Sulfur group elementary substance modified potassium ion battery phosphorus / carbon negative electrode material and preparation method thereof

Through the coating technology of chalcogen element, the structural stability and interface reaction of the phosphorus/carbon anode material of potassium ion battery during potassium storage are solved, the conductivity and cycling performance are improved, and the efficient anode material of potassium ion battery is realized. Modification.

CN118919693APending Publication Date: 2024-11-08XIAN UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411154102.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The phosphorus/carbon anode materials of potassium ion batteries face structural stability and interface reaction problems during potassium storage, resulting in poor electrochemical performance attenuation and cyclic performance. The existing modification methods are costly, complex processes and are not suitable for large-scale production. .

Method used

The vacuum air phase deposition method and liquid phase permeability method are used to controllably coat the chalcogen element on the surface of the phosphorus/carbon negative electrode material to improve its electrochemical reversibility and cyclic stability.

Benefits of technology

The conductivity and charge-discharge capacity of the phosphorus/carbon negative electrode material have been significantly improved, the initial charging capacity has been increased by 27.07%, the cycle stability and rate performance have been significantly improved, and the capacity retention rate has been increased from 81.32% to 85.62%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919693A_ABST
    Figure CN118919693A_ABST
Patent Text Reader

Abstract

The invention discloses a sulfur group elementary substance modified potassium ion battery phosphorus / carbon negative electrode material and a preparation method thereof, and belongs to the technical field of potassium ion batteries. The method comprises the following steps: (1) preparing a certain proportion of phosphorus / carbon negative electrode material by adopting a mechanical ball milling method; (2) mixing a certain amount of chalcogenide elementary substances with the phosphorus / carbon negative electrode material prepared in the step (1) according to a certain proportion, transferring into a quartz tube reactor, carrying out vacuum melting sealing at a relatively high temperature, then carrying out heat preservation for several hours at a specific temperature, and finally cooling to room temperature and taking out a corresponding powder material; and (3) cleaning, grinding and drying the obtained sample in a protective atmosphere, and sieving to obtain the sulfur group elementary substance modified potassium ion battery phosphorus / carbon negative electrode material. Preparing the negative electrode of the potassium ion battery from the material, and testing the electrochemical performance; according to the chalcogenide elementary substance modification method, the electron conductivity and the charging specific capacity of the phosphorus / carbon negative electrode material are remarkably improved, and meanwhile, the electrochemical reversibility and the cycling stability of the phosphorus / carbon negative electrode material in the potassium storage process can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of new energy, in particular to the technical field of potassium ion battery negative electrode materials, and in particular to a sulfide element-modified phosphorus / carbon negative electrode material and a related preparation method. Background Art

[0002] Increasingly severe environmental pollution and energy crises have forced human society to reduce its dependence on traditional fossil fuels and gradually increase the use of renewable energy, and advanced energy storage technology has become a key bottleneck restricting the adjustment of energy structure. Traditional high-energy-density lithium-ion batteries are constrained by relatively scarce lithium resources and face greater pressure on raw material costs after the industrialization of electric vehicles. Potassium-ion batteries, relying on abundant potassium resources, low manufacturing costs and stable working mechanisms, are considered to be a low-cost energy storage system that is expected to replace lithium-ion batteries in the field of large-scale energy storage. Although the larger mass-to-charge ratio of potassium ions will reduce the theoretical specific capacity of related electrode materials, K / K + The extremely low standard electrode potential in organic solvents can effectively increase the battery operating voltage, thereby compensating for the energy density disadvantage caused by the decrease in capacity. At the same time, the smaller solvation radius and desolvation energy of potassium ions in organic solvents can significantly increase their ion migration number and ion diffusion rate, ensuring that potassium ion batteries have excellent rate performance. However, the development of potassium ion batteries is still facing a series of technical problems, mainly involving the reaction kinetics caused by the slow solid-phase diffusion of larger potassium ions in the electrode material structure, the structural stability caused by the huge volume change of the electrode material structure during the potassiumization / depotassiumization process, and the electrochemical performance attenuation caused by the complex side reactions between active materials and active electrolytes.

[0003] As the core part of potassium ion batteries, negative electrode materials directly determine their safety characteristics and electrochemical performance. Conventional potassium metal is difficult to be directly used as a safe negative electrode material due to its low melting point and dendrite growth, while traditional carbon negative electrode materials are limited by fewer potassium storage sites, continuous interfacial side reactions and low reversible capacity. Red phosphorus is low-cost and abundant in reserves. It can react with multiple potassium ions to form alloys and exhibit a higher specific capacity (1154 mAh g -1 , K 4 P 3 ) and lower operating voltage (<0.6 V vs. K / K + ) and ideal energy density, and is therefore considered to be a highly competitive anode material for next-generation potassium ion batteries. However, the large volume change during potassium storage (293 mAh g -1 , K 4 P 3) will destroy the structural stability of the phosphorus negative electrode material, leading to internal structural collapse and overall electrode pulverization and rapid attenuation of electrochemical performance. At the same time, the low electronic conductivity of red phosphorus itself (10 -14 S cm -1 ) will further limit its electrochemical activity and charge transfer rate, and lead to poor reaction kinetics and poor rate performance during potassium storage. In response to the above problems, current research mainly combines electronically insulating red phosphorus with highly conductive and highly flexible carbon materials to synergistically improve its electronic and ion conduction properties and reaction kinetics, and improve its structural stability and electrochemical reversibility by buffering the huge volume change of the phosphorus negative electrode during potassium storage. However, in phosphorus / carbon negative electrode materials with high phosphorus loading, the carbon material is not sufficient to complete the volume change and structural collapse of the phosphorus material, and the introduction of porous carbon materials will significantly increase the specific surface area and surface activation energy of the composite material, accelerate its continuous and violent irreversible side reactions with the active electrolyte during discharge, and lead to the uncontrollable formation of the solid electrolyte interface layer and the loss of a large amount of active phosphorus material, resulting in lower coulombic efficiency and reversible capacity and poor cycle performance.

