Linear NTC thermistor and preparation method thereof
By adding RuO2 to the ZnO linear resistor and adjusting the ratio of ZnO to Al2O3, a linear NTC thermistor with NTC effect was prepared, which solved the problem of large changes in resistance value, and realized the adjustable and controllable resistivity and temperature coefficient. , expanding the application range of ZnO ceramic resistors.
Patent Information
- Application Number
- CN202411226021.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-11-08
AI Technical Summary
The resistance value of existing NTC thermistors varies greatly with temperature, and it is not easy to perform sampling and calculation processing during application. Few ZnO ceramic resistors become resistors with NTC effect, limiting their application range.
By adding RuO2 to the ZnO linear resistor and adjusting the ratio of ZnO to Al2O3, a linear NTC thermistor with NTC effect is prepared, so as to achieve adjustable and controllable resistivity and temperature coefficient.
The NTC effect of ZnO ceramic resistor is realized, making it available for both NTC temperature sensors and linear resistor components, improving application value and flexibility in use.
Smart Images

Figure CN118919194A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of linear NTC thermistors, in particular to a linear NTC thermistor and a preparation method thereof. Background Art
[0002] ZnO ceramic resistors can be divided into ZnO varistors and ZnO linear resistors. ZnO varistors are key components of lightning arresters, which utilize the high-energy barrier at grain boundaries to reduce lightning voltage and play a role in lightning protection. ZnO linear resistors are obtained by adding oxides such as Al2O3 and MgO to reduce the grain boundary barrier of ZnO varistors, and are mainly used in circuit breakers of power equipment.
[0003] NTC thermistors are important components of temperature sensors and play a role in temperature detection and control. However, the resistance value of conventional NTC thermistors varies greatly with temperature, making it difficult to perform sampling calculation processing during application. It is necessary to design a circuit to linearize the thermistor so that the R-T curve (the curve of the resistance value changing with temperature, which is usually not linear but shows an exponential relationship) becomes almost a straight line, and then use it after reducing the variation range. This causes great inconvenience in the use of NTC thermistors, so linear NTC thermistors came into being. The R-T curve of a linear NTC thermistor is a straight line, which is the main feature distinguishing it from conventional NTCs.
[0004] Currently, there are few studies on turning ZnO ceramic resistors into resistors with NTC effects and making them into linear NTC thermistors. Such research and practice will greatly expand the application of ZnO ceramic resistors and improve their use value. Summary of the Invention
[0005] Embodiments of the present invention provide a linear NTC thermistor and a preparation method thereof to solve the above problems in the prior art.
[0006] The present invention discloses a preparation method of a linear NTC thermistor, including the steps of:
[0007] By mass percentage, according to the component ratio of (85 + y)ZnO - (10 - y)Al2O3 - (5 - x)MgO (where 0 ≤ y ≤ 5, 0 < x < 1), weigh the raw materials of ZnO, Al2O3, and MgO oxides, perform primary ball milling and drying to obtain dry powder;
[0008] Calcine the dry powder to obtain a calcined powder;
[0009] By mass percentage, according to the component ratio of xRuO2 (where 0 < x < 1), add a Ru element-containing raw material to the calcined powder to obtain a mixed powder;
[0010] The mixed powder is subjected to secondary ball milling, drying and dry pressing, cold isostatic pressing, sintering, slicing, electrode printing, and dicing to obtain a linear NTC thermistor.
[0011] Optionally, the steps of subjecting the mixed powder to secondary ball milling, drying and dry pressing, cold isostatic pressing, sintering, slicing, printing electrodes, and scribing to obtain a linear NTC thermistor are specifically as follows:
[0012] The mixed powder is ball-milled for a second time and dried to obtain a mixed powder;
[0013] The mixed powder is subjected to dry pressing and cold isostatic pressing to obtain a green body;
[0014] The green body is sintered to obtain an oxide ceramic block;
[0015] Slicing the ceramic block to obtain ceramic sheets;
[0016] Printing the electrode slurry on the ceramic sheet and solidifying the electrode by sintering;
[0017] The electrode-containing ceramic sheet is diced to obtain a linear NTC thermistor.
[0018] Optionally, the ZnO, Al2O3 and MgO oxide raw materials are all analytically pure.
