NaFe1 / 3Ni1 / 3Mn1 / 3O2atCNT composite material and preparation method and application thereof
NaFe1/3Ni1/3Mn1/3O2 material was synthesized by high-pressure ultrasonic microwave hydrothermal method and mixed with carbon nanotubes to prepare high-purity NaFe1/3Ni1/3Mn1/3O2@CNT composite material, which solved the limited resources of lithium-ion batteries and sodium ions The complex synthesis of battery positive electrode materials improves the performance and cycle stability of the battery, simplifies the process, and facilitates industrial application.
Patent Information
- Application Number
- CN202411085623.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-08
Smart Images

Figure CN118919305A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of electrochemical energy storage, and specifically relates to a NaFe 1 / 3 Ni 1 / 3 Mn 1 / 3 O2@CNT composite material and its preparation method and application. Background Art
[0002] With the continuous growth of global energy demand and the gradual depletion of non-renewable energy, the development and utilization of green renewable energy has become an important strategy to solve the energy crisis and cope with climate change. Clean energy such as wind energy, hydropower, solar energy, nuclear energy, tidal energy, etc. has been rapidly developed due to its environmental friendliness and sustainability. However, these energy forms have problems of intermittent and unstable output, which limits their recycling and large-scale application.
[0003] Energy storage technology is a key way to solve the above problems. Battery systems, especially lithium-ion batteries, are widely used in portable electronic devices, electric vehicles and energy storage systems due to their high energy density, high operating voltage and long service life. However, the limited reserves and uneven distribution of lithium resources, as well as the sharp increase in demand, have led to an increase in the cost of lithium batteries, limiting their application in large-scale energy storage. To meet this challenge, researchers and the industry are seeking to develop new, cheap and environmentally friendly battery materials. Sodium has great potential in large-scale energy storage systems due to its abundant reserves in the earth's crust and oceans, its wide distribution and its relatively low price. Sodium-ion batteries, especially those using layered transition metal oxides as positive electrode materials, have attracted widespread attention due to their high theoretical capacity and simple preparation process. There are various methods for synthesizing positive electrode materials, including coprecipitation, sol-gel, high-temperature solid-phase and hydrothermal methods. The co-precipitation method has a lower cost but may lead to product heterogeneity; the sol-gel method can synthesize uniform electrode materials, but the operation is complicated; the high-temperature solid-phase method is simple and direct, but the particle size distribution of the obtained particles is uneven; the hydrothermal method can synthesize high-purity, uniform-sized, and perfectly crystallized materials, but requires a specific high-pressure reactor. Summary of the invention
[0004] The object of the present invention is to provide a NaFe 1 / 3 Ni 1 / 3 Mn 1 / 3 O2@CNT composite material and its preparation method and application. The preparation method of the present invention is simple and the prepared NaFe 1 / 3 Ni 1 / 3 Mn 1 / 3 The O2@CNT composites have high purity and crystallinity.
[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows:
[0006] A NaFe 1 / 3 Ni 1 / 3 Mn 1 / 3 The preparation method of the O2@CNT composite material comprises the following steps:
[0007] S1. Add NaOH, MnO2, Fe2O3 and NiO powder into a polytetrafluoroethylene tank, add deionized water and stir evenly to obtain a mixed solution;
[0008] S2, transferring the mixed solution obtained in S1 to a high-pressure reactor for reaction;
[0009] S3, cooling, filtering, repeatedly washing with distilled water, and vacuum drying at room temperature to obtain NaFe 1 / 3 Ni 1 / 3 Mn 1 / 3 O2;
[0010] S4, the NaFe obtained in step S3 1 / 3 Ni 1 / 3 Mn 1 / 3 After O2 and CNT are evenly mixed, they are placed in a cylinder and milled with ball mill beads to obtain NaFe 1 / 3 Ni 1 / 3 Mn 1 / 3 O2@CNT composite materials.
[0011] Preferably, the stoichiometric ratio of NaOH, MnO2, Fe2O3 and NiO powder in step S1 is 5:2:1:1-2:1:1:1.
[0012] Preferably, in step S2, the mixed solution obtained in S1 is transferred to a high-pressure reactor and heated at 130-250° C. for 0.5-4 h.
[0013] Preferably, in step S3, drying is performed under a vacuum degree of -0.5-0.05 MPa.