[0004] Chinese patent CN202410021150.4 provides a fast ion conductor coated phosphorus / carbon composite negative electrode material and its preparation method. This patent is based on fast ion conductor coated phosphorus / carbon composite negative electrode material to improve the migration rate of ions in the negative electrode material, improve the cycle performance and fast charging performance, provide better electrode contact and ion transmission channels, reduce the loss during the first charge and discharge process, and improve the first efficiency. However, the raw materials used in this preparation method are relatively expensive, the process flow is complicated, and the coating controllability is poor.

[0005] Chinese patent CN202311871484.2 provides a method for preparing a surface-modified phosphorus / carbon negative electrode. A method for interfacial modification of a phosphorus / carbon negative electrode is proposed: metallic lithium is dispersed on the surface of the prepared phosphorus / carbon negative electrode, and the metallic lithium is infiltrated and contacted with the phosphorus / carbon negative electrode by hot rolling-melting. First, a pre-lithiated phosphorus / carbon negative electrode is prepared, and it is directly immersed in the lithium-ion battery electrolyte to form a solid electrolyte interface in situ, and finally a phosphorus / carbon negative electrode with high reversible capacity and good stability is obtained. However, this method mainly carries out interfacial modification on the negative electrode sheet, which is not suitable for the surface modification of the negative electrode material, and the operating environment is harsh, and the safety hazard is high, which makes it difficult to be applied to the large-scale production of phosphorus / carbon negative electrode materials for potassium ion batteries. In view of the structural stability and interface problems faced by phosphorus / carbon negative electrode materials, the present invention intends to use sulfide elements to modify phosphorus / carbon negative electrode materials to inhibit their interfacial side reactions with active electrolytes, accelerate ion transmission at the electrode / electrolyte interface, and thus improve their cycle stability and rate performance.

[0006] The above are the domestic public patents on phosphorus / carbon negative electrode materials in recent years, but there is still no preparation method and application with simple interface modification method and high process controllability for phosphorus / carbon negative electrode materials. Summary of the invention

[0007] The present invention aims at the serious structural and interface stability problems faced by phosphorus / carbon negative electrode materials during the potassium storage process. The sulfide elements are controllably coated on the surface of the phosphorus / carbon negative electrode materials through vacuum vapor deposition and liquid phase infiltration, thereby synergistically improving their electrochemical reversibility, cycle stability and rate performance.

[0008] In a first aspect, the present invention provides a method for preparing a chalcogenide-modified phosphorus / carbon negative electrode material for a potassium ion battery, the method comprising the following steps: (1) Preparing a certain ratio of phosphorus / carbon negative electrode materials by mechanical ball milling; (2) A certain amount of sulfur element and the phosphorus / carbon negative electrode material prepared in step (1) are mixed in a certain proportion, transferred into a quartz tube reactor, and vacuum-sealed at a high temperature, then kept at a specific temperature for several hours, and finally cooled to room temperature to take out the corresponding powder material. (3) The obtained samples are cleaned, ground and dried under a protective atmosphere.

[0009] Furthermore, in step (1), the carbon material includes conductive carbon black and carbon nanomaterials, and the purity of the phosphorus source is 98-99.99%. In step (1), the carbon material is conductive carbon black or carbon nanomaterials, and the purity of the phosphorus source is 98-99.99%; the phosphorus / carbon ratio is 6:4-8:2 by mass, preferably 6:4 or 7:3 or 8:2.

[0010] Furthermore, in step (2), the chalcogenide element includes sulfur, selenium and tellurium.

[0011] Furthermore, in step (2), the mass ratio of the sulfur element to the phosphorus / carbon negative electrode material is 1:2-12; preferably 1:2, 1:4, 1:8, 1:12.

[0012] Furthermore, in step (2), the sealing of the sulfur element and the phosphorus / carbon negative electrode material includes vacuum sealing after mixing and grinding for 20 to 30 minutes and vacuum sealing after storing them in the same space.

[0013] Furthermore, in step (2), the heating temperature for heat treatment of the composite material in the vacuum quartz tube is 300-400° C., and the heat preservation time is 12-24 hours.

[0014] Furthermore, in step (2), the heating rate of high temperature sintering is 2-5°C / min, and the cooling rate is 1-2°C / min.

[0015] Furthermore, the modified phosphorus / carbon negative electrode material in step (3) should be cleaned with carbon disulfide.

