Conductive slurry preparation method
By forming a carbon nanotube-nano nickel composite layer and an electroless metal layer on the conductive microspheres, an equivalent hollow structure is achieved, the signal loss problem caused by the skin effect is solved, and the conductive performance of high-frequency circuits is improved.
Patent Information
- Application Number
- CN202411078007.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In high-frequency circuits, existing conductive microspheres increase signal transmission energy loss due to skin effect, reduce transmission bandwidth, and design of hollow structure in the printed conductive layer of ceramic substrate is complex, and the multi-conductor design space is insufficient, making it difficult to effectively improve trends. Skin depth.
The hollow conductive microsphere preparation method is adopted to form a carbon nanotube-nano nickel composite layer through surface modification, and the metal layer is electrolessly plated on its outer surface to form a core-shell structure of microspheres @carbon nanotube-carbon nanonier@metal. Achieve equivalent hollow structure and highly conductive network to reduce skin effect.
It effectively weakens the skin effect, reduces signal loss, increases the conductive interface of high-frequency current, ensures the sufficient thickness of the interface conductive channel, and improves the conductive performance of the conductive layer.
Smart Images

Figure CN118919167A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of conductive pastes, and in particular relates to a method for preparing conductive pastes. Background Art
[0002] The skin effect refers to the phenomenon that in high-frequency circuits, AC current tends to flow along the surface of the conductor. When the frequency increases, the current is no longer evenly distributed across the entire conductor cross section, but is mainly concentrated in a thin layer near the conductor surface. First, the skin effect causes the current to be mainly distributed near the conductor surface, rather than within the entire cross section, thereby increasing resistance and power consumption, which will increase energy loss in signal transmission and reduce system efficiency; secondly, the skin effect also limits the transmission capacity of high-frequency signals. Since the current is mainly concentrated near the conductor surface, the effective transmission area is reduced, resulting in higher frequencies and a corresponding decrease in the transmission bandwidth of the circuit.
[0003] In order to overcome the adverse effects of the skin effect, the methods commonly used are:
[0004] 1) Using gold plating or other surface treatment technology can effectively reduce the surface resistance of the conductor, reduce signal loss, and improve the ability of signal transmission;
[0005] 2) Selecting appropriate conductor materials and structural designs can also improve the skin effect. Multiple strands of thin conductors can effectively mitigate the impact of the skin effect and increase the effective transmission area.
[0006] 3) Flat copper wire is often used when high current is used. If possible, the thickness of the wire can be reduced and the width can be increased to make it strip-shaped. As long as the thickness and width of the strip line are reasonably determined, the influence of high-frequency skin effect can be minimized.
[0007] 4) Use tubes and poles to reduce the influence of skin effect. When the frequency is very high (at least greater than 1KHZ), the depth of skin effect is also very small. The current is basically concentrated on the surface of the conductor, and there is basically no current in the internal conductor part. After removing this part of the conductor and turning it into a tube, the weight of the conductor can be greatly reduced without affecting the transmission of current. Similarly, at very high frequencies, the strip line can also be pressed into a pole shape, which can not only ensure its transmission of current but also reduce its weight.
[0008] In the above-mentioned methods for solving or alleviating the skin effect, for the preparation of the printed conductive layer of the ceramic substrate, due to the limited thickness and fine structure space, it is relatively complicated to design a hollow structure, and there is insufficient space for a multi-conductor design.
[0009] Patent document No. 202310719083.9 discloses a conductive microsphere and a method for manufacturing the same. The conductive microsphere has three layers from the inside to the outside: the inner layer is a microsphere core of micrometer size, the middle layer is a nano buffer layer, and the outer layer is a metal plating layer; the nano buffer layer is a polymer nano layer or a graphene oxide layer with catalytically active functional groups; the polymer nano layer is a polymer nano layer containing a silane coupling agent and polyvinyl alcohol. The graphene oxide layer with functional groups is a coating formed by a graphene oxide aqueous solution on the surface of the microsphere core.
[0010] Since the buffer layer of the conductive microspheres in the prior art is made of organic materials coated with graphene, the skin effect of pure graphene is relatively large and the ability to improve the skin depth is limited. Summary of the invention
[0011] In view of the problems in the related art, the present invention proposes a method for preparing a conductive paste to overcome the above technical problems existing in the existing related art.
[0012] The technical solution of the present invention is achieved in this way:
[0013] A method for preparing a conductive paste comprises the following steps:
[0014] 1) The conductive paste comprises the following raw materials in percentage by weight:
[0015] 40-50wt% of hollow conductive microspheres, 40-50wt% of micron metal powder, 0.1-5wt% of adhesive, 0.01-3wt% of stabilizer and 9-30wt% of solvent.
[0016] 2) Mixing
[0017] The prepared raw materials are configured and mixed uniformly according to the preset weight percentage, and then added into a three-roll grinder for three-roll differential cycle peeling, the three-roll speed ratio is 1:3:9, the gap between the three rolls is 90-350 μm, and the cycle peeling is 2 to 50 times.
[0018] Discharging the material to obtain a conductive paste.
[0019] The preparation method of the hollow conductive microspheres comprises the following steps:
[0020] A) surface modification of hollow microspheres;
[0021] B) coating the surface-modified hollow microspheres with a mixture of polyolefin, carbon nanotubes and nano-nickel powder to form a composite layer outside the surface-modified hollow microspheres to prepare a microsphere intermediate;
[0022] The mass ratio of the surface-modified hollow microspheres: carbon nanotubes: nano nickel powder: polyolefin is 15-25: 5-10: 1-3: 45-55;
[0023] C) sensitizing the microsphere intermediate, plating the sensitized microsphere intermediate with metal by chemical plating to form a chemically plated metal layer, and washing;
[0024] D) Collect and make hollow conductive microspheres.