[0014] Preferably, in step S4, NaFe 1 / 3 Ni 1 / 3 Mn 1 / 3 After O2 and CNT are evenly mixed, they are placed in a cylinder with ball milling beads and ground at a rotation speed of 100-800r / min for 0.5-5h.
[0015] The present invention also provides NaFe prepared by the preparation method 1 / 3 Ni 1 / 3 Mn 1 / 3 O2@CNT composite materials.
[0016] The present invention also provides NaFe prepared by the preparation method 1 / 3 Ni 1 / 3 Mn 1 / 3 O2@CNT composite material or the NaFe 1 / 3 Ni 1 / 3 Mn 1 / 3 Application of O2@CNT composite materials in the preparation of positive electrode materials for sodium ion batteries.
[0017] The present invention also provides a positive electrode material for a sodium ion battery, wherein the positive electrode material contains the above-mentioned NaFe 1 / 3 Ni 1 / 3 Mn 1 / 3 O2@CNT composite materials.
[0018] Compared with the prior art, the present invention has the following advantages and technical effects:
[0019] The present invention provides a NaFe 1 / 3 Ni 1 / 3 Mn 1 / 3 O2@CNT composite material and its preparation method and application, NaFe was synthesized by high pressure ultrasonic microwave combined hydrothermal method with NaOH, MnO2, Fe2O3 and NiO as raw materials. 1 / 3 Ni 1 / 3 Mn 1 / 3 O2, and then mixed it with carbon nanotubes by ball milling to prepare NaFe 1 / 3 Ni 1 / 3 Mn 1 / 3 O2@CNT composites with high purity and crystallinity, and NaFe was observed by TEM images. 1 / 3 Ni 1 / 3 Mn 1 / 3 The sheet structure of O2 is tightly combined with carbon nanotubes. The carbon nanotubes are attached to the surface of the ternary material, providing an effective channel for the migration of sodium ions and promoting the efficiency of ion transmission. At the same time, SEM-EDS analysis shows that the elements Na, Fe, Mn, Ni, O, and C are evenly distributed in the composite material, which is crucial to ensure the electrochemical reaction activity of the electrode material during the charging and discharging process, and to ensure the overall capacity, cycle stability and safety of the battery.
[0020] The NaFe prepared by the present invention 1 / 3 Ni 1 / 3 Mn 1 / 3 O2@CNT composite materials have a simple preparation process and are easy to industrialize, providing a solid foundation for improving the performance and expanding the application of sodium-ion batteries, and are expected to promote the development and industrialization of related technologies.
[0021] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 The CNT and NaFe provided in Comparative Example 1 and Examples 1-4 of the present invention are 1 / 3 Ni 1 / 3 Mn 1 / 3 O2、NaFe 1 / 3Ni 1 / 3 Mn 1 / 3 O2@1.00%CNT、NaFe 1 / 3 Ni 1 / 3 Mn 1 / 3 O2@0.70%CNT、NaFe 1 / 3 Ni 1 / 3 Mn 1 / 3 XRD pattern of O2@0.50%CNT composite;
[0023] Figure 2 The CNT, NaFe provided in Comparative Example 1, Example 1 and Example 3 of the present invention are 1 / 3 Ni 1 / 3 Mn 1 / 3 O2、NaFe 1 / 3 Ni 1 / 3 Mn 1 / 3 Scanning electron microscope image of O2@0.70%CNT composite material, where Figure 2 (a) is the NaFe provided in Example 1 1 / 3 Ni 1 / 3 Mn 1 / 3 SEM image of O2, scale is 10μm, Figure 2 (b) is a SEM image of CNT provided in Comparative Example 1, with a scale of 1 μm. Figure 2 (c) is NaFe provided in Example 3 1 / 3 Ni 1 / 3 Mn 1 / 3 O2@0.70% CNT SEM image, scale is 1μm, Figure 2 (d) is NaFe provided in Example 3 1 / 3 Ni 1 / 3 Mn 1 / 3 TEM image of O2@0.70% CNT, scale is 5nm;
