MXene-coated NiCo-MOF composite material and preparation and application thereof
By growing NiCo-MOF in situ on the MXene surface, a tightly connected heterostructure is constructed, which solves the poor conductivity and aggregation problems of MOF in supercapacitors, and achieves high specific capacitance and low charge transfer resistance, improving electrochemical performance.
Patent Information
- Application Number
- CN202411188667.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-08
AI Technical Summary
In the prior art, metal organic frames (MOFs) have problems such as poor conductivity, easy particles aggregation and insufficient cycle life in supercapacitor electrode materials, which limits their wide application.
Using a preparation method of MXene@NiCo-MOF composite material, NiCo-MOF is grown in situ on the surface of MXene, and a tightly connected heterostructure is constructed by hydrothermal method and ultrasonic dispersion technology, and Ni/Co-O- Ti bond bridge improves charge transfer channels.
It achieves high specific capacitance, low charge transfer resistance and excellent rate performance, improves electrochemical reaction efficiency, and has a simple and efficient process.
Smart Images

Figure CN118919307A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of supercapacitor electrode materials and relates to a MXene@NiCo-MOF composite material and a preparation method and application thereof. Background Art
[0002] In recent years, energy shortage and environmental pollution have been the main challenges facing mankind. In addition, the large-scale combustion of fossil fuels will inevitably produce CO2, CO, SO2 and NO X At the same time, in order to cope with increasingly severe environmental problems, the Chinese government vigorously advocates and adheres to the goal of "carbon peak and carbon neutrality". Compared with batteries or other energy storage devices, supercapacitors (SC) have the advantages of high power density, good reversibility, long cycle life and green environmental protection, and have great application value in the field of energy storage.
[0003] Electrode materials are the core part of supercapacitors. Among many emerging materials, metal organic frameworks (MOFs) have attracted widespread interest in the field of energy storage due to their fine structure, controllable morphology, large specific surface area, adjustable structure, and diverse functions. MOFs are a type of crystalline porous material with a periodic network structure formed by the self-assembly of inorganic metal centers (metal ions or metal clusters) and bridging organic ligands. MOFs have both the rigidity of inorganic materials and the flexibility of organic materials; at the same time, their poor electrical conductivity, easy aggregation of particles during the preparation process (resulting in reduced porosity), and the need to improve the cycle life limit their widespread application. To this end, some effective solutions have been explored.
[0004] (1) Rationally construct bimetallic or multimetallic MOFs. The Chinese patent document with publication number CN118280745A prepares ternary metal ZnCoFe-MOF materials for supercapacitors by spray drying and calcination, and utilizes the synergistic effect between multiple metals to improve the performance of single metal MOF. However, this method has a high production cost, is not conducive to industrialization, and high-temperature calcination will inevitably cause damage to the MOF structure.
[0005] (2) Using MOF as a precursor template to prepare derivative materials. The Chinese patent document with publication number CN118352165A uses ZIF-67 as a template and obtains surface-etched layered double hydroxide NiCo-LDH by metal ion exchange with nickel nitrate hexahydrate. Although the method is simple and low in cost, the electrochemical properties such as specific capacitance still need to be further improved.
[0006] (3) Combine MOF with other functional materials to construct composite materials. The Chinese patent document with publication number CN117253725A uses a one-pot method to prepare MOF@MXene by stirring a mixed solution containing nickel salt, organic ligand, MXene and potassium hydroxide at room temperature for a long time. This method seems simple, but in fact, during the entire reaction process, the strong base has been corroding the prepared MXene and MOF. This directly leads to the difficulty in controlling the morphology of MOF@MXene prepared by this mechanical mixing method. From the scanning electron microscopy spectrum, it was found that the material on the surface of MXene is mainly a mixture, with a small amount of MOF structural material.
[0007] Li et al. proposed the use of hydrothermal method to x A strategy for in situ growth of Ni-MOF arrays on surfaces. This strategy aims to utilize Ti3C2T x The surface conditions are favorable for the nucleation and growth of Ni-MOF, which promotes the nucleation and growth of Ni-MOF arrays on its surface. This strategy effectively improves the lack of bonding between elements in the materials prepared by mechanical mixing. When the prepared nanocomposite material is used as the electrode material, the supercapacitor has a current density of 0.5A g -1 When the specific capacitance is 497.6F g -1 .