[0025] A carbonization treatment is provided between step B) and step C), or a carbonization treatment is provided between step C) and step D);
[0026] The carbonization treatment at least includes carbonization at a carbonization temperature of 230 to 330° C. for 5 to 120 minutes.
[0027] Specifically, one of the methods for preparing the hollow conductive microspheres comprises the following steps:
[0028] A) surface modification of hollow microspheres;
[0029] B) coating the surface-modified hollow microspheres with a mixture of polyolefin, carbon nanotubes and nano-nickel powder to form a composite layer outside the surface-modified hollow microspheres to prepare a microsphere intermediate;
[0030] The mass ratio of the surface-modified hollow microspheres: carbon nanotubes: nano nickel powder: polyolefin is 15-25: 5-10: 1-3: 45-55;
[0031] Carbonization treatment;
[0032] The carbonized microsphere intermediates were ball milled to separate the materials. The ball milling parameters were: revolution 50 / min, rotation 200 / min, ball milling time 6h, and 30% ethanol was added for wet milling.
[0033] C) sensitizing the microsphere intermediate, washing the excess free substances on the surface with deionized water, and then plating metal on the outside of the microsphere intermediate by chemical plating to form a chemically plated metal layer, and washing;
[0034] D) Collect the prepared hollow conductive microspheres.
[0035] Specifically, the second method for preparing the hollow conductive microspheres comprises the following steps:
[0036] A) surface modification of hollow microspheres;
[0037] B) coating the surface-modified hollow microspheres with a mixture of polyolefin, carbon nanotubes and nano-nickel powder to form a composite layer outside the surface-modified hollow microspheres to prepare a microsphere intermediate;
[0038] The mass ratio of the surface-modified hollow microspheres: carbon nanotubes: nano nickel powder: polyolefin is 15-25: 5-10: 1-3: 45-55;
[0039] The above materials are preliminarily crushed and mixed, and then spheroidized by a jet mill until the particle size is 2 to 3 times that of the hollow microspheres;
[0040] C) sensitizing the microsphere intermediate, washing the excess free substances on the surface with deionized water, and then plating metal on the outside of the microsphere intermediate by chemical plating to form a chemically plated metal layer, and washing;
[0041] Carbonization treatment;
[0042] D) Collect and make hollow conductive microspheres.
[0043] Preferably, the carbonization treatment comprises the following steps:
[0044] 1) heating the mixture to be carbonized to 150-180° C. and keeping the temperature for 1-10 minutes to melt the polyolefin and wrap it on the surface of the hollow microspheres;
[0045] 2) Continue heating to 180-230°C and keep warm for 1-10 minutes to allow the polyolefin to react with oxygen in the air to generate oxygen-containing functional groups;
[0046] 3) Continue heating to the set carbonization temperature of 230-330°C, carbonize for 5-120 minutes, and complete the carbonization after cooling.
[0047] In step A), the hollow microspheres and the silane coupling agent are configured in a weight ratio of 100:3-7, the hollow microspheres are first dispersed in an organic solvent (such as anhydrous ethanol, etc.), and then the silane coupling agent is added, heated, cooled, and separated to obtain surface-modified hollow microspheres.
[0048] In step B), preferably, the average particle size of the nano nickel powder is 10-25 nm, the carbon nanotubes are single-walled carbon nanotubes with no special length restriction, and the average particle size of the nano nickel powder is greater than the diameter of the carbon nanotubes.
[0049] Specifically, the main raw materials of the hollow microspheres are highly insulating materials such as oxides and silicon dioxide.
[0050] Specifically, the polyolefin is low-density polyethylene, high-density polyethylene, isotactic polypropylene, atactic polypropylene, or syndiotactic polypropylene.
[0051] In step C), the specific operation of the sensitization is: immersing the microsphere intermediate or the carbonized microsphere intermediate in 1×10 -2 M of PdSO4 aqueous solution, soaking time is 10 to 30 minutes.
[0052] In step C), the specific operation of the chemical plating is:
[0053] 1) NaOH, metal salt, KNaC4H4O6 and water are mixed in a mass ratio of 1:1-2:2.5-5:50 to prepare a mixed solution;
[0054] 2) Put the sensitized microsphere intermediate into the mixed solution, and then add formaldehyde, the mass ratio of the sensitized microsphere intermediate to formaldehyde is 30:5, the temperature is 25-30° C., the pH is 7-8 weak alkaline, and the duration is 5-10 minutes.
[0055] The metal salt may be CuSO4, AgNO3 or the like.
[0056] The hollow conductive microspheres prepared by the present invention are microspheres@carbon nanotubes-carbon-nano nickel@metal core-shell structures.
[0057] The core of the hollow conductive microsphere is the hollow microsphere, the exterior of the hollow microsphere is coated with a carbon nanotube-carbon-nano nickel composite layer, and the exterior of the carbon nanotube-carbon-nano nickel composite layer is coated with a chemically plated metal layer.
[0058] Specifically, the average particle size of the hollow microspheres is 100-500 nm, the thickness of the carbon nanotube-carbon-nano nickel composite layer is 100-300 nm, and the thickness of the chemically plated metal layer is 300-600 nm.
[0059] The average particle size of the hollow microspheres is 100-500 nm, the average particle size of the micron metal powder is 1-5 μm, and the particle size of the micron metal powder increases with the increase of the particle size of the hollow microspheres.
[0060] The micron metal powder has a polyhedral shape, preferably a polyhedron approximately in the shape of a sphere. The micron metal powder can be a metal powder with good conductivity, such as copper powder, silver powder, nickel powder, gold powder, etc.
[0061] The adhesive is one or more of acrylic resin, polyacrylic resin, polyurethane, epoxy resin, amino resin and phenolic resin.
[0062] The stabilizer is one or more of glycolic acid, citric acid, glycine, ascorbic acid, and a diamine stabilizer.