[0016] Furthermore, the sample in step (3) is ground for 20 to 30 minutes and vibrated to pass through a sieve.

[0017] Furthermore, the mechanical ball milling method comprises the following steps: 1) Weighing phosphorus element and carbon material according to the phosphorus / carbon ratio as claimed in claim 1; 2) ball-milling the phosphorus element and the carbon material in step 1) in a ball mill, and assembling the ball mill in an argon atmosphere glove box; 3) High-energy ball milling was performed at 200 and 300 rpm for 12 h, respectively, and then at 400 rpm for 24 h; 4) Repeat the ball milling step at least twice to achieve uniform composite of phosphorus and porous carbon at the nanometer scale to obtain phosphorus / carbon negative electrode material.

[0018] In a second aspect, the present invention provides a sulfide element-modified potassium ion battery phosphorus / carbon negative electrode material prepared by the preparation method provided in the first aspect.

[0019] Furthermore, the sulfide element-modified potassium ion battery phosphorus / carbon negative electrode material; in some embodiments, the initial charge specific capacity can be increased by 9.16-22.19%, and the charge specific capacity can be increased by 12.84-22.14% after 40 cycles of activation are basically completed; in some embodiments, the initial charge specific capacity can be increased by 9.23-15.72%, and the charge specific capacity can be increased by 19.97-26.82% after 40 cycles of activation are basically completed; in some embodiments, the initial charge specific capacity can be increased by 4.76-18.31%, and the charge specific capacity can be increased by 22.37-22.77% after 40 cycles of activation are basically completed; in some embodiments, the capacity retention rate is 78.32% after the 80th cycle is stable compared with the 40th cycle; in some embodiments, the capacity retention rate is 77.53% after the 80th cycle is stable compared with the 40th cycle, and in some embodiments, the capacity retention rate is 87.47% after the 80th cycle is stable compared with the 40th cycle.

[0020] In some embodiments, the material can increase the initial charge capacity by 27.07%, and the capacity retention rate after the 80th cycle is stable compared with the 40th cycle is 85.62%.

[0021] The third aspect: The present invention further provides a half-cell assembly method using the sulfur-containing element-modified phosphorus / carbon negative electrode material for potassium ion batteries provided in the second aspect: Specifically, the potassium ion half-cell is composed of a positive electrode shell, a phosphorus / carbon negative electrode, a composite diaphragm, potassium metal, a gasket, a spring, a negative electrode shell and an electrolyte.

[0022] The assembly method comprises the following steps: (1) A potassium ion battery negative electrode material, conductive carbon black and sodium alginate are mixed in a mass ratio of m:n:l, wherein m=60~80 wt.%, n=10~20 wt.%, and l=10~20 wt.%, and the mixture is dissolved in deionized water to obtain a slurry.

[0023] (2) The slurry obtained in step (1) is evenly coated on copper foil or aluminum foil, dried at 60-70°C for 10-15 hours, and then cut into circular electrodes.

[0024] (3) The electrode obtained in step (2) is used as the negative electrode and the potassium metal sheet is used as the counter electrode. After adding electrolyte, the battery is assembled. The obtained battery is a potassium ion battery whose negative electrode is a sulfur-modified phosphorus / carbon negative electrode material.

[0025] Furthermore, the battery is a CR2032 button type battery.

[0026] Furthermore, the diaphragm is composed of at least one layer of polymer diaphragm and / or glass fiber diaphragm with a thickness of 14 to 16 mm.

[0027] Furthermore, the electrolyte includes 1.0 M KFSI in EC:DEC=1:1 Vol% electrolyte. In a fourth aspect, the present invention also discloses a potassium ion battery using a chalcogenide element-modified phosphorus / carbon negative electrode material prepared by the method of the first aspect.