[0008] Therefore, how to develop a MXene@NiCo-MOF composite material with improved electrochemical performance and its preparation and application is an urgent problem to be solved by technicians in this field. Summary of the invention
[0009] In view of this, the present invention provides a MXene@NiCo-MOF composite material and its preparation and application.
[0010] In order to achieve the above object, the present invention adopts the following technical solution:
[0011] A method for preparing a MXene@NiCo-MOF composite material comprises the following steps:
[0012] (1) Preparation of MXene substrate: Slowly add MAX precursor into hydrofluoric acid for etching reaction to obtain a mixed solution containing two-dimensional layered MXene;
[0013] (2) Separation and purification of MXene substrate: The mixed solution obtained in step (1) is centrifuged and washed with deionized water until the pH value is close to neutral, and then freeze-dried to obtain a two-dimensional layered MXene powder;
[0014] (3) Preparation of MXene@NiCo-MOF precursor: The MXene powder, organic ligand and metal salt obtained in step (2) are sequentially added to an organic solvent, and ultrasonic dispersion and stirring are used to mix to obtain a uniformly dispersed mixed solution;
[0015] (4) In situ growth of NiCo-MOF on MXene substrate: The mixed solution obtained in step (3) was placed in a reactor for hydrothermal reaction, and the reaction product was then centrifuged and washed with deionized water and vacuum dried to obtain MXene@NiCo-MOF powder.
[0016] Furthermore, in step (1), the MAX precursor is any one of Ti3AlC2, Ti3ZnC2, Ti3AlCN or Ti3SiC2.
[0017] Furthermore, in step (1), the mass volume ratio of the MAX precursor and hydrofluoric acid is (1-4) g: (10-40) mL, the etching reaction temperature is 20-50° C., and the etching reaction time is 12-60 hours.
[0018] Furthermore, in step (1), the MAX precursor is slowly added into hydrofluoric acid and stirred to perform an etching reaction, and the stirring speed is 200-600 rpm.
[0019] Furthermore, in step (1), the MAX precursor is slowly added to the hydrofluoric acid at a feeding rate of 10-30 mg / s.
[0020] Furthermore, in step (2), the mixed solution obtained in step (1) is centrifuged and washed with deionized water at a rotation speed of 5000-10000 rpm until the pH value of the supernatant is close to neutral, and the washed product is freeze-dried at -40 to -50°C for 24-72 hours.
[0021] Furthermore, in step (2), the mixed solution obtained in step (1) is washed by centrifugation with deionized water until the pH value is neutral.
[0022] Furthermore, in step (3), the mass volume ratio of MXene powder, organic ligand, metal salt and organic solvent is (0.01-1) mg: (0.01-1) mg: (0.01-1.5) mg: (30-60) mL, and the total time of ultrasonic dispersion and stirring mixing is 10-60 minutes.
[0023] Further, in step (3), the organic ligand is any one of terephthalic acid, 2-methylimidazole or 4,4'-bipyridine;
[0024] The above-mentioned metal salts are nickel salts and cobalt salts, the mass ratio of nickel salt to cobalt salt is (0.5-3):1, the above-mentioned nickel salt is any one of nickel nitrate, nickel chloride or nickel sulfate, and the above-mentioned cobalt salt is any one of cobalt nitrate, cobalt chloride or cobalt sulfate.
[0025] Furthermore, in step (3), the organic solvent is a mixed solution of anhydrous ethanol, deionized water and aprotic polar solvent, and the volume ratio of the three is (1-4):(0.1-3):(1-5), and the aprotic polar solvent is any one of formamide, acetonitrile, acetone or N,N-dimethylformamide.
[0026] Furthermore, in step (3), the power of the ultrasonic dispersion is 10-20 W / L, the time of the ultrasonic dispersion is 5-30 minutes, the speed of the stirring and mixing is 200-600 rpm, and the time of the stirring and mixing is 5-30 minutes.
[0027] Furthermore, in step (4), the hydrothermal reaction temperature is 100-200° C., and the reaction time is 6-36 hours.
[0028] Furthermore, in step (4), the reaction product is washed by centrifugation with deionized water at a rotation speed of 3000-6000 rpm for 1-10 minutes, and the washed product is vacuum dried at 30-60° C. for 10-24 hours.
[0029] The present invention also provides a MXene@NiCo-MOF composite material prepared by the above method.