[0063] The solvent is selected from one or more of deionized water, propylene glycol, isopropanol, ethylene glycol, glycerol, monoethanolamine, diethanolamine, triethanolamine, DBE and DPM.
[0064] The curing temperature of the conductive paste is ≤300°C. Preferably, the curing temperature of the conductive paste is ≤200°C.
[0065] It should be noted that the conductive paste of the present invention may also be adaptively added with functional additives such as silane coupling agents.
[0066] Beneficial effects of the present invention:
[0067] Compared with the prior art, the present invention improves the powder structure in the conductive slurry, realizes an equivalent hollow structure design and negative magnetic permeability material construction, increases the skin depth to weaken the skin effect, and thereby solves the signal loss problem caused by the skin effect of the conductive layer in high-frequency and high-speed circuits.
[0068] Furthermore, the hollow conductive microspheres prepared by the present invention have a core-shell structure of microspheres @ carbon nanotubes-carbon-nanonickernel @ metal, completing an equivalent hollow structure of the conductive layer, similar to a honeycomb structure, thereby increasing the conductive interface of high-frequency current signals, thereby reducing the surface current concentration effect; at the same time, the carbon nanotube-carbon-nanonickernel composite layer forms a highly conductive network and a negative magnetic permeability structure, reducing the skin effect of the material and ensuring sufficient thickness of the interface conductive channel. BRIEF DESCRIPTION OF THE DRAWINGS
[0069] Figure 1 It is a schematic structural diagram of the hollow conductive microsphere of the present invention;
[0070] Figure 2 This is the SEM image of the hollow conductive microspheres of Example 3;
[0071] Figure 3 This is the SEM image of the hollow conductive microspheres of Example 6;
[0072] Figure 4 The figure is a sheet resistance test result diagram of Examples 1 to 5 and Comparative Example 1;
[0073] Figure 5 This is a graph showing the magnetic permeability test results of Example 3.
[0074] Reference numerals
[0075] 1. Hollow microspheres;
[0076] 2. Carbon nanotube-carbon-nano nickel composite layer;
[0077] 3. Chemically plated metal layer. DETAILED DESCRIPTION
[0078] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0079] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present invention.
[0080] Example 1
[0081] A method for preparing a conductive paste comprises the following steps:
[0082] 1) The conductive paste comprises the following raw materials in percentage by weight:
[0083] 40 g of hollow conductive microspheres, 40 g of spherical micron copper powder with a particle size of 3 μm, 0.1 g of a binder (acrylic resin), 0.1 g of a stabilizer (hydroxyacetic acid), and 9 g of a solvent (ethylene glycol).
[0084] 2) Mixing
[0085] The prepared raw materials are configured and mixed uniformly according to a preset weight percentage, and then added into a three-roll grinder for three-roll differential speed cyclic stripping, the three-roll speed ratio is 1:3:9, the gap between the three rolls is 300 μm, the cyclic stripping is repeated 10 times, and the material is discharged to obtain a conductive paste.
[0086] The preparation method of the hollow conductive microspheres comprises the following steps:
[0087] A) Surface modification of hollow microspheres (specifically hollow silica microspheres).
[0088] The hollow microspheres and the silane coupling agent KH550 are configured at a weight ratio of 100:3. The hollow microspheres are first dispersed in anhydrous ethanol, and then the silane coupling agent KH550 is added, heated, cooled, and separated to obtain surface-modified hollow microspheres.
[0089] B) the surface-modified hollow microspheres are coated with a mixture of polyolefin (low-density polyethylene), single-walled carbon nanotubes with a tube diameter of 5 nm, and nano-nickel powder with a particle diameter of 10 nm, to form a composite layer outside the surface-modified hollow microspheres to prepare a microsphere intermediate;
[0090] The mass ratio of the surface-modified hollow microspheres: carbon nanotubes: nano-nickel powder: polyolefin is 20:5:1:50.
[0091] C) Carbonization treatment.
[0092] The carbonization process comprises the following steps:
[0093] C-1) heating the mixture to be carbonized to 150° C. and keeping the temperature for 3 minutes to melt the polyolefin and wrap it on the surface of the hollow microspheres;
[0094] C-2) Continue heating to 180°C and keep warm for 3 minutes to allow the polyolefin to react with oxygen in the air to generate oxygen-containing functional groups;
[0095] C-3) Continue heating to the set carbonization temperature of 230°C, carbonize for 40 minutes, and then cool to complete the carbonization.
[0096] The carbonized microsphere intermediates were ball milled to achieve material separation. The ball milling parameters were: revolution 50 / min, rotation 200 / min, ball milling time 6h, and 30% ethanol was added for wet milling.
[0097] ) to sensitize the carbonized microsphere intermediate, immerse the microsphere intermediate or the carbonized microsphere intermediate in 1×10 -2 M of PdSO4 aqueous solution, soak for 10 min, and then use deionized water to clean the excess free substances on the surface.
[0098] E) Exo-plating metal on the exterior of the microsphere intermediate by chemical plating.
[0099] E-1) NaOH, CuSO4, KNaC4H4O6 and water are mixed in a mass ratio of 1:1:2.5:50 to prepare a mixed solution;
[0100] E-2) The sensitized microsphere intermediate is placed in a mixed solution, and then formaldehyde is added, the mass ratio of the sensitized microsphere intermediate to formaldehyde is 30:5, the temperature is 25° C., the pH is 7, the duration is 5 minutes, a chemically plated metal layer is formed, and then washed.
[0101] F) Collect the prepared hollow conductive microspheres.
[0102] The hollow conductive microspheres prepared in this embodiment are of a core-shell structure of microspheres@carbon nanotubes-carbon-nanonickernel@metal.
[0103] Reference Figure 1 The core of the hollow conductive microsphere is the hollow microsphere 1, the exterior of the hollow microsphere 1 is coated with a carbon nanotube-carbon-nano nickel composite layer 2, and the exterior of the carbon nanotube-carbon-nano nickel composite layer 2 is wrapped with a chemically plated metal layer 3.