[0028] The beneficial effects of the present invention are: The present invention successfully prepares a chalcogenide-modified phosphorus / carbon negative electrode material through a simple and easy-to-implement vapor deposition method, and successfully utilizes the high conductivity and high theoretical specific capacity of the chalcogenide to improve the conductivity and charge-discharge specific capacity of the phosphorus / carbon negative electrode material for a potassium ion battery, and the initial charge specific capacity can be increased by 27.07%; and the amorphous phase formed by the chalcogenide and P can be used as a buffer to improve its structure / interface stability during the potassium storage process, thereby improving the electrochemical reversibility and cycle stability of the phosphorus / carbon negative electrode material in the potassium ion battery, and after 80 cycles, the capacity retention rate is increased from 83.93% to 86.53% compared with the first cycle, and the capacity retention rate is increased from 81.32 to 85.62% after the 40th cycle is stable; the rate performance is significantly improved, and the capacity retention rate is increased from 4.51% to 45.50% after the current density gradually increases from 100 mA g-1 to 8000 mA g-1. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 XRD patterns of the P / C negative electrode material prepared in Comparative Example 1 of the present invention and the negative electrode materials prepared in Examples 8 and 11; Figure 2 SEM image of the potassium ion battery negative electrode material P / C-Se prepared in the embodiment of the present invention; Figure 3 Mapping diagram of preparing P / C-Se, a negative electrode material for potassium ion batteries in an embodiment of the present invention; Figure 4 SEM image of the potassium ion battery negative electrode material P / C-Te prepared in the embodiment of the present invention; Figure 5 Mapping diagram of preparing P / C-Te, a negative electrode material for potassium ion batteries in an embodiment of the present invention; Figure 6 XPS test chart of the negative electrode material for potassium ion battery prepared in Example 8 of the present invention; Figure 7 XPS test chart of the negative electrode material for potassium ion battery prepared in Example 11 of the present invention; Figure 8 Cycling performance diagram of negative electrode materials prepared in Comparative Example 1, Example 1, Example 2, and Example 3; Fig. 9 Cycling performance diagram of negative electrode materials prepared in Comparative Example 1, Example 4, Example 5, and Example 6; Fig.10 Cycling performance diagram of negative electrode materials prepared in Comparative Example 1, Example 7, Example 8 and Example 9; Fig.11 Cycling performance diagram of negative electrode materials prepared in Comparative Example 1, Example 2, Example 5, and Example 8; Fig.12 Cycling performance diagram of negative electrode materials prepared in Comparative Example 1, Example 8, Example 10, Example 11, and Example 12; Fig.13 Cycling performance diagrams of negative electrode materials prepared in Example 8, Example 11 and Example 13; Fig.14 Cyclic performance diagram of the negative electrode material prepared in Example 8 tested at different current densities; Fig.15 Example 8 at 400 mA g -1 The charge and discharge curves tested under current density; Fig.16 Cyclic performance diagram of the negative electrode material prepared in Example 11 tested at different current densities; Fig.17 Example 11 at 400 mA g -1 The charge and discharge curves tested under current density; Fig.18Rate performance diagram of negative electrode materials prepared in Comparative Example 1, Example 8, Example 11, and Example 13; Fig.19 CV curve of the negative electrode material for potassium ion battery prepared in Comparative Example 1 of the present invention under the voltage window of 0.001-2 V; Fig. 20 CV curve of the negative electrode material for a potassium ion battery prepared in Example 8 of the present invention in a voltage window of 0.001-2 V; Fig.21 CV curve of the negative electrode material for potassium ion battery prepared in Example 11 of the present invention in the voltage window of 0.001-2 V; Fig. 22 CV curve of the potassium ion battery negative electrode material prepared in Example 13 of the present invention under the voltage window of 0.001-2 V. DETAILED DESCRIPTION

[0030] In order to express the present invention more clearly, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments.

[0031] Preparation of phosphorus / carbon negative electrode materials: Weigh red phosphorus and commercial porous carbon black in a mass ratio of 8:2, put them into a stainless steel ball mill, and add an appropriate amount of stainless steel ball mill beads of different diameters. The ball mill beads have diameters of 2, 3, and 5 mm, respectively, and are added in a mass ratio of 1:1:1. The ball mill is assembled in an argon atmosphere glove box. After assembly, it is placed in a high-energy ball mill for gradient speed high-energy ball milling. High-energy ball milling is performed at 200 and 300 rpm for 12 h, and then at 400 rpm for 24 h. The ball milling steps are repeated twice to achieve uniform composite of phosphorus and porous carbon at the nanometer size. Finally, the ball mill is disassembled in an argon atmosphere glove box, sieved, collected and stored. Example

[0032] 0.2 g of P / C negative electrode material and 0.05 g of Se powder were put into an agate mortar and mixed and ground in an argon atmosphere glove box for 20 min, then put into a quartz tube and sealed with a tube sealer. The sealed material was then placed in a muffle furnace and heated to 320 °C at a heating rate of 2 °C / min, kept warm for 12 h, then cooled to room temperature at a cooling rate of 1 °C / min and taken out. The sealed quartz tube was disassembled in an argon atmosphere glove box, and the sample was cleaned with carbon disulfide, then repeatedly rinsed and filtered with alcohol and deionized water in a fume hood, sieved, collected and stored after vacuum drying.

[0033] The modified P / C negative electrode material was mixed with conductive carbon black and sodium alginate in a mass ratio of 7:1.5:1.5 to prepare an electrode as the negative electrode, metallic potassium was used as the counter electrode, and the electrolyte was 1.0 M KFSI in EC:DEC=1:1 Vol%, and assembled into a button-type potassium ion battery. Example

[0034] 0.2g of P / C negative electrode material and 0.025g of Se powder were put into an agate mortar and mixed and ground in an argon atmosphere glove box for 20 min, then put into a quartz tube and sealed with a tube sealer. The sealed material was then placed in a muffle furnace and heated to 320 °C at a heating rate of 2 °C / min, kept warm for 12 h, then cooled to room temperature at a cooling rate of 1 °C / min and taken out. The sealed quartz tube was disassembled in an argon atmosphere glove box, and the sample was cleaned with carbon disulfide, then repeatedly rinsed and filtered with alcohol and deionized water in a fume hood, sieved, collected and stored after vacuum drying.

