Sulfur polymer molecular framework composite material as well as preparation method and application thereof

By constructing an organic polymer-organic small molecule sulfur polymer molecular framework composite material, the problems of electronic insulation and volume expansion of sulfur cathode in lithium-sulfur batteries were solved, improving the electrochemical performance and cycle life of the battery, and achieving high specific capacity and good charge-discharge performance.

CN118919729APending Publication Date: 2024-11-08HENAN UNIV OF SCI & TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411168636.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In lithium-sulfur batteries, the electronic insulation and volume expansion problems of the sulfur cathode lead to a decline in electrochemical performance, and the shuttle effect seriously affects battery life and capacity.

Method used

An organic polymer-organic small molecule sulfur polymer molecular framework composite material is used. Organic small molecules are linked to organic polymers to construct a molecular framework that provides a channel for lithium-ion transport. Carbon chains are used as a stable skeleton to adapt to volume changes.

Benefits of technology

It improves the electrochemical performance and cycle life of the lithium-sulfur battery cathode, enhances the rate performance of the material, and achieves high specific capacity and good charge-discharge performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919729A_ABST
    Figure CN118919729A_ABST
Patent Text Reader

Abstract

The invention discloses a sulfur polymer molecular framework composite material as well as a preparation method and application thereof, the sulfur polymer molecular framework composite material is optimized, the characteristics of an organic polymer are utilized, small molecules of the organic polymer are grafted on branched chains of the organic polymer, and a sulfur polymer molecular framework is successfully constructed; and after the polymer is expanded from the inside, more active sites are provided for sulfur, a channel can be provided for lithium ion transmission, and the rate capability is improved. According to the preparation process, a carbon chain is used as an organic framework, the carbon chain has good stability and is easy to combine with sulfur, the sulfur chain is combined to the carbon framework to construct a sulfur polymer electrode which is good in stability and adapts to volume change, and due to the fact that a common sulfur polymer is easy to agglomerate, small organic molecules are bonded in the sulfur polymer, so that the volume change of the sulfur polymer electrode is reduced. The constructed sulfur polymer molecular framework can effectively solve the problem, so that the electrochemical performance of the polymer is effectively improved, the cycle life of the polymer is effectively prolonged, the rate capability of the material is improved, and high-rate charge / discharge is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium-sulfur batteries, and in particular relates to a sulfur polymer molecular framework composite material and a preparation method and application thereof. Background Art

[0002] With the rapid development of clean energy such as intermittent and distributed solar and wind energy, there is an urgent need to develop efficient storage devices to collect distributed electricity and stably supply the power grid. Lithium-ion batteries have been used in most energy storage fields, but the energy density of commercial lithium-ion batteries is close to the upper limit, making it difficult to effectively power larger power grids. The widespread use of small electronic devices and electric vehicles has put forward more stringent requirements on the sustainability, low cost and high energy / power density of energy storage equipment. The development of a new generation of high energy density lithium batteries has become the current research focus.

[0003] The emergence of lithium-sulfur batteries (Li-S) has made this type of battery with a high energy density of 1675 mAh g -1 A promising energy storage technology with low cost and high efficiency has been developed, far surpassing the most advanced lithium-ion batteries. Naturally abundant sulfur is considered the most promising candidate due to its environmental and economic characteristics. Battery reactions are usually SS bond breaking / generation and electron transfer, thus realizing the mutual conversion between chemical energy and electrical energy.

[0004] Sulfur is the electrode material with the highest specific energy among known solid rechargeable positive electrode materials, far higher than traditional positive electrode materials. However, sulfur has poor electrochemical stability and is easily pulverized during the cycle. After the material is broken, it will dissolve and diffuse in the electrolyte.

[0005] There are still many challenges to achieve the commercialization of lithium-sulfur batteries: (1) The electronic insulation of elemental sulfur and its discharge products. Elemental sulfur and the final discharge products have extremely low electronic and ionic conductivity, which increases the internal impedance of the battery, causing increased polarization and thus increasing the energy loss inside the battery. At the same time, the later discharge product Li 2 S 2 and Li 2 S will form an insoluble insulating layer on the surface of sulfur particles, further reducing the conductivity of the electrode and hindering the reduction of sulfur, thereby reducing the utilization rate of active materials in the sulfur cathode. (2) Volume strain of sulfur cathode due to the interaction between sulfur and discharge product Li 2S has different densities, so when single sulfur forms polysulfide, it will produce a large volume expansion (about 79%). During the charge and discharge process. The positive electrode surface will produce many irreversible morphological changes due to repeated changes in stress. These changes will cause the electrode material structure to deteriorate and the conduction path to deform, seriously affecting the electrochemical performance of the battery and the battery life. (3) There is a shuttle effect: When the lithium-sulfur battery is working normally, the polysulfide undergoes oxidation reaction at the positive electrode, but in the actual process, due to the concentration difference, the polysulfide will diffuse through the diaphragm to the lithium metal surface to undergo reduction reaction, and then diffuse to the surface of the positive electrode again, and then be oxidized into polysulfide. Thus, a vicious cycle of positive electrode oxidation and negative electrode reduction is formed, which is the shuttle effect. When the shuttle effect is severe, it may cause overcharging of the sulfur positive electrode, and the charging capacity is higher than the discharge capacity in the same cycle. The shuttle effect is the special feature of lithium-sulfur batteries and one of the main reasons for the capacity decay of lithium-sulfur batteries, which reduces the active substances of lithium-sulfur batteries and reduces the coulombic efficiency. Summary of the invention