[0030] The present invention also provides an application of the MXene@NiCo-MOF composite material in an electrode material of a supercapacitor.
[0031] The beneficial effects of the present invention are as follows: the bimetallic NiCo-MOF of the present invention combines the superior basic properties of Ni-MOF and Co-MOF, and the ionic radii of nickel and cobalt are similar, which ensures the stability of their structure. The one-step hydrothermal method provided by the present invention is used to prepare the MXene@NiCo-MOF composite material. With the help of the abundant oxygen-containing functional groups on the surface of the two-dimensional material MXene, nucleation sites are provided for NiCo-MOF nanosheets to construct a tightly connected heterogeneous structure; the Ni / Co-O-Ti bond bridge formed between the MXene and NiCo-MOF interfaces provides an effective channel for improving the charge transfer in the electrochemical reaction of NiCo-MOF, and effectively inhibits the stacking and agglomeration of NiCo-MOF nanosheets, so that they grow uniformly on the MXene surface. The MXene@NiCo-MOF electrode material provided by the present invention has a current density of 1 mA cm -2 The specific capacitance is 2.09 F cm -2; EIS impedance fitting analysis shows that the charge transfer resistance of MXene@NiCo-MOF electrode material is Rct=1.195Ω, which is much lower than 2.574Ω of NiCo-MOF; when the current density is increased to 10mA cm -2 When the capacitance retention rate is 74.21%, it is better than 61.81% of NiCo-MOF and 34.48% of MXene. EIS detection shows that the Rct of the MXene@NiCo-MOF composite material provided by the present invention is much lower than that of NiCo-MOF, proving that the composite material has a more efficient charge transfer rate.
[0032] The preparation process of the present invention is simple and efficient, and the prepared electrode material has the characteristics of high specific capacitance, high conductivity, etc., and has broad application prospects in the field of electrochemical energy storage. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 This is a SEM image of the two-dimensional layered MXene prepared in Example 1 of the present invention;
[0034] Figure 2 This is a SEM image of the MXene@NiCo-MOF electrode material prepared in Example 1 of the present invention;
[0035] Figure 3 TEM image of the MXene@NiCo-MOF electrode material prepared in Example 1 of the present invention;
[0036] Figure 4 XRD diagrams of electrode materials prepared in Example 1 and Comparative Example 1 of the present invention;
[0037] Figure 5 BET diagrams of electrode materials prepared in Example 1 and Comparative Example 1 of the present invention;
[0038] Figure 6 CV (Figure a) and GCD (Figure b) of the MXene@NiCo-MOF electrode material prepared in Example 1 of the present invention at different scan rates;
[0039] Figure 7 The electrode materials prepared in Example 1 and Comparative Example 1 of the present invention are -1 CV at scan rate (Fig. a) and 1 mA cm -2 GCD (Fig. b) diagram under current density;
[0040] Figure 8 The EIS impedance and fitted impedance comparison diagram (Figure a) and rate performance comparison diagram (Figure b) of the electrode materials prepared in Example 1 of the present invention and Comparative Example 1 are shown. DETAILED DESCRIPTION
[0041] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0042] Example 1
[0043] The preparation method of MXene@NiCo-MOF composite material comprises the following steps:
[0044] (1) Preparation of MXene substrate: 2 g Ti3AlC2 was slowly added to 20 mL hydrofluoric acid at a feeding rate of 15 mg / s, and stirred at 35 °C for 24 h at a stirring speed of 500 rpm to obtain a mixed solution containing two-dimensional layered MXene;
[0045] (2) Separation and purification of MXene substrate: The mixed solution obtained in step (1) was centrifuged and washed with deionized water at a speed of 10,000 rpm until the pH value of the supernatant was neutral, and the washed product was freeze-dried at -40°C for 36 hours to obtain a two-dimensional layered MXene powder;
[0046] (3) Preparation of MXene@NiCo-MOF precursor: 0.08 mg of the MXene powder obtained in step (2), 0.15 mg of terephthalic acid, 0.14 mg of nickel chloride and 0.08 mg of cobalt chloride were added to 50 mL of an organic solvent in sequence. The organic solvent was a mixed solution of anhydrous ethanol, deionized water and N,N-dimethylformamide in a volume ratio of 3:2:5. Ultrasonic dispersion and stirring were used for mixing. The power of ultrasonic dispersion was 15 W / L. The time of ultrasonic dispersion was 10 minutes. The speed of stirring was 500 rpm. The time of stirring was 20 minutes. A uniformly dispersed mixed solution was obtained.