[0019] Optionally, the raw material containing Ru element is a simple substance or an oxide.
[0020] Optionally, the drying temperature after the first ball milling is 80-100° C. and the drying time is 12-24 hours.
[0021] Optionally, the drying temperature after the secondary ball milling is 80-100° C. and the drying time is 12-24 hours.
[0022] Optionally, the dry powder is calcined at a temperature of 800 to 1000° C. for 3 to 8 hours.
[0023] Optionally, the cold isostatic pressing pressure is 300 MPa.
[0024] Optionally, the sintering temperature of the green body is 1200-1400° C., the temperature is kept for 3-10 hours, and the sintering atmosphere is air atmosphere.
[0025] The present invention also discloses a linear NTC thermistor, wherein the linear NTC thermistor is based on ZnO and has a composition of (85+y)ZnO-(10-y)Al2O3-(5-x)MgO-xRuO2, wherein 0≤y≤5, 0 <x<1。
[0026] Compared with the prior art, the beneficial effects of the preparation method of the linear NTC thermistor provided by the embodiment of the present invention are as follows: In the preparation method of the present invention, based on the ZnO linear resistor, a small amount of RuO2 is added to make it a thermistor with NTC effect; then by changing the ratio of ZnO to Al2O3, it is made into a linear NTC thermistor with adjustable resistivity and controllable TCR. This ZnO ceramic resistor can be used both in NTC temperature sensor devices and in linear resistor elements. By adjusting the value of variable x, the ZnO ceramic resistor can be made into a linear NTC thermistor with NTC effect, and by changing the value of variable y, the resistivity and TCR of the NTC thermistor can be adjusted to be adjustable and controllable. Therefore, adding RuO2 makes the ZnO ceramic resistor into a linear resistor with NTC effect, and changing the ratio of ZnO to Al2O3 can adjust the electrical properties of this linear NTC thermistor. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] The technical solutions of the present invention will be further described in detail below with reference to the drawings and embodiments. In the drawings:
[0028] Figure 1 is the R-T curve diagram of the linear NTC thermistor under different RuO2 addition amounts in Embodiments 1-6 of the present invention;
[0029] Figure 2 is the data diagram of the TCR magnitudes of the linear NTC thermistors in Embodiments 1-6 of the present invention in the oil bath at three temperature ranges. DETAILED DESCRIPTION OF THE EMBODIMENTS
[0030] It should be noted that, without conflict, the embodiments in the present application and the features in the embodiments can be combined with each other. Now, with reference to the drawings, the preferred embodiments of the present invention will be described in detail.
[0031] The embodiment of the present invention provides a preparation method of a linear NTC thermistor. The preparation method of the linear NTC thermistor includes the steps:
[0032] By mass percentage, according to the component ratio of (85 + y)ZnO - (10 - y)Al2O3 - (5 - x)MgO (where 0 ≤ y ≤ 5, 0 < x < 1), weigh the oxide raw materials of ZnO, Al2O3, and MgO, and perform primary ball milling and drying to obtain dry powder;
[0033] Calcine the dry powder to obtain a calcined powder;
[0034] By mass percentage, according to the component ratio of xRuO2 (where 0 < x < 1), add the raw material containing Ru element to the calcined powder to obtain a mixed powder;
[0035] The mixed powder is subjected to secondary ball milling, drying and dry pressing, cold isostatic pressing, sintering, slicing, electrode printing, and dicing to obtain a linear NTC thermistor.
[0036] Conventional ZnO ceramic resistors use ZnO as the matrix, and add oxides such as Al2O3 and MgO to reduce the grain boundary barrier of ZnO to obtain ZnO linear resistors. In the preparation method of the present invention, based on the ZnO linear resistor, a small amount of RuO2 is added to make it a thermistor with NTC effect; then by changing the ratio of ZnO to Al2O3, it becomes a linear NTC thermistor with adjustable resistivity and controllable TCR. The ZnO ceramic resistor can be used for both NTC temperature sensor devices and linear resistor elements. The ZnO ceramic resistor can be turned into a linear NTC thermistor with NTC effect by adjusting the value of variable x, and the resistivity and TCR of the NTC thermistor can be adjusted by changing the value of variable y, making it adjustable and controllable. Therefore, adding RuO2 turns the ZnO ceramic resistor into a linear resistor with NTC effect, and changing the ratio of ZnO to Al2O3 can adjust the electrical properties of the linear NTC thermistor.