[0104] The average particle size of the hollow microspheres is 300 nm, the thickness of the carbon nanotube-carbon-nano nickel composite layer is 112 nm, and the thickness of the chemically plated metal layer is 304 nm.
[0105] Example 2
[0106] A method for preparing a conductive paste comprises the following steps:
[0107] 1) The conductive paste comprises the following raw materials in percentage by weight:
[0108] 42 g of hollow conductive microspheres, 42 g of spherical micron copper powder with a particle size of 3 μm, 0.3 g of a binder (polyacrylic resin), 0.3 g of a stabilizer (citric acid), and 9 g of a solvent (deionized water).
[0109] 2) Mixing
[0110] The prepared raw materials are configured and mixed uniformly according to a preset weight percentage, and then added into a three-roll grinder for three-roll differential speed cyclic stripping, the three-roll speed ratio is 1:3:9, the gap between the three rolls is 300 μm, the cyclic stripping is repeated 10 times, and the material is discharged to obtain a conductive paste.
[0111] The preparation method of the hollow conductive microspheres comprises the following steps:
[0112] B) surface modification of hollow microspheres (specifically hollow silica microspheres);
[0113] The hollow microspheres and the silane coupling agent are configured at a weight ratio of 100:4. The hollow microspheres are first dispersed in anhydrous ethanol, and then the silane coupling agent is added, heated, cooled, and separated to obtain surface-modified hollow microspheres.
[0114] B) the surface-modified hollow microspheres are coated with a mixture of polyolefin (low-density polyethylene), single-walled carbon nanotubes with a tube diameter of 5 nm, and nano-nickel powder with a particle diameter of 10 nm, to form a composite layer outside the surface-modified hollow microspheres to prepare a microsphere intermediate;
[0115] The mass ratio of surface-modified hollow microspheres: carbon nanotubes: nano-nickel powder: polyolefin is 20:5:3:50;
[0116] C) Carbonization treatment;
[0117] The carbonization process comprises the following steps:
[0118] C-1) heating the mixture to be carbonized to 155° C. and keeping the temperature for 4 minutes to melt the polyolefin and wrap it on the surface of the hollow microspheres;
[0119] C-2) Continue heating to 195°C and keep warm for 4 minutes to allow the polyolefin to react with oxygen in the air to generate oxygen-containing functional groups;
[0120] C-3) Continue heating to the set carbonization temperature of 250°C, carbonize for 50 minutes, and then cool to complete the carbonization.
[0121] The carbonized microsphere intermediates were ball milled to separate the materials. The ball milling parameters were: revolution 50 / min, rotation 200 / min, ball milling time 6h, and 30% ethanol was added for wet milling.
[0122] D) Sensitizing the microsphere intermediate, immersing the microsphere intermediate or the carbonized microsphere intermediate in 1×10 - 2 M in a PdSO4 aqueous solution for 15 min, and then use deionized water to clean the excess free substances on the surface;
[0123] E) coating the outside of the microsphere intermediate with metal by chemical plating,
[0124] E-1) NaOH, CuSO4, KNaC4H4O6 and water are mixed in a mass ratio of 1:1.5:3.5:50 to prepare a mixed solution;
[0125] E-2) placing the sensitized microsphere intermediate into the mixed solution, and then adding formaldehyde, the mass ratio of the sensitized microsphere intermediate to formaldehyde is 30:5, the temperature is 26° C., the pH is 7, the duration is 6 minutes, to form a chemically plated metal layer, and then washing;
[0126] F) Collect the prepared hollow conductive microspheres.
[0127] The hollow conductive microspheres prepared in this embodiment are of a core-shell structure of microspheres@carbon nanotubes-carbon-nanonickernel@metal.
[0128] Reference Figure 1 The core of the hollow conductive microsphere is the hollow microsphere 1, the exterior of the hollow microsphere 1 is coated with a carbon nanotube-carbon-nano nickel composite layer 2, and the exterior of the carbon nanotube-carbon-nano nickel composite layer 2 is wrapped with a chemically plated metal layer 3.
[0129] Specifically, the average particle size of the hollow microspheres is 300 nm, the thickness of the carbon nanotube-carbon-nano nickel composite layer is 168 nm, and the thickness of the chemically plated metal layer is 348 nm.
[0130] Example 3
[0131] A method for preparing a conductive paste comprises the following steps:
[0132] 1) The conductive paste comprises the following raw materials in percentage by weight:
[0133] 45 g of hollow conductive microspheres, 45 g of spherical micron copper powder with a particle size of 3 μm, 0.5 g of a binder (polyurethane), 0.5 g of a stabilizer (citric acid), and 9 g of a solvent (ethylene glycol).
[0134] 2) Mixing
[0135] The prepared raw materials are configured and mixed uniformly according to a preset weight percentage, and then added into a three-roll grinder for three-roll differential speed cyclic stripping, the three-roll speed ratio is 1:3:9, the gap between the three rolls is 300 μm, the cyclic stripping is repeated 10 times, and the material is discharged to obtain a conductive paste.
[0136] The preparation method of the hollow conductive microspheres comprises the following steps:
[0137] C) surface modification of hollow microspheres (specifically hollow silica microspheres);
[0138] The hollow microspheres and the silane coupling agent are configured at a weight ratio of 100:5. The hollow microspheres are first dispersed in anhydrous ethanol, and then the silane coupling agent is added, heated, cooled, and separated to obtain surface-modified hollow microspheres.