[0047] (4) In situ growth of NiCo-MOF on MXene substrate: The mixed solution obtained in step (3) was placed in a reactor and heated at 120°C for 24 hours. The reaction product was then centrifuged and washed with deionized water at a speed of 4500 rpm for 10 minutes. The washed product was vacuum dried at 40°C for 20 hours to obtain MXene@NiCo-MOF powder.
[0048] Example 2
[0049] In step (3), the organic ligand is 2-methylimidazole, and the remaining operations are the same as those in Example 1.
[0050] Example 3
[0051] In step (3), the organic ligand is 4,4'-bipyridine, and the remaining operations are the same as in Example 1.
[0052] Example 4
[0053] The heating reaction time in step (4) is 6 hours, and the remaining operations are the same as in Example 1.
[0054] Example 5
[0055] The heating reaction time in step (4) is 36 hours, and the remaining operations are the same as in Example 1.
[0056] Comparative Example 1
[0057] This comparative example provides a preparation method of a NiCo-MOF supercapacitor electrode material, comprising the following steps:
[0058] (1) 0.15 mg of terephthalic acid, 0.14 mg of nickel chloride and 0.08 mg of cobalt chloride were sequentially added to 50 mL of an organic solvent, wherein the organic solvent was a mixed solution of anhydrous ethanol, deionized water and N,N-dimethylformamide, and the volume ratio of the three was 3:2:5, and ultrasonic dispersion and stirring were performed, the power of ultrasonic dispersion was 15 W / L, the time of ultrasonic dispersion was 10 minutes, the speed of stirring was 500 rpm, and the time of stirring was 20 minutes, to obtain a uniformly dispersed mixed solution;
[0059] (2) The mixed solution obtained in step (1) was placed in a reactor and heated at 120° C. for 24 hours, and then the reaction product was centrifuged and washed with deionized water at 4500 rpm for 10 minutes. The washed product was vacuum dried at 40° C. for 20 hours to obtain NiCo-MOF powder.
[0060] The morphology and structure of the prepared materials were analyzed by field emission scanning electron microscopy (SEM, NovaNanoSEM 450) and field emission transmission electron microscopy (TEM, JEM-F200). The crystal structure of the sample was confirmed by X-ray diffraction (XRD, Rigaku TTRIII). The specific surface area and pore size distribution curve of the porous material were determined by nitrogen adsorption analyzer (BET).
[0061] The two-dimensional layered MXene material prepared in step (2) of Example 1 was tested using SEM. Figure 1 As shown, the two-dimensional layered MXene shows a distinct accordion nanostructure, and the surface of the sheets is smooth and free of oxidized particles.
[0062] The MXene@NiCo-MOF supercapacitor electrode material prepared in step (4) of Example 1 was tested using SEM. Figure 2 As shown, the composite material MXene@NiCo-MOF retains the two-dimensional layered structure of MXene, and the nanosheet-like NiCo-MOF grows uniformly on the MXene surface.
[0063] The MXene@NiCo-MOF supercapacitor electrode material prepared in Example 1 was tested by TEM. Figure 3 As shown in the figure, the two physical phases of MXene and NiCo-MOF in the composite material MXene@NiCo-MOF are significantly combined at the interface to construct a tightly connected heterogeneous structure.
[0064] The supercapacitor electrode materials prepared in Example 1 and Comparative Example 1 were tested using XRD. Figure 4 As shown in the figure, the composite material MXene@NiCo-MOF has the characteristic peaks of both MXene and NiCo-MOF. Combined with SEM and TEM tests, it further shows that the composite material was successfully prepared. In addition, the characteristic peak corresponding to the (002) crystal plane in MXene@NiCo-MOF is significantly shifted to a lower angle compared to the characteristic peak corresponding to the (002) crystal plane in MXene, indicating that the nanosheet NiCo-MOF inhibits the stacking of MXene sheets during the nucleation and growth process, effectively increasing the interlayer spacing and being more conducive to electron transport.
[0065] The supercapacitor electrode materials prepared in Example 1 and Comparative Example 1 were tested using BET. Figure 5 It shows that the specific surface area of the composite material MXene@NiCo-MOF is between MXene and NiCo-MOF, and it is a mesoporous material.