[0035] The modified P / C negative electrode material was mixed with conductive carbon black and sodium alginate in a mass ratio of 7:1.5:1.5 to prepare an electrode as the negative electrode, metallic potassium was used as the counter electrode, and the electrolyte was 1.0 M KFSI in EC:DEC=1:1 Vol%, and assembled into a button-type potassium ion battery. Example

[0036] 0.2 g of P / C negative electrode material and 0.017 g of Se powder were put into an agate mortar and mixed and ground in an argon atmosphere glove box for 20 min, then put into a quartz tube and sealed with a tube sealer. The sealed material was then placed in a muffle furnace and heated to 320 °C at a heating rate of 2 °C / min, kept warm for 12 h, then cooled to room temperature at a cooling rate of 1 °C / min and taken out. The sealed quartz tube was disassembled in an argon atmosphere glove box, and the sample was cleaned with carbon disulfide, then repeatedly rinsed and filtered with alcohol and deionized water in a fume hood, sieved, collected and stored after vacuum drying.

[0037] The modified P / C negative electrode material was mixed with conductive carbon black and sodium alginate in a mass ratio of 7:1.5:1.5 to prepare an electrode as the negative electrode, metallic potassium was used as the counter electrode, and the electrolyte was 1.0 M KFSI in EC:DEC=1:1 Vol%, and assembled into a button-type potassium ion battery. Example

[0038] 0.2 g of P / C negative electrode material and 0.05 g of Se powder were put into an agate mortar and mixed and ground in an argon atmosphere glove box for 20 min, then put into a quartz tube and sealed with a tube sealer. The sealed material was then placed in a muffle furnace and heated to 360 °C at a heating rate of 2 °C / min, kept at this temperature for 12 h, then cooled to room temperature at a cooling rate of 1 °C / min and taken out. The sealed quartz tube was disassembled in an argon atmosphere glove box, and the sample was cleaned with carbon disulfide, then repeatedly rinsed and filtered with alcohol and deionized water in a fume hood, sieved, collected and stored after vacuum drying.

[0039] The modified P / C negative electrode material was mixed with conductive carbon black and sodium alginate in a mass ratio of 7:1.5:1.5 to prepare an electrode as the negative electrode, metallic potassium was used as the counter electrode, and the electrolyte was 1.0 M KFSI in EC:DEC=1:1 Vol%, and assembled into a button-type potassium ion battery. Example

[0040] 0.2 g of P / C negative electrode material and 0.025 g of Se powder were put into an agate mortar and mixed and ground in an argon atmosphere glove box for 20 min, then put into a quartz tube and sealed with a tube sealer. The sealed material was then placed in a muffle furnace and heated to 360 °C at a heating rate of 2 °C / min, kept at this temperature for 12 h, then cooled to room temperature at a cooling rate of 1 °C / min and taken out. The sealed quartz tube was disassembled in an argon atmosphere glove box, and the sample was cleaned with carbon disulfide, then repeatedly rinsed and filtered with alcohol and deionized water in a fume hood, sieved, collected and stored after vacuum drying.

[0041] The modified P / C negative electrode material was mixed with conductive carbon black and sodium alginate in a mass ratio of 7:1.5:1.5 to prepare an electrode as the negative electrode, metallic potassium was used as the counter electrode, and the electrolyte was 1.0 M KFSI in EC:DEC=1:1 Vol%, and assembled into a button-type potassium ion battery. Example

[0042] 0.2 g of P / C negative electrode material and 0.017 g of Se powder were put into an agate mortar and mixed and ground in an argon atmosphere glove box for 20 min, then put into a quartz tube and sealed with a tube sealer. The sealed material was then placed in a muffle furnace and heated to 360 °C at a heating rate of 2 °C / min, kept at this temperature for 12 h, then cooled to room temperature at a cooling rate of 1 °C / min and taken out. The sealed quartz tube was disassembled in an argon atmosphere glove box, and the sample was cleaned with carbon disulfide, then repeatedly rinsed and filtered with alcohol and deionized water in a fume hood, sieved, collected and stored after vacuum drying.

[0043] The modified P / C negative electrode material was mixed with conductive carbon black and sodium alginate in a mass ratio of 7:1.5:1.5 to prepare an electrode as the negative electrode, metallic potassium was used as the counter electrode, and the electrolyte was 1.0 M KFSI in EC:DEC=1:1 Vol%, and assembled into a button-type potassium ion battery. Example

[0044] 0.2 g of P / C negative electrode material and 0.05 g of Se powder were put into an agate mortar and mixed and ground in an argon atmosphere glove box for 20 min, then put into a quartz tube and sealed with a tube sealer. The sealed material was then placed in a muffle furnace and heated to 400 °C at a heating rate of 2 °C / min, kept at this temperature for 12 h, then cooled to room temperature at a cooling rate of 1 °C / min and taken out. The sealed quartz tube was disassembled in an argon atmosphere glove box, and the sample was cleaned with carbon disulfide, then repeatedly rinsed and filtered with alcohol and deionized water in a fume hood, sieved, collected and stored after vacuum drying.