[0139] B) the surface-modified hollow microspheres are coated with a mixture of polyolefin (low-density polyethylene), single-walled carbon nanotubes with a tube diameter of 10 nm, and nano-nickel powder with a particle diameter of 15 nm, to form a composite layer outside the surface-modified hollow microspheres to prepare a microsphere intermediate;
[0140] The mass ratio of surface-modified hollow microspheres: carbon nanotubes: nano-nickel powder: polyolefin is 20:8:1:50;
[0141] C) Carbonization treatment;
[0142] The carbonization process comprises the following steps:
[0143] C-1) heating the mixture to be carbonized to 165° C. and keeping the temperature for 5 minutes to melt the polyolefin and wrap it on the surface of the hollow microspheres;
[0144] C-2) continue heating to 200°C and keep warm for 5 minutes to allow the polyolefin to react with oxygen in the air to generate oxygen-containing functional groups;
[0145] C-3) Continue heating to the set carbonization temperature of 280°C, carbonize for 60 minutes, and then cool to complete the carbonization.
[0146] D) ball milling the carbonized microsphere intermediate to achieve material separation, ball milling parameters: revolution 50 / min, rotation 200 / min, ball milling time 6h, adding concentration of 30% ethanol wet milling;
[0147] E) Sensitizing the microsphere intermediate, immersing the microsphere intermediate or the carbonized microsphere intermediate in 1×10 - 2 M in a PdSO4 aqueous solution for 20 min, and then use deionized water to clean the excess free substances on the surface;
[0148] F) coating the outside of the microsphere intermediate with metal by chemical plating,
[0149] F-1) NaOH, CuSO4, KNaC4H4O6 and water are mixed in a mass ratio of 1:1.5:3:50 to prepare a mixed solution;
[0150] F-2) placing the sensitized microsphere intermediate into the mixed solution, and then adding formaldehyde, the mass ratio of the sensitized microsphere intermediate to formaldehyde is 30:5, the temperature is 27° C., the pH is 7.5, the duration is 7 minutes, to form a chemically plated metal layer, and then washing;
[0151] G) Collect the prepared hollow conductive microspheres.
[0152] The hollow conductive microspheres prepared in this embodiment are of a core-shell structure of microspheres@carbon nanotubes-carbon-nanonickernel@metal.
[0153] Reference Figure 1 The core of the hollow conductive microsphere is the hollow microsphere 1, the exterior of the hollow microsphere 1 is coated with a carbon nanotube-carbon-nano nickel composite layer 2, and the exterior of the carbon nanotube-carbon-nano nickel composite layer 2 is wrapped with a chemically plated metal layer 3.
[0154] Specifically, the average particle size of the hollow microspheres is 300 nm, the thickness of the carbon nanotube-carbon-nano nickel composite layer is 202 nm, and the thickness of the chemically plated metal layer is 411 nm.
[0155] Example 4
[0156] A method for preparing a conductive paste comprises the following steps:
[0157] 1) The conductive paste comprises the following raw materials in percentage by weight:
[0158] 48 g of hollow conductive microspheres, 48 g of spherical micron copper powder with a particle size of 3 μm, 0.8 g of a binder (epoxy resin), 0.8 g of a stabilizer (glycine), and 10 g of a solvent (deionized water).
[0159] 2) Mixing
[0160] The prepared raw materials are configured and mixed uniformly according to a preset weight percentage, and then added into a three-roll grinder for three-roll differential speed cyclic stripping, the three-roll speed ratio is 1:3:9, the gap between the three rolls is 300 μm, the cyclic stripping is repeated 10 times, and the material is discharged to obtain a conductive paste.
[0161] The preparation method of the hollow conductive microspheres comprises the following steps:
[0162] D) surface modification of hollow microspheres (specifically hollow silica microspheres);
[0163] The hollow microspheres and the silane coupling agent are configured at a weight ratio of 100:6. The hollow microspheres are first dispersed in anhydrous ethanol, and then the silane coupling agent is added, heated, cooled, and separated to obtain surface-modified hollow microspheres.
[0164] B) the surface-modified hollow microspheres are coated with a mixture of polyolefin (low-density polyethylene), single-walled carbon nanotubes with a diameter of 15 nm, and nano-nickel powder with a particle size of 20 nm, to form a composite layer outside the surface-modified hollow microspheres to prepare a microsphere intermediate;
[0165] The mass ratio of surface-modified hollow microspheres: carbon nanotubes: nano-nickel powder: polyolefin is 20:8:3:50;
[0166] C) Carbonization treatment;
[0167] The carbonization process comprises the following steps:
[0168] C-1) heating the mixture to be carbonized to 170° C. and keeping the temperature for 8 minutes to melt the polyolefin and wrap it on the surface of the hollow microspheres;
[0169] C-2) Continue heating to 210°C and keep warm for 8 minutes to allow the polyolefin to react with oxygen in the air to generate oxygen-containing functional groups;
[0170] C-3) Continue heating to the set carbonization temperature of 300°C, carbonize for 70 minutes, and then cool to complete the carbonization.
[0171] The carbonized microsphere intermediates were ball milled to separate the materials. The ball milling parameters were: revolution 50 / min, rotation 200 / min, ball milling time 6h, and 30% ethanol was added for wet milling.
[0172] D) Sensitizing the microsphere intermediate, immersing the microsphere intermediate or the carbonized microsphere intermediate in 1×10 - 2 M in a PdSO4 aqueous solution for 20 min, and then use deionized water to clean the excess free substances on the surface;
[0173] E) coating the outside of the microsphere intermediate with metal by chemical plating,
[0174] E-1) NaOH, CuSO4, KNaC4H4O6 and water are mixed in a mass ratio of 1:1.5:4:50 to prepare a mixed solution;
[0175] E-2) The sensitized microsphere intermediate was placed in the mixed solution, and then formaldehyde was added, the mass ratio of the sensitized microsphere intermediate to formaldehyde was 30:5, the temperature was 28° C., the pH was 7.5, and the duration was 9 minutes.
