is prevented from being damaged in the following grinding step, and dust can also be prevented from falling on the surface of the substrate 100.
[0054] Next, the first photoresist is first etched with oxygen to chamfer the first photoresist to form a photoresist chamfer 111 on the first photoresist. If the substrate 100 is a quadrilateral structure, in this embodiment, similarly, the four sides and four corners of the first photoresist are chamfered. In the first etching, the oxygen flow rate is 200sccm to 400sccm. That is, the oxygen flow rate can be 200sccm, 250sccm, 300sccm, 350sccm, 400sccm, or any value in the range of 200sccm to 400sccm. In this embodiment, preferably, the oxygen flow rate is 300sccm.
[0055] Then, a second etching is performed on the first end portion 130 of the substrate 100 using a mixed gas of CH4, H2, and Ar to chamfer the substrate 100. In the second etching, the volume ratio of CH4, H2, and Ar is 1:2:6. By performing the second etching on the substrate 100, not only the chamfering of the substrate 100 can be performed, but also the first photoresist can be removed, so as to facilitate the next process step.
[0056] Ginseng Figure 6 As shown, as a reasonable improvement of the above embodiment, the edge of the first end 130 of the substrate 100 may also be chamfered to form a chamfered portion 110 at the first end 130. The chamfered portion 110 may also be as follows: Figure 6 The step 120 is shown. By setting the structure of the step 120, when coating the photoresist 200, it is also possible to avoid the photoresist 200 coated on the surface of the substrate 100 from being thicker at the four corners, while the thickness of the photoresist 200 in the middle of the surface of the substrate 100 is relatively thin. Therefore, during exposure, there is no gap between the photomask 300 and the photoresist 200, which improves the uniformity of photolithography exposure, improves the resolution of the exposure pattern, and also improves the pattern effect.
[0057] Furthermore, in order to improve the effect of photolithography exposure and further improve the resolution and pattern effect of the exposure pattern, before the first end portion 130 of the substrate 100 is chamfered, the method for improving the uniformity of photolithography exposure further includes: using a cleaning liquid to clean the surface of the substrate 100. Preferably, a 68% HBr solution is used to clean the surface of the substrate 100 to remove impurities such as dust on the surface of the substrate 100.
[0058] Step S2: coating the substrate 100 having the chamfered portion 110 with the photoresist 200 and curing the photoresist 200 .
[0059] Specifically, refer to Figures 2 to 5 As shown, the substrate 100 having the chamfered portion 110 is coated with a photoresist 200, and the photoresist 200 is cured by baking. Figure 3 and Figure 5 In the disclosed embodiment, the photoresist 200 here may be referred to as a second photoresist.
[0060] Step S3: exposing the cured photoresist 200 to obtain a target pattern.
[0061] Specifically, refer to Figures 2 to 5 As shown, the cured photoresist 200 is exposed by contact exposure to form a target pattern on the photoresist plate.
[0062] Through the above-mentioned embodiment, the first end 130 of the substrate 100, for example, the HgCdTe chip, is chamfered to form a chamfered portion 110 at the first end 130. The chamfered portion 110 may be an arc-shaped structure, or may be formed at the first end 130 as Figure 6 The step 120 is shown. When the substrate 100 is subsequently coated with photoresist and the photoresist 200 is cured, the substrate 100 is exposed by contact exposure, so that a gap between the photoresist 300 and the photoresist 200 can be avoided, and the photoresist 300 and the photoresist 200 are closely attached. The uniformity of photolithography exposure is improved, the resolution of the exposed pattern is improved, and the pattern effect is also improved.
[0063] In summary, the above embodiments provide detailed descriptions of different configurations of the method for improving the uniformity of photolithography exposure. Of course, the above description is only a description of the preferred embodiments of the present invention, and is not any limitation to the scope of the present invention. The present invention includes but is not limited to the configurations listed in the above embodiments. Those skilled in the art can draw inferences based on the contents of the above embodiments. Any changes and modifications made by ordinary technicians in the field of the present invention based on the above disclosure are within the scope of protection of the claims.
Claims
1. A method for improving photolithography exposure uniformity, characterized in that: include: Providing a substrate, the substrate having a first end and a second end, and performing chamfering on the first end of the substrate to form a chamfered portion at the first end; Coating a photoresist on a substrate having a chamfered portion, and curing the photoresist; The cured photoresist is exposed to light to obtain a target pattern.
2. The method for improving photolithography exposure uniformity according to claim 1, characterized in that: The chamfering the first end of the substrate to form a chamfered portion at the first end comprises: Applying a first photoresist to a first end of the substrate; Chamfering the first end of the substrate coated with the first photoresist by grinding to form a chamfered portion at the first end; The first photoresist is removed.
3. The method for improving lithography exposure uniformity according to claim 1, characterized in that: The chamfering the first end of the substrate to form a chamfered portion at the first end comprises: The first end portion of the substrate is etched by using an etching solution to perform a chamfering process, thereby forming a chamfered portion at the first end portion.
4. The method for improving photolithography exposure uniformity according to claim 3, characterized in that: The etching liquid is an etching liquid that can corrode mercury cadmium telluride materials.
5. The method for improving photolithography exposure uniformity according to claim 4, characterized in that: The etching solution is HBr solution, and the concentration of the HBr solution is 68%.
6. The method for improving photolithography exposure uniformity according to claim 1, characterized in that: The chamfering the first end of the substrate to form a chamfered portion at the first end comprises: coating the substrate with a first photoresist; Performing a first etching on the first photoresist by using oxygen to perform a chamfering process on the first photoresist; The substrate is subjected to a second etching process using a mixed gas of CH4, H2 and Ar to chamfer the first end of the substrate and form a chamfered portion at the first end.
7. The method for improving photolithography exposure uniformity according to claim 6, characterized in that: In the first etching, the oxygen flow rate is 200 sccm to 400 sccm.
8. The method for improving photolithography exposure uniformity according to claim 6, characterized in that: In the second etching, the volume ratio of CH4, H2, and Ar is 1:2:
6.
9. The method for improving photolithography exposure uniformity according to any one of claims 1 to 8, characterized in that: The chamfered portion is an arc-shaped structure.
10. The method for improving photolithography exposure uniformity according to claim 1, characterized in that: Before the first end of the substrate is chamfered, the method for improving photolithography exposure uniformity further includes: The surface of the substrate is cleaned with a cleaning liquid.