[0037] Specifically, the steps of subjecting the mixed powder to secondary ball milling, drying and dry pressing, cold isostatic pressing, sintering, slicing, printing electrodes, and scribing to obtain a linear NTC thermistor are as follows:
[0038] The mixed powder is ball-milled for a second time and dried to obtain a mixed powder;
[0039] The mixed powder is subjected to dry pressing and cold isostatic pressing to obtain a green body; wherein the size of the green body is 50 mm×50 mm×15 mm;
[0040] The green body is sintered to obtain an oxide ceramic block;
[0041] The ceramic block is sliced to obtain a ceramic sheet, and the thickness of the ceramic sheet is 0.5 mm;
[0042] Printing electrode slurry on a ceramic sheet and solidifying the electrode by sintering; wherein the electrode slurry is silver slurry and the sintered and solidified electrode is a silver electrode;
[0043] The electrode-containing ceramic sheet is diced to obtain a linear NTC thermistor, wherein the size of the linear NTC thermistor is 1.0 mm×1.0 mm×0.5 mm.
[0044] Furthermore, the ZnO, Al2O3, and MgO oxide raw materials are all analytically pure. High-purity raw materials are crucial for the preparation of electronic components such as thermistors, because the presence of impurities may affect the material properties during the preparation process and the performance of the final product. The use of high-purity oxide raw materials can ensure that the prepared thermistors have stable quality and reliable performance, and avoiding the presence of impurities can reduce the impact on material properties. The use of analytically pure oxide raw materials can reduce uncertainty in the preparation process, help ensure the repeatability of the preparation process, so that each batch of products has similar performance and characteristics, and improve the stability and reliability of the product.
[0045] The raw material containing Ru (ruthenium) element is a simple substance or an oxide. The flexibility of using either a simple substance or an oxide can select the form of adding Ru element according to specific requirements to achieve the required electrical performance adjustment. The source of adding Ru element includes both simple Ru and Ru oxide. This flexibility helps to adjust the performance of linear NTC thermistor according to specific needs, thereby meeting the requirements of different application scenarios.
[0046] The drying temperature after the first ball milling is 80-100°C, and the time is 12-24h. The drying step after the first ball milling provides necessary pre-treatment for the preparation process, which helps to ensure the quality and stability of the final product. The drying process helps to remove moisture from the powder, minimize the interference caused by the presence of moisture, better control the stability and consistency of the preparation process, and avoid changes or instability in material properties in subsequent steps. Drying at a temperature of 80-100°C helps to drive off moisture at a lower temperature while avoiding excessive impact on other properties of the material; the drying time of 12-24 hours allows the material to be fully dried to ensure its stability and consistency. For example, the drying temperature after one ball milling can be any one of 80°C, 82°C, 84°C, 86°C, 88°C, 90°C, 92°C, 94°C, 96°C, 98°C, and 100°C, and the drying time can be any one of 12h, 13h, 14h, 15h, 16h, 17h, 18h, 19h, 20h, 21h, 22h, 23h, and 24h.
[0047] Specifically, the drying temperature after the secondary ball milling is 80-100°C, and the time is 12-24h. The drying conditions after the secondary ball milling are similar to those after the primary ball milling, both of which are to ensure the stability and consistency of the material during the preparation process, so as to obtain high-quality linear NTC thermistor products. Specifically, drying after the secondary ball milling helps to further reduce the residual humidity and ensure the stability of the material in subsequent processing. Drying can improve the uniformity of the powder, so that the material is more evenly heat-treated, which is beneficial to the subsequent process. Through secondary drying, the influence of moisture on the material properties and reactions can be effectively reduced, providing better conditions for the next process, and controlling the time range of 12 to 24 hours to ensure that the material is fully dried while avoiding the negative effects of excessive drying. For example, the drying temperature after the secondary ball milling can be any one of 80°C, 82°C, 84°C, 86°C, 88°C, 90°C, 92°C, 94°C, 96°C, 98°C, and 100°C, and the drying time can be any one of 12h, 13h, 14h, 15h, 16h, 17h, 18h, 19h, 20h, 21h, 22h, 23h, and 24h.