[0024] Figure 3 The NaFe provided in Example 3 1 / 3 Ni 1 / 3 Mn 1 / 3 SEM-EDS element distribution diagram of O2@0.70%CNT, where Figure 3a is NaFe provided in Example 3 1 / 3 Ni 1 / 3 Mn 1 / 3 Element distribution diagram of O2@0.70%CNT, scale is 3μm, Figure 3 b is NaFe provided in Example 3 1 / 3 Ni 1 / 3 Mn 1 / 3 Na element distribution diagram of O2@0.70% CNT, scale is 3μm, Figure 3 Where c is NaFe provided in Example 3 1 / 3 Ni 1 / 3 Mn 1 / 3 Mn element distribution diagram of O2@0.70%CNT, scale is 3μm, Figure 3 Where d is NaFe provided in Example 3 1 / 3 Ni 1 / 3 Mn 1 / 3 Fe element distribution diagram of O2@0.70%CNT, scale is 3μm, Figure 3 e in the formula is NaFe provided in Example 3 1 / 3 Ni 1 / 3 Mn 1 / 3 Ni element distribution diagram of O2@0.70% CNT, scale is 3μm, Figure 3 Where f is NaFe provided in Example 3 1 / 3 Ni 1 / 3 Mn 1 / 3 O2@0.70%CNT O element distribution diagram, scale is 3μm, Figure 3 g is the NaFe provided in Example 3 1 / 3 Ni 1 / 3 Mn 1 / 3 C element distribution diagram of O2@0.70%CNT, scale is 3μm;
[0025] Figure 4 is a graph showing the XPS test results of the composite material provided in Example 1 of the present invention, wherein: Figure 4 (a) is NaFe provided in Example 1 1 / 3 Ni 1 / 3 Mn 1 / 3 O2 full spectrum, Figure 4 (b) is the NaFe provided in Example 1 1 / 3 Ni 1 / 3 Mn 1 / 3 XPS spectrum of Fe 2p of O2, Figure 4 (c) is the NaFe provided in Example 1 1 / 3 Ni 1 / 3 Mn 1 / 3 XPS spectrum of Mn 2p of O2, Figure 4(d) is the NaFe provided in Example 1 1 / 3 Ni 1 / 3 Mn 1 / 3 XPS pattern of Ni 2p of O2. DETAILED DESCRIPTION
[0026] The technical solution of the present invention is further described below through the accompanying drawings and embodiments.
[0027] Unless otherwise defined, technical or scientific terms used in the present invention shall have the common meanings understood by one having ordinary skills in the field to which the present invention belongs.
[0028] In the present invention, unless otherwise specified, the raw materials used are conventional commercial products in the art, including sodium hydroxide (Alfa, 99.5%), manganese dioxide (Aladdin, 99.5%), ferric oxide (Aladdin, 99.9%), and nickel monoxide (Aladdin, 99.9%).
[0029] Example 1 This example provides a NaFe 1 / 3 Ni 1 / 3 Mn 1 / 3 O2 material and preparation method thereof, comprising the following steps:
[0030] S1. Add 2.400 g NaOH, 0.174 g MnO2, 0.320 g Fe2O3, and 0.150 g NiO powder into a polytetrafluoroethylene tank, add 20 mL deionized water and stir evenly to obtain a mixed solution;
[0031] S2, transferring the mixed solution obtained in S1 into a high pressure reactor and heating at 180°C for 2.5h;
[0032] S3, cooling, filtering, repeatedly washing with distilled water, and vacuum drying at room temperature, wherein the vacuum degree is -0.1 MPa, to obtain NaFe 1 / 3 Ni 1 / 3 Mn 1 / 3 O2.
[0033] Example 2 This example provides a NaFe 1 / 3 Ni 1 / 3 Mn 1 / 3 O2@1.00%CNT composite material, the NaFe 1 / 3 Ni 1 / 3 Mn 1 / 3 After O2 and CNT were mixed evenly in a ratio of 99% and 1%, they were placed in a cylinder with ball milling beads and ground at a speed of 300r / min for 3h to obtain NaFe 1 / 3 Ni 1 / 3 Mn1 / 3 O2@1.00%CNT composite material.
[0034] Example 3 This example provides a NaFe 1 / 3 Ni 1 / 3 Mn 1 / 3 O2@0.70%CNT composite material, the NaFe 1 / 3 Ni 1 / 3 Mn 1 / 3 After O2 and CNT were mixed evenly in a ratio of 99.3% and 0.70%, they were placed in a cylinder with ball milling beads and ground at a speed of 300r / min for 3h to obtain NaFe 1 / 3 Ni 1 / 3 Mn 1 / 3 O2@0.70%CNT composite material.