[0045] The modified P / C negative electrode material was mixed with conductive carbon black and sodium alginate in a mass ratio of 7:1.5:1.5 to prepare an electrode as the negative electrode, metallic potassium was used as the counter electrode, and the electrolyte was 1.0 M KFSI in EC:DEC=1:1 Vol%, and assembled into a button-type potassium ion battery. Example

[0046] 0.2 g of P / C negative electrode material and 0.025 g of Se powder were put into an agate mortar and mixed and ground in an argon atmosphere glove box for 20 min, then put into a quartz tube and sealed with a tube sealer. The sealed material was then placed in a muffle furnace and heated to 400 °C at a heating rate of 2 °C / min, kept at this temperature for 12 h, then cooled to room temperature at a cooling rate of 1 °C / min and taken out. The sealed quartz tube was disassembled in an argon atmosphere glove box, and the sample was cleaned with carbon disulfide, then repeatedly rinsed and filtered with alcohol and deionized water in a fume hood, sieved, collected and stored after vacuum drying.

[0047] The modified P / C negative electrode material was mixed with conductive carbon black and sodium alginate in a mass ratio of 7:1.5:1.5 to prepare an electrode as the negative electrode, metallic potassium was used as the counter electrode, and the electrolyte was 1.0 M KFSI in EC:DEC=1:1 Vol%, and assembled into a button-type potassium ion battery. Example

[0048] 0.2 g of P / C negative electrode material and 0.017 g of Se powder were put into an agate mortar and mixed and ground in an argon atmosphere glove box for 20 min, then put into a quartz tube and sealed with a tube sealer. The sealed material was then placed in a muffle furnace and heated to 400 °C at a heating rate of 2 °C / min, kept at this temperature for 12 h, then cooled to room temperature at a cooling rate of 1 °C / min and taken out. The sealed quartz tube was disassembled in an argon atmosphere glove box, and the sample was cleaned with carbon disulfide, then repeatedly rinsed and filtered with alcohol and deionized water in a fume hood, sieved, collected and stored after vacuum drying.

[0049] The modified P / C negative electrode material was mixed with conductive carbon black and sodium alginate in a mass ratio of 7:1.5:1.5 to prepare an electrode as the negative electrode, metallic potassium was used as the counter electrode, and the electrolyte was 1.0 M KFSI in EC:DEC=1:1 Vol%, and assembled into a button-type potassium ion battery.

[0050] 0.2 g of P / C negative electrode material and 0.05 g of Te powder were put into an agate mortar and mixed and ground in an argon atmosphere glove box for 20 min, then put into a quartz tube and sealed with a tube sealer. The sealed material was then placed in a muffle furnace and heated to 400 °C at a heating rate of 2 °C / min, kept at this temperature for 12 h, then cooled to room temperature at a cooling rate of 1 °C / min and taken out. The sealed quartz tube was disassembled in an argon atmosphere glove box, and the sample was cleaned with carbon disulfide, then repeatedly rinsed and filtered with alcohol and deionized water in a fume hood, sieved, collected and stored after vacuum drying.

[0051] The modified P / C negative electrode material was mixed with conductive carbon black and sodium alginate in a mass ratio of 7:1.5:1.5 to prepare an electrode as the negative electrode, metallic potassium was used as the counter electrode, and the electrolyte was 1.0 M KFSI in EC:DEC=1:1 Vol%, and assembled into a button-type potassium ion battery.

[0052] 0.2 g of P / C negative electrode material and 0.025 g of Te powder were put into an agate mortar and mixed and ground in an argon atmosphere glove box for 20 min, then put into a quartz tube and sealed with a tube sealer. The sealed material was then placed in a muffle furnace and heated to 400 °C at a heating rate of 2 °C / min, kept at this temperature for 12 h, then cooled to room temperature at a cooling rate of 1 °C / min and taken out. The sealed quartz tube was disassembled in an argon atmosphere glove box, and the sample was cleaned with carbon disulfide, then repeatedly rinsed and filtered with alcohol and deionized water in a fume hood, sieved, collected and stored after vacuum drying.

[0053] The modified P / C negative electrode material was mixed with conductive carbon black and sodium alginate in a mass ratio of 7:1.5:1.5 to prepare an electrode as the negative electrode, metallic potassium was used as the counter electrode, and the electrolyte was 1.0 M KFSI in EC:DEC=1:1 Vol%, and assembled into a button-type potassium ion battery.

[0054] 0.2 g of P / C negative electrode material and 0.017 g of Te powder were put into an agate mortar and mixed and ground in an argon atmosphere glove box for 20 min, then put into a quartz tube and sealed with a tube sealer. The sealed material was then placed in a muffle furnace and heated to 400 °C at a heating rate of 2 °C / min, kept at this temperature for 12 h, then cooled to room temperature at a cooling rate of 1 °C / min and taken out. The sealed quartz tube was disassembled in an argon atmosphere glove box, and the sample was cleaned with carbon disulfide, then repeatedly rinsed and filtered with alcohol and deionized water in a fume hood, sieved, collected and stored after vacuum drying.

[0055] The modified P / C negative electrode material was mixed with conductive carbon black and sodium alginate in a mass ratio of 7:1.5:1.5 to prepare an electrode as the negative electrode, metallic potassium was used as the counter electrode, and the electrolyte was 1.0 M KFSI in EC:DEC=1:1 Vol%, and assembled into a button-type potassium ion battery.