[0048] The calcination temperature of the dry powder calcination is 800-1000°C, and the heat preservation is 3-8 hours. The calcination step provides a necessary prerequisite for adjusting the structure and performance of the material and ensuring the quality of the product. By controlling the calcination temperature and time, the desired material properties and resistance characteristics can be achieved. High-temperature calcination helps the growth of grains and the improvement of crystallinity, which in turn affects the physicochemical properties of the material, and also helps the volatilization and decomposition of impurities and improves the purity of the material. Temperature control during the calcination process can improve the stability of the material, eliminate residual organic matter or gas, and ensure the stability and consistency of the product. By controlling the temperature and time during the calcination process, the resistance characteristics of the material can be adjusted to meet the needs and improve the functionality of the product. Calcination within a certain temperature range may cause changes in the crystal phase, which has an important impact on the performance of the material. For example, the calcination temperature can be any one of 800°C, 820°C, 840°C, 860°C, 880°C, 900°C, 920°C, 940°C, 960°C, 980°C, and 1000°C, and the insulation time can be any one of 3h, 3.5h, 4h, 4.5h, 5h, 5.5h, 6h, 6.5h, 7h, 7.5h, and 8h.
[0049] Furthermore, the pressure of the cold isostatic pressing is 300MPa. The main purpose of cold isostatic pressing is to press the powder under high pressure at room temperature to improve the density and mechanical properties of the material. The cold isostatic pressing pressure of 300MPa is determined according to the specific material and product requirements of this scheme, and this step can improve the performance and quality of the material. The cold isostatic pressing pressure is 300MPa, and this pressure can affect the densification degree of the material and the performance of the final product. Specifically, the high pressure of this scheme can effectively reduce the porosity and increase the density of the material, thereby improving the mechanical properties and thermal conductivity of the material. Appropriate pressure helps the bonding between powder particles, making it easier for the material to form a uniform structure during sintering. Through high-pressure pressing, the pores and defects in the material can be reduced, and the quality and stability of the material can be improved. High-pressure treatment can improve the strength and hardness of the material, making the final product more wear-resistant and corrosion-resistant.
[0050] The sintering temperature of the green body is 1200-1400°C, and the insulation time is 3-10 hours, and the sintering atmosphere is an air atmosphere. Sintering is a very important step in the ceramic preparation process, which can combine the powder green body into a dense bulk material at high temperature. By controlling the sintering temperature, insulation time and atmosphere, the crystal structure, density and performance of the material can be adjusted to ensure that the final product has the required quality and characteristics. For example, the sintering temperature can be any of 1200°C, 1250°C, 1300°C, 1350°C, and 1400°C, and the insulation time can be any of 3h, 3.5h, 4h, 4.5h, 5h, 5.5h, 6h, 6.5h, 7h, 7.5h, 8h, 8.5h, 9h, 9.5h, and 10h.
[0051] Specifically, the sintering and curing silver electrode has a temperature of 800-1000°C and a time of 10-20 minutes. The main purpose of sintering and curing the silver electrode in preparation is to firmly bond the silver electrode to the substrate material to improve the conductivity and overall stability. Taking into account the influence of sintering temperature and time, proper control of these parameters can ensure the quality, performance and stability of the cured silver electrode, which is one of the key steps in preparing high-quality devices. Lower temperatures may result in incomplete curing and low electrode bonding strength. Higher temperatures may cause the electrode and the ceramic sheet to diffuse with each other, resulting in structural changes or material damage. In this scheme, by selecting a suitable sintering temperature in the range of 800-1000°C, a uniform and firm bond between the electrode and the ceramic sheet can be achieved. The length of the sintering time affects the adequacy and firmness of the electrode curing. A shorter time may result in insufficient electrode curing, affecting the conductivity and stability of the electrode. A longer time may increase cost and energy consumption, and may also affect other properties. By selecting an appropriate sintering time in the range of 2-5 hours, a good bond between the silver electrode and the ceramic sheet can be achieved, and manufacturing efficiency and quality can be maintained.