[0176] Forming a chemically plated metal layer and cleaning;
[0177] F) Collect the prepared hollow conductive microspheres.
[0178] The hollow conductive microspheres prepared in this embodiment are of a core-shell structure of microspheres@carbon nanotubes-carbon-nanonickernel@metal.
[0179] Reference Figure 1 The core of the hollow conductive microsphere is the hollow microsphere 1, the exterior of the hollow microsphere 1 is coated with a carbon nanotube-carbon-nano nickel composite layer 2, and the exterior of the carbon nanotube-carbon-nano nickel composite layer 2 is wrapped with a chemically plated metal layer 3.
[0180] Specifically, the average particle size of the hollow microspheres is 300 nm, the thickness of the carbon nanotube-carbon-nano nickel composite layer is 246 nm, and the thickness of the chemically plated metal layer is 441 nm.
[0181] Example 5
[0182] A method for preparing a conductive paste comprises the following steps:
[0183] 1) The conductive paste comprises the following raw materials in percentage by weight:
[0184] 50g of hollow conductive microspheres, 50g of spherical micron copper powder with a particle size of 3μm, 1g of a binder (acrylic resin, polyacrylic resin, polyurethane, epoxy resin, amino resin), 1g of a stabilizer (ascorbic acid), and 15g of a solvent (ethylene glycol).
[0185] 2) Mixing
[0186] The prepared raw materials are configured and mixed uniformly according to a preset weight percentage, and then added into a three-roll grinder for three-roll differential speed cyclic stripping, the three-roll speed ratio is 1:3:9, the gap between the three rolls is 300 μm, the cyclic stripping is repeated 10 times, and the material is discharged to obtain a conductive paste.
[0187] The preparation method of the hollow conductive microspheres comprises the following steps:
[0188] E) surface modification of hollow microspheres (specifically hollow silica microspheres);
[0189] The hollow microspheres and the silane coupling agent are configured at a weight ratio of 100:5. The hollow microspheres are first dispersed in anhydrous ethanol, and then the silane coupling agent is added, heated, cooled, and separated to obtain surface-modified hollow microspheres.
[0190] B) the surface-modified hollow microspheres are coated with a mixture of polyolefin (low-density polyethylene), single-walled carbon nanotubes with a diameter of 20 nm, and nano-nickel powder with a particle size of 25 nm, to form a composite layer outside the surface-modified hollow microspheres to prepare a microsphere intermediate;
[0191] The mass ratio of the surface-modified hollow microspheres: carbon nanotubes: nano-nickel powder: polyolefin is 20:10:3:50;
[0192] C) Carbonization treatment;
[0193] The carbonization process comprises the following steps:
[0194] C-1) heating the mixture to be carbonized to 180° C. and keeping the temperature for 10 minutes to melt the polyolefin and wrap it on the surface of the hollow microspheres;
[0195] C-2) Continue heating to 230°C and keep warm for 10 minutes to allow the polyolefin to react with oxygen in the air to generate oxygen-containing functional groups;
[0196] C-3) Continue heating to a set carbonization temperature of 330°C, carbonize for 100 minutes, and then cool to complete the carbonization.
[0197] The carbonized microsphere intermediates were ball milled to separate the materials. The ball milling parameters were: revolution 50 / min, rotation 200 / min, ball milling time 6h, and 30% ethanol was added for wet milling.
[0198] D) Sensitizing the microsphere intermediate, immersing the microsphere intermediate or the carbonized microsphere intermediate in 1×10 - 2 M in a PdSO4 aqueous solution for 25 min, and then use deionized water to clean the excess free substances on the surface;
[0199] E) coating the outside of the microsphere intermediate with metal by chemical plating,
[0200] E-1) NaOH, CuSO4, KNaC4H4O6 and water are mixed in a mass ratio of 1:2:5:50 to prepare a mixed solution;
[0201] E-2) The sensitized microsphere intermediate was placed in the mixed solution, and then formaldehyde was added, the mass ratio of the sensitized microsphere intermediate to formaldehyde was 30:5, the temperature was 30° C., the pH was 8, and the duration was 10 minutes.
[0202] Forming a chemically plated metal layer and cleaning;
[0203] F) Collect the prepared hollow conductive microspheres.
[0204] The hollow conductive microspheres prepared in this embodiment are of a core-shell structure of microspheres@carbon nanotubes-carbon-nanonickernel@metal.
[0205] Reference Figure 1 The core of the hollow conductive microsphere is the hollow microsphere 1, the exterior of the hollow microsphere 1 is coated with a carbon nanotube-carbon-nano nickel composite layer 2, and the exterior of the carbon nanotube-carbon-nano nickel composite layer 2 is wrapped with a chemically plated metal layer 3.
[0206] Specifically, the average particle size of the hollow microspheres is 300 nm, the thickness of the carbon nanotube-carbon-nano nickel composite layer is 284 nm, and the thickness of the chemically plated metal layer is 495 nm.
[0207] Example 6
[0208] A method for preparing a conductive paste comprises the following steps:
[0209] 1) The conductive paste comprises the following raw materials in percentage by weight:
[0210] 45 g of hollow conductive microspheres, 45 g of spherical micron copper powder with a particle size of 3 μm, 0.5 g of a binder (polyurethane), 0.5 g of a stabilizer (citric acid), and 9 g of a solvent (ethylene glycol).
[0211] 2) Mixing
[0212] The prepared raw materials are configured and mixed uniformly according to a preset weight percentage, and then added into a three-roll grinder for three-roll differential speed cyclic stripping, the three-roll speed ratio is 1:3:9, the gap between the three rolls is 300 μm, the cyclic stripping is repeated 10 times, and the material is discharged to obtain a conductive paste.