[0056] 0.2 g of P / C negative electrode material and 0.025 g of S powder were put into an agate mortar and mixed and ground in an argon atmosphere glove box for 20 min, then put into a quartz tube and sealed with a tube sealer. The sealed material was then placed in a muffle furnace and heated to 400 °C at a heating rate of 2 °C / min, kept at this temperature for 12 h, then cooled to room temperature at a cooling rate of 1 °C / min and taken out. The sealed quartz tube was disassembled in an argon atmosphere glove box, and the sample was cleaned with carbon disulfide, then repeatedly rinsed and filtered with alcohol and deionized water in a fume hood, sieved, collected and stored after vacuum drying.

[0057] The modified P / C negative electrode material was mixed with conductive carbon black and sodium alginate in a mass ratio of 7:1.5:1.5 to prepare an electrode as the negative electrode, metallic potassium was used as the counter electrode, and the electrolyte was 1.0 M KFSI in EC:DEC=1:1 Vol%, and assembled into a button-type potassium ion battery.

[0058] The P / C negative electrode material before modification was mixed with conductive carbon black and sodium alginate in a mass ratio of 7:1.5:1.5 to prepare an electrode as the negative electrode, metallic potassium as the counter electrode, and the electrolyte 1.0 M KFSI in EC:DEC=1:1 Vol% to assemble into a button-type potassium ion battery.

[0059] Table 1 Cyclic performance of the negative electrode material of the present invention applied to batteries Initial charge capacity (mAh / g) Charge capacity after 40 cycles (mAh / g) Charge capacity after 80 cycles (mAh / g) Example 1 628.01 670.02 496.78 Example 2 703.47 725.20 568.00 Example 3 650.49 713.80 550.67 Example 4 628.43 712.30 606.98 Example 5 662.47 753.00 583.85 Example 6 665.77 719.11 565.44 Example 7 680.68 726.59 595.52 Example 8 665.66 728.96 637.67 Example 9 602.75 727.05 641.64 Example 10 458.58 514.12 493.44 Embodiment 11 731.30 739.07 632.81 Example 12 653.06 652.40 583.81 Example 13 375.32 421.28 378.90 Comparative Example 1 575.31 593.73 482.88 In combination with the relevant illustrations of the present invention, Figure 3 , 5 This is a mapping diagram of the preparation of the potassium ion battery negative electrode material P / C-Se in the embodiment. It can be seen from the figure that the embodiment contains C element, P element, Se element and each element is evenly distributed. It further shows that the Se element in the sample is successfully coated on the surface of the phosphorus / carbon negative electrode material and no impurities appear.

[0060] In some embodiments, a cycle test was performed on phosphorus / carbon negative electrode materials coated with different amounts of Se at 320°C. The results showed that the initial charge capacity can be increased by 9.16-22.19%, and the charge capacity can be increased by 12.84-22.14% after 40 cycles of activation are basically completed.

[0061] In some embodiments, a cycle test was performed on phosphorus / carbon negative electrode materials coated with different amounts of Se at 360°C. The results showed that the initial charge capacity could be increased by 9.23-15.72%, and the charge capacity could be increased by 19.97-26.82% after 40 cycles of activation were basically completed.

[0062] In some embodiments, a cycle test was performed on phosphorus / carbon negative electrode materials coated with different amounts of Se at 400°C, and the results showed that the initial charge capacity could be increased by 4.76-18.31%, and the charge capacity could be increased by 22.37-22.77% after 40 cycles of activation were basically completed.

[0063] In some embodiments, cycle tests are performed on phosphorus / carbon negative electrode materials coated with the same amount of Se at different temperatures to compare the cycle stability when the charge and discharge specific capacities are significantly improved: the capacity retention rate of Example 2 after the 80th cycle is stable compared with the 40th cycle is 78.32%, the capacity retention rate of Example 5 after the 80th cycle is stable compared with the 40th cycle is 77.53%, and the capacity retention rate of Example 8 after the 80th cycle is stable compared with the 40th cycle is 87.47%.

[0064] In some embodiments, the embodiment 8 with the highest comprehensive performance among the phosphorus / carbon negative electrode materials coated with Se elements at 400°C and the phosphorus / carbon negative electrode materials coated with different Te amounts at 400°C were subjected to cycle tests. It can be seen that after selecting the appropriate coated Te amount, the initial charging specific capacity can be increased by 27.07%, and the capacity retention rate after the 80th cycle is stable compared with the 40th cycle is 85.62%.

[0065] In some embodiments, the phosphorus / carbon negative electrode materials coated with different sulfur elements were tested for cycling at 400°C. In comparison, S coating has better stability, but the charge-discharge specific capacity is significantly reduced. Se and Te coating have obvious advantages in comprehensive stability and charge-discharge specific capacity.

[0066] In some embodiments, the rate performance is significantly improved, with a current density of 100 mA g -1 Gradually increase to 8000mA g -1 The capacity retention rate can be increased to 45.50%.