[0052] Specifically, the sintering and curing electrode temperature can be any one of 800°C, 820°C, 840°C, 860°C, 880°C, 900°C, 920°C, 940°C, 960°C, 980°C, and 1000°C, and the time can be any one of 10 min, 11 min, 12 min, 13 min, 14 min, 15 min, 16 min, 17 min, 18 min, 19 min, and 20 min.
[0053] The present invention also discloses a linear NTC thermistor. The linear NTC thermistor is based on ZnO and has a composition of (85+y)ZnO-(10-y)Al2O3-(5-x)MgO-xRuO2, wherein 0≤y≤5, 0 <x<1。
[0054] Conventional ZnO ceramic resistors use ZnO as the matrix, and add oxides such as Al2O3 and MgO to reduce the grain boundary barrier of ZnO to obtain ZnO linear resistors. The linear NTC thermistor of the present invention is based on the ZnO linear resistor, and a small amount of RuO2 is added to make it a thermistor with NTC effect; then by changing the ratio of ZnO to Al2O3, it becomes a linear NTC thermistor with adjustable resistivity and controllable TCR. The ZnO ceramic resistor can be used for both NTC temperature sensor devices and linear resistor elements. The ZnO ceramic resistor can be turned into a linear NTC thermistor with NTC effect by adjusting the value of variable x, and the resistivity and TCR of the NTC thermistor can be adjusted by changing the value of variable y, making it adjustable and controllable. Therefore, adding RuO2 turns the ZnO ceramic resistor into a linear resistor with NTC effect, and changing the ratio of ZnO to Al2O3 can adjust the electrical properties of the linear NTC thermistor.
[0055] The technical solution of the present application is further illustrated by means of specific embodiments below.
[0056] Examples 1-6
[0057] The preparation of the linear NTC thermistor of Examples 1-6 comprises the following steps:
[0058] (1) According to the proportions of the six embodiments in Table 1 below, ZnO, Al2O3, and MgO oxide raw materials are respectively poured into six different ball mills for wet ball milling. After ball milling, the mixed slurry is placed in an oven at 90° C. and baked for 20 h, ground to obtain a powder, and then the powder is calcined in air at 900° C. for 6 h to obtain a base material; wherein the oxide raw materials such as ZnO, Al2O3, and MgO are all analytically pure;
[0059] (2) According to the proportions of the six embodiments in Table 1 below, the base material was mixed with different contents of RuO2 and poured into a ball mill, and the mixed slurry was placed in an oven at 100°C for 12 hours for grinding to obtain a calcined powder, which was dry-formed and cold isostatically pressed at 300 MPa to form a 50 mm × 50 mm × 15 mm green body;
[0060] (3) The green body was kept in an air atmosphere at 1300°C for 8 hours. After sintering, the sintered block was sliced into ceramic sheets with a thickness of 0.5 mm. Silver paste was printed on the ceramic sheets by screen printing. The silver electrode was solidified by sintering at 800°C for 15 minutes. Then, the silver electrode-containing ceramic sheet was diced to obtain a linear NTC thermistor with a size of 1.0 mm × 1.0 mm × 0.5 mm.
[0061] (4) Randomly select 20 to 30 pieces of resistor samples from Examples 1 to 6. Place the selected samples in oil baths at 25°C, 50°C, 80°C and 100°C in turn, and use a resistance tester to measure the resistance values at 25°C, 50°C, 80°C and 100°C respectively, then calculate the average resistance value of each example sample to obtain the resistance value of Examples 1 to 6.
[0062] Table 1
[0063]
[0064] Figure 1 and Figure 2 The beneficial effects of the six embodiments are shown in Table 1. Figure 1 The RT curve of ZnO ceramic resistor with different RuO2 addition amounts is shown. Figure 2 Indicates the size of TCR in three temperature ranges.
[0065] from Figure 1 It can be seen that in Examples 1 to 4, as the value of variable x increases gradually (0 to 0.9), the resistivity of the ZnO ceramic resistor increases from 26Ω·mm to 414Ω·mm; the RT curves are all straight lines. Figure 2 It can also be seen from the TCR size of different temperature ranges that the TCR size of the same x value remains basically unchanged; with the increase of RuO2 addition, the straight line gradually becomes steeper from gentle, and TCR gradually increases from -135ppm to -3960ppm. In Examples 5 and 6, the value of variable y is changed, the resistivity of the ZnO ceramic resistor decreases rapidly, and the TCR first increases slightly, and then also decreases rapidly.