[0213] The preparation method of the hollow conductive microspheres comprises the following steps:
[0214] F) surface modification of hollow microspheres (specifically hollow silica microspheres);
[0215] The hollow microspheres and the silane coupling agent are configured at a weight ratio of 100:5. The hollow microspheres are first dispersed in anhydrous ethanol, and then the silane coupling agent is added, heated, cooled, and separated to obtain surface-modified hollow microspheres.
[0216] B) The surface-modified hollow microspheres are coated with a mixture of polyolefin (low-density polyethylene), single-walled carbon nanotubes with a tube diameter of 15 nm, and nano-nickel powder with a particle diameter of 20 nm, to form a composite layer outside the surface-modified hollow microspheres;
[0217] The mass ratio of surface-modified hollow microspheres: carbon nanotubes: nano-nickel powder: polyolefin is 20:8:1:50;
[0218] The materials in step B) are preliminarily crushed and mixed, and then spheroidized by a jet mill until the particle size is 2 to 3 times that of the hollow microspheres to prepare a microsphere intermediate;
[0219] C) Sensitize the microsphere intermediate by immersing the microsphere intermediate in 1×10 -2 M in a PdSO4 aqueous solution for 20 min, and then use deionized water to clean the excess free substances on the surface;
[0220] D) coating the outside of the microsphere intermediate with metal by chemical plating,
[0221] D-1) NaOH, CuSO4, KNaC4H4O6 and water are mixed in a mass ratio of 1:1.5:3.5:50 to prepare a mixed solution;
[0222] D-2) placing the sensitized microsphere intermediate into the mixed solution, and then adding formaldehyde, the mass ratio of the sensitized microsphere intermediate to formaldehyde is 30:5, the temperature is 29° C., the pH is 8, the duration is 7 minutes, to form a chemically plated metal layer, and then washing;
[0223] E) carbonization treatment, comprising the following steps:
[0224] E-1) heating the mixture to be carbonized to 165° C. and keeping the temperature for 5 minutes to melt the polyolefin and wrap it on the surface of the hollow microspheres;
[0225] E-2) Continue heating to 200°C and keep warm for 5 minutes to allow the polyolefin to react with oxygen in the air to generate oxygen-containing functional groups;
[0226] E-3) Continue heating to the set carbonization temperature of 280°C, carbonize for 60 minutes, and then cool to complete the carbonization.
[0227] F) Collect the prepared hollow conductive microspheres.
[0228] The hollow conductive microspheres prepared in this embodiment are of a core-shell structure of microspheres@carbon nanotubes-carbon-nanonickernel@metal.
[0229] The core of the hollow conductive microsphere is the hollow microsphere, the exterior of the hollow microsphere is coated with a carbon nanotube-carbon-nano nickel composite layer, and the exterior of the carbon nanotube-carbon-nano nickel composite layer is coated with a chemically plated metal layer.
[0230] Specifically, the average particle size of the hollow microspheres is 300 nm, the thickness of the carbon nanotube-carbon-nano nickel composite layer is 217 nm, and the thickness of the chemically plated metal layer is 429 nm.
[0231] Comparative Example 1
[0232] A method for preparing a conductive paste comprises the following steps:
[0233] 1) The conductive paste comprises the following raw materials in percentage by weight:
[0234] 45 g of copper powder with a particle size of 300 nm, 45 g of spherical micron copper powder with a particle size of 3 μm, 0.5 g of a binder (polyurethane), 0.5 g of a stabilizer (citric acid), and 9 g of a solvent (ethylene glycol).
[0235] 2) Mixing
[0236] The prepared raw materials are configured and mixed uniformly according to a preset weight percentage, and then added into a three-roll grinder for three-roll differential speed cyclic stripping, the three-roll speed ratio is 1:3:9, the gap between the three rolls is 300 μm, the cyclic stripping is repeated 10 times, and the material is discharged to obtain a conductive paste.
[0237] Performance Testing
[0238] (1) Scanning electron microscope test
[0239] The hollow conductive microspheres prepared in Examples 1 to 6 were observed and photographed using a SEM scanning electron microscope.
[0240] The electron microscope images of Examples 1 to 5 are highly similar, and Example 3 is used as an example. Figure 2 As shown, the present invention successfully prepared hollow conductive microspheres, and the process stability was excellent, and the surface was slightly rough; the hollow conductive microspheres prepared in Example 6 were as shown in Figure 3 As shown, the microspheres have a higher degree of shape preservation and a higher particle size roundness, which is beneficial to ensure the fluidity of the conductive paste prepared subsequently, but the preparation cost is slightly increased compared to Examples 1 to 5.
[0241] (2) Sheet resistance and magnetic permeability test
[0242] (2-1) Examples 1 to 5 and Comparative Example 1 were leveled in a mold, respectively, and then placed in an oven at 180° C. to dry to form conductive films of the same thickness. The square resistance of the different conductive films was tested by a four-probe method.
[0243] (2-2) A small circular ring is cut out of the conductive film made in Example 3, and the changes in the resonant frequency and Q value before and after the small circular ring is placed are measured by the coaxial resonant cavity method. The real part re and the imaginary part im of the magnetic permeability are then calculated, and a curve graph of the change in magnetic permeability with frequency is prepared.
[0244] Results of Test (2-1) Figure 4 As shown in the figure, it can be seen that when the frequency is appropriate, the square resistance of Examples 1 to 5 all have an obvious minimum value. Combined with the test (2-2) results (i.e. Figure 5 ), when the normal operating frequency is 12 GHz, the magnetic permeability of the conductive film prepared in Example 3 is only about -5, that is, the entire conductive layer shows a non-proportional relationship between the magnetic permeability and the frequency. At the same time, the lower the magnetic permeability, the higher the skin depth, and the less obvious the skin effect. That is, the conductive film prepared in Example 3 is in a high conduction state at this time, indicating that the conductive slurry of the present invention can effectively increase the skin depth to weaken the skin effect, thereby solving the signal loss problem caused by the skin effect of the conductive layer in high-frequency and high-speed circuits.