[0066] The electrochemical performance of the samples was tested using a CHI 660E electrochemical workstation (Shanghai Chenhua, China). In a three-electrode system at room temperature, the supercapacitor electrodes prepared in Example 1 and Comparative Example 1 were used as working electrodes, Hg / HgO electrodes and Pt sheets were used as reference electrodes and counter electrodes, respectively, and 3M KOH solution was used as the electrolyte. Cyclic voltammetry (CV) tests were performed in a potential window of 0-0.7 V at a rate of 2 to 20 mVs -1 The GCD test was performed in a potential window of 0–0.5 V at a scan rate of 1 to 10 mA cm -2 The electrochemical impedance spectroscopy (EIS) was carried out at a current density of 0.01 Hz to 10 6 The area specific capacitance Cs (F cm) of the electrode material is -2 ) is determined by formula (1):
[0067]
[0068] Where I is the current (mA), Δt is the discharge time (s), and s is the loading area of the electrode material (cm 2 ), ΔV is the voltage window (V).
[0069] like Figure 6 a and b show the CV and GCD graphs of the composite material MXene@NiCo-MOF, respectively, showing obvious pseudocapacitive characteristics and excellent coulombic efficiency. Corresponding to the redox pair of metal ion transition assisted by OH ions, the Faraday redox reaction occurring in this process can be expressed by the following formula:
[0070]
[0071]
[0072] Figure 7 a and b are the CV and GCD graphs of MXene@NiCo-MOF, NiCo-MOF and MXene, respectively. The CV curve of each electrode has a pair of redox peaks, showing pseudocapacitive characteristics. When the scan rate is the same, the CV curve of MXene@NiCo-MOF has the largest integrated area, indicating that the constructed Ni / Co-O-Ti bond bridge can effectively promote the migration of electrolyte ions and the transport of charges, thereby obtaining a better specific capacitance. According to the GCD curve and formula (1), the three electrode materials have a specific capacitance of 1 mA cm -2 The specific capacitances are 2.09 F cm -2 , 1.81F cm -2 and 0.02 F cm -2 , the detailed test data comparison is shown in Table 1; and this result is better than some related materials reported previously, as shown in Table 2.
[0073] Figure 8 a is the Nyquist plot of MXene@NiCo-MOF, NiCo-MOF and MXene and the resistance value comparison after fitting. It can be clearly found that compared with NiCo-MOF, the charge transfer resistance (Rct) of the composite material MXene@NiCo-MOF is significantly reduced, which shows that the strategy of providing nucleation sites for NiCo-MOF nanosheets with the help of the rich oxygen-containing functional groups on the surface of the two-dimensional material MXene and building Ni / Co-O-Ti bond bridges at the interface of the tightly connected heterogeneous structure can effectively improve the conductivity of the composite material, greatly improving the problem of poor conductivity of traditional MOFs materials. Figure 8b further reflects the excellent rate performance of MXene@NiCo-MOF composites. When the current density is increased to 10 mA cm -2 When , the capacitance retention rate is still 74.21%, which is better than 61.81% of NiCo-MOF and 34.48% of MXene.
[0074] Table 1 Specific capacitance of different electrode materials at different current densities
[0075]
[0076] Table 2 Comparison of the performance of MXene@NiCo-MOF composites as supercapacitor electrodes with other electrode materials
[0077]
[0078]
[0079] Note: CN113077991A, CN118263038A, and CN118263038A in Table 2 are mass specific capacitances, which are still lower than those in Example 1 after conversion to area specific capacitances.
[0080] Citation 1: Dong Chaoqun. Promoting honeycomb layered double hydroxide nanosheets as advanced electrodes for supercapacitors[J]. Solid Films. 2020, 715, 138439.
[0081] Reference 2: Jiao Yang. Metal-organic framework-derived Ni / NiO microparticles with subtle lattice distortion for high-performance electrocatalysts and supercapacitors[J]. Applied Catalysis B: Environmental. 2019, 244, 732-739.
[0082] Reference 3: Cheng Cheng. Preparation of RGO / Ni-MOF thin film flexible supercapacitors on nickel-coated polyester fabric[J]. Journal of Electrochimica Sinica. 2019, 318, 23-31.