[0035] Example 4 This example provides a NaFe 1 / 3 Ni 1 / 3 Mn 1 / 3 O2@0.50%CNT composite material, the NaFe 1 / 3 Ni 1 / 3 Mn 1 / 3 After O2 and CNT were mixed evenly in a ratio of 99.5% and 0.50%, they were placed in a cylinder with ball milling beads and ground at a speed of 300 r / min for 3 h to obtain NaFe 1 / 3 Ni 1 / 3 Mn 1 / 3 O2@0.50%CNT composite material.
[0036] Comparative Example 1 provides a CNT material purchased from Beijing Dekedaojin Technology Co., Ltd., >98%.
[0037] The effects of the materials provided in the above examples 1-4 and comparative example 1 were verified by the following tests:
[0038] Physicochemical characterization:
[0039] The X-ray diffractometer (XRD, Cu-Kα target, D8 Advance, Bruker, Germany) was used. ) was used to analyze the crystal structure of the electrode material; the microscopic morphology and element distribution of the electrode material were analyzed using a SU8010 scanning electron microscope (SEM) produced by Hitachi, Japan, and a JEM-2100F transmission electron microscope (TEM) produced by JEOL Ltd. The element valence state of the material was analyzed using a 250XI XPS energy spectrum analyzer produced by THERMO ESCALAB, with Al-Kα rays as the radiation source and C1s (284.8eV) as the calibration standard. The test results are as follows:
[0040] Figure 1 The XRD diagram of the materials provided in the above embodiments is shown in the figure above, and the enlarged diagram of the characteristic peak at CNT (002) is attached in the upper right corner. Figure 1 It can be seen that NaFe 1 / 3 Ni 1 / 3 Mn 1 / 3 The characteristic peak of O2 is consistent with the R-3m space group of the O3 phase (α-NaFeO2) structure, and the characteristic peak is sharp and narrow, indicating that the crystal purity of the sample synthesized by ultrasonic microwave hydrothermal method is high. At the same time, the characteristic peak of the composite material not only has NaFe 1 / 3 Ni 1 / 3 Mn 1 / 3 The characteristic diffraction peaks of O2 at (003) and (104) also exist, and there is a characteristic diffraction peak of CNT at (002) with a smaller intensity, and no other impurity peaks appear, indicating that this crystal material is made of NaFe 1 / 3 Ni 1 / 3 Mn 1 / 3 It is a composite of O2 and CNT crystal materials, and the crystal purity is high.
[0041] In order to study the morphology of the material, the NaFe 1 / 3 Ni 1 / 3 Mn 1 / 3 O2、NaFe 1 / 3 Ni 1 / 3 Mn 1 / 3 The O2@0.70% CNT composite material and CNT were subjected to scanning electron microscopy. Figure 2-3 .
[0042] Depend on Figure 2 From a in Example 1, it can be seen that the material provided in Example 1 is a sheet structure with a particle size within 5 μm. Figure 2 As can be seen from b in the figure, the CNT provided in Comparative Example 1 is in the form of nanotubes. Figure 2 As can be seen from c, the NaFe provided in Example 3 1 / 3Ni 1 / 3 Mn 1 / 3O2@0.70%NaFe in CNT 1 / 3 Ni 1 / 3 Mn 1 / 3 The sheet structure of O2 is combined with CNT, which is attached to the surface of the ternary material, providing a channel for the migration of sodium ions. Figure 2 From the d in the figure, we can see that NaFe 1 / 3 Ni 1 / 3 Mn 1 / 3 The lattice spacing of O2@0.70% CNT was measured to be 0.50 nm, corresponding to the (003) crystal plane of the O3 phase.
[0043] Figure 3 NaFe 1 / 3 Ni 1 / 3 Mn 1 / 3 SEM-EDS image of O2@0.70%CNT. It can be seen that Na, Fe, Mn, Ni, O, and C elements are present in NaFe 1 / 3 Ni 1 / 3 Mn 1 / 3 O2@0.70%CNT is uniformly distributed. The uniformity of element distribution is crucial to the overall performance of electrode materials, because non-uniform distribution may lead to differences in local electrochemical reaction activity, affecting the overall capacity, cycle stability and safety of the battery.
[0044] In order to study the oxidation state of transition metals in materials, μ is used for the NaFe 1 / 3 Ni 1 / 3 Mn 1 / 3 O2 was tested with XPS, and the results were as follows Figure 4 shown.