[0067] It can be seen that the sulfur-modified carbon-phosphorus negative electrode material for potassium ion batteries disclosed in the present invention successfully utilizes the high chemical activity and high electrical conductivity of the sulfide element to improve the electrical conductivity and charge-discharge specific capacity of the phosphorus / carbon negative electrode material for potassium ion batteries, which can be increased by 27.07% compared with the initial charge specific capacity of the comparative example. At the same time, the amorphous phase formed by the sulfide element and phosphorus can serve as a buffer layer, effectively improving its structural / interface stability during potassium storage, thereby improving the electrochemical reversibility and cycle stability of the phosphorus / carbon negative electrode material in potassium ion batteries; and the rate performance is significantly improved, compared with the comparative example, at a current density of 100 mA g -1 Step up to 8000 mA g -1 The capacity retention rate increased from 4.51% to 45.50%.

[0068] The above is only a detailed description of the preferred feasible embodiments of the present invention, and is not intended to limit the present application. For those skilled in the art, the present application may have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.

Claims

1. A method for preparing a sulfur-containing element-modified phosphorus / carbon negative electrode material for potassium ion batteries, The following steps are involved: (1) Preparing a certain ratio of phosphorus / carbon negative electrode materials by mechanical ball milling; (2) mixing the chalcogenide and the phosphorus / carbon negative electrode material prepared in step (1) in a certain proportion, transferring them into a quartz tube reactor, and vacuum melting and sealing them, then keeping the temperature for several hours, and finally cooling them to room temperature to take out the corresponding powder material; (3) Cleaning, grinding and drying the obtained samples under a protective atmosphere; In step (1), the carbon material is conductive carbon black or carbon nanomaterial, the purity of the phosphorus source is 98-99.99%; the phosphorus / carbon ratio is 6:4-8:2 by mass, preferably 6:4 or 7:3 or 8:2; In the step (2), the chalcogen element is selenium, tellurium or sulfur.

2. The method for preparing the sulfide-modified potassium ion battery phosphorus / carbon negative electrode material according to claim 1, Features: The mechanical ball milling method comprises the following steps: 1) Weighing phosphorus element and carbon material according to the phosphorus / carbon ratio as claimed in claim 1; 2) ball-milling the phosphorus element and the carbon material in step 1) in a ball mill, and assembling the ball mill in an argon atmosphere glove box; 3) High-energy ball milling was performed at 200 and 300 rpm for 12 h, respectively, and then at 400 rpm for 24 h; 4) Repeat the ball milling step at least twice to achieve uniform composite of phosphorus and porous carbon at the nanometer scale to obtain phosphorus / carbon negative electrode material.

3. The method for preparing the sulfide-modified potassium ion battery phosphorus / carbon negative electrode material according to claim 1, Features: In the step (2), the mass ratio of the sulfur element to the phosphorus / carbon negative electrode material is 1:2-12, preferably 1:2, 1:4, 1:8, 1:

12.

4. The method for preparing the sulfide-modified potassium ion battery phosphorus / carbon negative electrode material according to claim 1, Features: The step of sealing the chalcogenide element and the phosphorus / carbon negative electrode material in step (2) comprises mixing and grinding the chalcogenide element and the phosphorus / carbon negative electrode material for 20 to 30 minutes and then vacuum sealing the mixture, and storing the mixture in the same space and vacuum sealing the mixture.

5. The method for preparing the sulfide element-modified phosphorus / carbon negative electrode material for potassium ion batteries according to claim 1, Features: The sealing step in step (2) comprises placing a mixture of a chalcogenide element and a phosphorus / carbon negative electrode material in a quartz tube reactor, and performing vacuum melting sealing, followed by heat treatment at a specific temperature for a certain period of time, wherein the heating temperature of the composite material is 300-400° C., and the insulation time is 12-24 hours.

6. The method for preparing the sulfide element-modified phosphorus / carbon negative electrode material for potassium ion batteries according to claim 1, Features: The modified phosphorus / carbon negative electrode material in step (3) is cleaned with carbon disulfide, vacuum dried, ground for 20 to 30 minutes, and vibrated and sieved.

7. A chalcogenide-modified phosphorus / carbon negative electrode material for potassium ion batteries prepared by the method for preparing a chalcogenide-modified phosphorus / carbon negative electrode material for potassium ion batteries according to any one of claims 1 to 6.

8. A method for preparing a battery using the sulfur-containing element-modified potassium ion battery phosphorus / carbon negative electrode material as claimed in claim 7: (1) mixing a potassium ion battery negative electrode material with conductive carbon black and sodium alginate in a mass ratio of m:n:l, wherein m is 60-80 wt.%, n is 10-20 wt.%, l is 10-20 wt.%, and dissolving them in deionized water to obtain a slurry; (2) The slurry obtained in step (1) is uniformly coated on copper foil or aluminum foil, dried at 60-70°C for 10-15 hours, and then cut into circular electrodes; (3) Using the electrode obtained in step (2) as the negative electrode and the potassium metal sheet as the counter electrode, adding electrolyte and assembling into a battery; The electrolyte is 1.0 M KFSI in EC:DEC=1:1 Vol%.

9. According to the method for preparing the sulfide element-modified phosphorus / carbon negative electrode material for potassium ion batteries as claimed in claim 8, Features: The potassium ion battery is also provided with a diaphragm, which is composed of a 14-16 mm polymer diaphragm and a glass fiber diaphragm.

10. A potassium ion battery, Features: Prepared by the preparation method according to any one of claims 8 to 9.