[0083] The disclosed embodiments are described to enable one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing a MXene@NiCo-MOF composite material, characterized in that: The steps include: (1) Preparation of MXene substrate: Slowly add MAX precursor into hydrofluoric acid for etching reaction to obtain a mixed solution containing two-dimensional layered MXene; (2) Separation and purification of MXene substrate: The mixed solution obtained in step (1) is centrifuged and washed with deionized water until the pH value is close to neutral, and then freeze-dried to obtain a two-dimensional layered MXene powder; (3) Preparation of MXene@NiCo-MOF precursor: The MXene powder, organic ligand and metal salt obtained in step (2) are sequentially added to an organic solvent, and ultrasonic dispersion and stirring are used to mix to obtain a uniformly dispersed mixed solution; (4) In situ growth of NiCo-MOF on MXene substrate: The mixed solution obtained in step (3) was placed in a reactor for hydrothermal reaction, and the reaction product was then centrifuged and washed with deionized water and vacuum dried to obtain MXene@NiCo-MOF powder.
2. The method for preparing a MXene@NiCo-MOF composite material according to claim 1, characterized in that: In step (1), the MAX precursor is any one of Ti3AlC2, Ti3ZnC2, Ti3AlCN or Ti3SiC2.
3. The method for preparing a MXene@NiCo-MOF composite material according to claim 1, characterized in that: In step (1), the mass volume ratio of the MAX precursor and hydrofluoric acid is (1-4) g: (10-40) mL, the etching reaction temperature is 20-50° C., and the reaction time is 12-60 hours.
4. The method for preparing a MXene@NiCo-MOF composite material according to claim 1, characterized in that: In step (2), the mixed solution obtained in step (1) is centrifuged and washed with deionized water at a rotation speed of 5000-10000 rpm until the pH value of the supernatant is close to neutral, and the washed product is freeze-dried at -40 to -50°C for 24 to 72 hours.
5. The method for preparing a MXene@NiCo-MOF composite material according to claim 1, characterized in that: In step (3), the mass volume ratio of MXene powder, organic ligand, metal salt and organic solvent is (0.01-1) mg: (0.01-1) mg: (0.01-1.5) mg: (30-60) mL, and the total time of ultrasonic dispersion and stirring mixing is 10-60 minutes.
6. The method for preparing a MXene@NiCo-MOF composite material according to claim 1, characterized in that: In step (3), the organic ligand is any one of terephthalic acid, 2-methylimidazole or 4,4'-bipyridine; The metal salts are nickel salt and cobalt salt, the mass ratio of nickel salt to cobalt salt is (0.5-3):1, the nickel salt is any one of nickel nitrate, nickel chloride or nickel sulfate, and the cobalt salt is any one of cobalt nitrate, cobalt chloride or cobalt sulfate.
7. The method for preparing a MXene@NiCo-MOF composite material according to claim 1, characterized in that: In step (3), the organic solvent is a mixed solution of anhydrous ethanol, deionized water and aprotic polar solvent, and the volume ratio of the three is (1-4):(0.1-3):(1-5), and the aprotic polar solvent is any one of formamide, acetonitrile, acetone or N,N-dimethylformamide.
8. The method for preparing a MXene@NiCo-MOF composite material according to claim 1, characterized in that: In step (4), the hydrothermal reaction temperature is 100-200° C., and the reaction time is 6-36 hours.
9. A MXene@NiCo-MOF composite material prepared by the method according to any one of claims 1 to 8.
10. Use of the MXene@NiCo-MOF composite material according to claim 9 in an electrode material for a supercapacitor.
Citation Information
Patent Citations
MXene / nickel phosphate electrode material and preparation method and application thereof
CN113077991A
MOF-coated MXene composite structure electrode material for super capacitor and preparation method of MOF-coated MXene composite structure electrode material
CN117253725A
Co-MOF (at) MXene high-specific-capacitance supercapacitor electrode material and preparation method thereof
CN118263038A
Preparation method and application of ZnCoFe-MOF material
CN118280745A
NiCo-LDH material, preparation method and application thereof
CN118352165A
Cited By
MXene / two-dimensional conductive MOF composite material as well as derivative material, flexible electrode and application thereof
CN119775576A
Bimetal conductive MOF-based gas sensitive material, preparation method and semiconductor sensor
CN121453859A
An accordion-shaped nano-NiCo-MOF electrode material, its preparation method and application
CN123095560A