[0045] Depend on Figure 4 As can be seen from a in Example 1, the NaFe 1 / 3 Ni 1 / 3 Mn 1 / 3 O2 materials contain five elements: Na, Fe, Ni, Mn, and O. Figure 4 From the b in the figure, we can see that Fe 2p 3 / 2 and Fe 2p 1 / 2 The binding energies of the peaks are 711 eV and 725 eV, respectively, which are similar to those of Fe 3+ The iron in the material is mostly in the +3 state (Fe 3+ ) exists in the form of Figure 4 From the c in Mn2p 1 / 2 The peaks are located at 653.4eV and 654.4eV, while the Mn 2p 3 / 2The peaks are located at 642eV and 643.5eV, where the peaks at 643.5eV and 654.4eV represent Mn at +4 valence (Mn 4+ ), while the peaks at 642 eV and 653.4 eV correspond to Mn 3+ . This indicates that the manganese in the material also exists as Mn 3+ and Mn 4+ Two oxidation states. Figure 4 From the d in the figure, we can see that Ni 2p 3 / 2 and Ni 2p 1 / 2 The main peaks are located at 854.4 eV and 872.4 eV, respectively. These two binding energies correspond to Ni 2+ There are also satellite peaks, which are related to Ni with a higher oxidation state. The presence of satellite peaks here indicates that the material also contains a small amount of Ni 3+ Therefore, the nickel in the material is mainly Ni 2+ Exists in the form of Ni 3+ .
[0046] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.
Claims
1. A type of NaFe 1 / 3 Ni 1 / 3 Mn 1 / 3 The preparation method of O2@CNT composite material is characterized in that: The steps include: S1. Add NaOH, MnO2, Fe2O3 and NiO powder into a polytetrafluoroethylene tank, add deionized water and stir evenly to obtain a mixed solution; S2, transferring the mixed solution obtained in S1 to a high-pressure reactor for reaction; S3, cooling, filtering, repeatedly washing with distilled water, and vacuum drying at room temperature to obtain NaFe 1 / 3 Ni 1 / 3 Mn 1 / 3 O2; S4, the NaFe obtained in step S3 1 / 3 Ni 1 / 3 Mn 1 / 3 After O2 and CNT are evenly mixed, they are placed in a cylinder and milled with ball mill beads to obtain NaFe 1 / 3 Ni 1 / 3 Mn 1 / 3 O2@CNT composite materials.
2. The preparation method according to claim 1, characterized in that: The stoichiometric ratio of NaOH, MnO2, Fe2O3, and NiO powder in step S1 is 5:2:1:1-2:1:1:
1.
3. The preparation method according to claim 1, characterized in that: In step S2, the mixed solution obtained in S1 is transferred to a high-pressure reactor and heated at 130-250° C. for 0.5-4 h.
4. The preparation method according to claim 1, characterized in that: In step S3, the mixture is dried under a vacuum degree of -0.5-0.05 MPa.
5. The preparation method according to claim 1, characterized in that: In step S4, NaFe 1 / 3 Ni 1 / 3 Mn 1 / 3 After O2 and CNT are evenly mixed, they are placed in a cylinder with ball milling beads and ground at a rotation speed of 100-800r / min for 0.5-5h.
6. The NaFe prepared by the preparation method according to any one of claims 1 to 5 1 / 3 Ni 1 / 3 Mn 1 / 3 O2@CNT composite materials.
7. NaFe prepared by the preparation method according to any one of claims 1 to 6 1 / 3 Ni 1 / 3 Mn 1 / 3 O2@CNT composite material or NaFe as claimed in claim 6 1 / 3 Ni 1 / 3 Mn 1 / 3 Application of O2@CNT composite materials in the preparation of positive electrode materials for sodium ion batteries.
8. A positive electrode material for a sodium ion battery, characterized in that: The positive electrode material contains the NaFe 1 / 3 Ni 1 / 3 Mn 1 / 3 O2@CNT composite materials.
Citation Information
Patent Citations
Preparation method of composite anode material of lithium-ion power battery
CN102931383A
Transition metal oxide material and preparation method thereof
CN112591804A
Novel nickel-manganese-based layered sodium ion battery positive electrode material
CN114784266A
Sodium-ion battery positive electrode material, preparation method thereof and sodium-ion battery