[0066] It can be seen that by adjusting the value of variable x, the ZnO ceramic resistor can be turned into a linear NTC thermistor with NTC effect, and by changing the value of variable y, the resistivity and TCR of the NTC thermistor can be adjusted to make it adjustable and controllable. Therefore, adding RuO2 can turn the ZnO ceramic resistor into a linear resistor with NTC effect, and changing the ratio of ZnO to Al2O3 can adjust the electrical properties of the linear NTC thermistor.
[0067] TCR (temperature coefficient) is an important parameter in thermistor technology, which indicates the degree to which the material's resistance changes with temperature. Generally speaking, the TCR value describes the slope of the thermistor material's resistance change with temperature, usually expressed in ppm / ℃ (parts per million degrees / ℃).
[0068] It should be understood that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. For those skilled in the art, the technical solutions described in the above embodiments can be modified, or some of the technical features therein can be replaced by equivalents; and all these modifications and replacements should fall within the scope of protection of the claims attached to the present invention.
Claims
1. A method for preparing a linear NTC thermistor, characterized in that: Including the steps: By mass percentage, according to the component ratio of (85 + y)ZnO-(10 - y)Al2O3-(5 - x)MgO (where 0 ≤ y ≤ 5, 0 < x < 1), weigh the oxide raw materials of ZnO, Al2O3, and MgO, conduct primary ball milling and drying to obtain dry powder materials; Calcine the dry powder materials to obtain calcined powder; By mass percentage, according to the component ratio of xRuO2 (where 0 < x < 1), add the raw material containing Ru element to the calcined powder to obtain mixed powder materials; Conduct secondary ball milling, drying, dry pressing, cold isostatic pressing, sintering, slicing, printing electrodes, and scribing on the mixed powder materials to obtain a linear NTC thermistor.
2. The method for preparing a linear NTC thermistor according to claim 1, characterized in that: The steps of conducting secondary ball milling, drying, dry pressing, cold isostatic pressing, sintering, slicing, printing electrodes, and scribing on the mixed powder materials to obtain a linear NTC thermistor are specifically as follows: Conduct secondary ball milling on the mixed powder materials and obtain mixed powder through drying; Manufacture a green body from the mixed powder through dry pressing and cold isostatic pressing; Sinter the green body to obtain an oxide ceramic block; Slice the ceramic block to obtain ceramic sheets; Print electrode paste on the ceramic sheets and cure the electrodes through sintering; Scribe the ceramic sheets with electrodes to obtain a linear NTC thermistor.
3. The method for preparing a linear NTC thermistor according to claim 1, characterized in that: The oxide raw materials of ZnO, Al2O3, and MgO are all of analytical purity.
4. The method for preparing a linear NTC thermistor according to claim 1, characterized in that: The raw material containing Ru element is a single substance or an oxide.
5. The method for preparing a linear NTC thermistor according to claim 1, characterized in that: The drying temperature after the primary ball milling is 80 - 100 °C, and the time is 12 - 24 h.
6. The method for preparing a linear NTC thermistor according to claim 2, characterized in that: The drying temperature after the secondary ball milling is 80 - 100 °C, and the time is 12 - 24 h.
7. The method for preparing a linear NTC thermistor according to claim 1, characterized in that: The calcination temperature for calcining the dry powder materials is 800 - 1000 °C, and the heat preservation time is 3 - 8 hours.
8. The method for preparing a linear NTC thermistor according to claim 1, characterized in that: The pressure of the cold isostatic pressing is 300 MPa.
9. The method for preparing a linear NTC thermistor according to claim 1, characterized in that: The sintering temperature of the green body is 1200 - 1400 °C, the heat preservation time is 3 - 10 hours, and the sintering atmosphere is an air atmosphere.
10. A linear NTC thermistor, characterized in that: The linear NTC thermistor uses ZnO as the matrix, and its composition is (85 + y)ZnO-(10 - y)Al2O3-(5 - x)MgO-xRuO2, where 0 ≤ y ≤ 5, 0 < x < 1.