[0245] According to the disclosure and teaching of the above description, those skilled in the art to which the present invention belongs may also change and modify the above implementation modes. Therefore, the present invention is not limited to the specific implementation modes disclosed and described above, and some modifications and changes to the present invention should also fall within the protection scope of the claims of the present invention. In addition, although some specific terms are used in this specification, these terms are only for the convenience of description and do not constitute any limitation to the present invention.
Claims
1. A method for preparing a conductive paste, characterized in that: The following steps are involved: 1) The conductive paste includes the following raw materials in percentage by weight: 40-50wt% of hollow conductive microspheres, 40-50wt% of micron metal powder, 0.1-5wt% of binder, 0.01-3wt% of stabilizer and 9-30wt% of solvent; 2) Mixing The prepared raw materials are configured according to a preset weight percentage and mixed evenly, and the materials are discharged after being fully ground to obtain a conductive paste.
2. The method for preparing a conductive paste according to claim 1, characterized in that: The preparation method of the hollow conductive microspheres comprises the following steps: A) surface modification of hollow microspheres; B) coating the surface-modified hollow microspheres with a mixture of polyolefin, carbon nanotubes and nano-nickel powder to form a composite layer outside the surface-modified hollow microspheres to prepare a microsphere intermediate; The mass ratio of the surface-modified hollow microspheres: carbon nanotubes: nano nickel powder: polyolefin is 15-25: 5-10: 1-3: 45-55; C) sensitizing the microsphere intermediate, plating the sensitized microsphere intermediate with metal by chemical plating to form a chemically plated metal layer, and washing; D) collecting and preparing hollow conductive microspheres; A carbonization treatment is provided between step B) and step C), or a carbonization treatment is provided between step C) and step D); The carbonization treatment at least includes carbonization at a carbonization temperature of 230 to 330° C. for 5 to 120 minutes.
3. The method for preparing the conductive paste according to claim 2, characterized in that: The preparation method of the hollow conductive microspheres comprises the following steps: A) surface modification of hollow microspheres; B) coating the surface-modified hollow microspheres with a mixture of polyolefin, carbon nanotubes and nano-nickel powder to form a composite layer outside the surface-modified hollow microspheres to prepare a microsphere intermediate; The mass ratio of the surface-modified hollow microspheres: carbon nanotubes: nano nickel powder: polyolefin is 15-25: 5-10: 1-3: 45-55; Carbonization treatment; ball milling; C) sensitizing the microsphere intermediate, and then plating metal on the outside of the microsphere intermediate by chemical plating to form a chemically plated metal layer, and washing; D) Collect the prepared hollow conductive microspheres.
4. The method for preparing a conductive paste according to claim 2, characterized in that: The preparation method of the hollow conductive microspheres comprises the following steps: A) surface modification of hollow microspheres; B) coating the surface-modified hollow microspheres with a mixture of polyolefin, carbon nanotubes and nano-nickel powder to form a composite layer outside the surface-modified hollow microspheres to prepare a microsphere intermediate; The mass ratio of the surface-modified hollow microspheres: carbon nanotubes: nano nickel powder: polyolefin is 15-25: 5-10: 1-3: 45-55; The above materials are preliminarily crushed and mixed, and then spheroidized by a jet mill until the particle size is 2 to 3 times that of the hollow microspheres; C) sensitizing the microsphere intermediate, and then plating metal on the outside of the microsphere intermediate by chemical plating to form a chemically plated metal layer, and washing; Carbonization treatment; D) Collect and make hollow conductive microspheres.
5. The method for preparing a conductive paste according to any one of claims 2 to 4, characterized in that: The carbonization process comprises the following steps: 1) heating the mixture to be carbonized to 150-180° C. and keeping the temperature for 1-10 minutes; 2) Continue heating to 180-230°C and keep warm for 1-10 minutes; 3) Continue heating to the set carbonization temperature of 230-330°C, carbonize for 5-120 minutes, and complete the carbonization after cooling.
6. The method for preparing a conductive paste according to claim 2 or 3, characterized in that: In step B), the average particle size of the nano nickel powder is 10-25 nm, the carbon nanotubes are single-walled carbon nanotubes, and the average particle size of the nano nickel powder is greater than the diameter of the carbon nanotubes.
7. The method for preparing a conductive paste according to claim 2 or 3, characterized in that: In step C), the specific operation of the sensitization is: immersing the microsphere intermediate or the carbonized microsphere intermediate in 1×10 -2 M of PdSO4 aqueous solution, soaking time is 10 to 30 minutes.
8. The method for preparing a conductive paste according to claim 2 or 3, characterized in that: In step C), the specific operation of the chemical plating is: 1) NaOH, metal salt, KNaC4H4O6 and water are mixed in a mass ratio of 1:1-2:2.5-5:50 to prepare a mixed solution; 2) Put the sensitized microsphere intermediate into the mixed solution, and then add formaldehyde, the mass ratio of the sensitized microsphere intermediate to formaldehyde is 30:5, the temperature is 25-30° C., the pH is 7-8 weak alkaline, and the duration is 5-10 minutes.
9. The method for preparing a conductive paste according to any one of claims 1 to 4, characterized in that: The hollow conductive microspheres are of a core-shell structure of microspheres@carbon nanotubes-carbon-nano nickel@metal.
10. The method for preparing a conductive paste according to claim 9, characterized in that: The core of the hollow conductive microsphere is the hollow microsphere, the exterior of the hollow microsphere is coated with a carbon nanotube-carbon-nano nickel composite layer, and the exterior of the carbon nanotube-carbon-nano nickel composite layer is coated with a chemically plated metal layer; The average particle size of the hollow microspheres is 100-500nm, the thickness of the carbon nanotube-carbon-nano nickel composite layer is 100-300nm, and the thickness of the chemically plated metal layer is 300-600nm.