[0006] In order to solve the problems existing in the above-mentioned prior art, the present invention provides an organic polymer-organic small molecule sulfur polymer molecular framework composite material, and its preparation method and application, by using organic small molecules to connect organic polymers, constructing a molecular framework to provide ion channels for lithium ion transmission. The preparation method of the present invention has a wide range of raw materials, a simple preparation process, and the prepared material has a high actual specific capacity for the positive electrode of a lithium-sulfur battery.

[0007] One of the purposes of the present invention is to provide a method for preparing a sulfide polymer molecular framework composite material, comprising the following steps: Step 1: dissolving a certain amount of organic polymer polyacrylonitrile or polyacrylic acid resin in a solvent and stirring the mixture to prepare an organic polymer precursor solution; Step 2: dissolving a certain amount of organic small molecules in a solvent, stirring with ultrasound until completely dissolved, to prepare an organic small molecule precursor solution; Step 3: taking a certain amount of a mixture of carbon nanotubes and polyvinyl pyrrolidone and dissolving it in a solvent in proportion and then ultrasonically dispersing it; Step 4: Mix the solutions obtained in steps 1, 2 and 3, and stir them evenly to obtain a mixed solution; Step 5, adding sublimed sulfur and a catalyst to the mixed solution obtained in step 4, or adding sublimed sulfur to the mixed solution obtained in step 4; stirring and dispersing by ultrasonication to obtain a mixed solution; Step 6: Disperse the mixed solution obtained in step 5 in the salt template and keep it at 235-265° C. for a certain period of time under Ar atmosphere; Step 7, the product solution after the heat preservation in step 6 is fully washed in a detergent and separated and dried; Step 8: Grind the dried material from step 7 and diffuse it for a certain time under certain temperature conditions. After the diffusion is completed, the product is sieved to obtain a sulfide polymer molecular framework composite material.

[0008] As a preferred embodiment, the mass ratio of the polyacrylonitrile in step 1 to the organic small molecule in step 2 is 1:1-2.1.

[0009] As a preferred embodiment, the mass ratio of the polyacrylic acid resin in step one to the organic small molecule in step two is 1:0.2-0.65.

[0010] As a preferred embodiment, in step seven, the detergent is a mixed solution of water and anhydrous ethanol, wherein the volume ratio of water to anhydrous ethanol is 4:1.

[0011] As a preferred embodiment, in step seven, the drying conditions are as follows: the drying temperature range is 55-65° C. under vacuum conditions, and the drying time is 10-15 h.

[0012] As a preferred solution, the following steps are included: Step 1: dissolving a certain amount of polyacrylonitrile in N,N-dimethylformamide and stirring evenly to prepare an organic polymer precursor solution; Step 2: dissolving a certain amount of p-phenylenediamine in N,N-dimethylformamide solution, stirring by ultrasonic until completely dissolved, for preparing an organic small molecule precursor solution; Step 3: taking a certain amount of a mixture of carbon nanotubes and polyvinyl pyrrolidone and dissolving it in N, N-dimethylformamide according to a certain proportion and performing ultrasonic dispersion; Step 4: Mix the solutions obtained in steps 1, 2 and 3, and stir them evenly to obtain a mixed solution; Step 5, adding sublimed sulfur to the mixed solution obtained in step 4, and uniformly dispersing by ultrasonic stirring to obtain a mixed solution; Step 6: Disperse the mixed solution obtained in step 5 in the salt template and keep it warm at 235-265° C. for a certain period of time under Ar atmosphere; Step 7, the product solution after the heat preservation in step 6 is fully washed in a detergent and separated and dried; Step 8: Grind the dried material from step 7 and diffuse it under a certain temperature for more than 12 hours. After the diffusion is completed, the product is sieved to obtain a sulfide polymer molecular framework composite material.

[0013] As a preferred solution, step 1, dissolving a certain amount of organic polymer polyacrylic acid resin in a solvent and stirring the mixture evenly to prepare an organic polymer precursor solution; Step 2: dissolving a certain amount of 5-aminoisophthalic acid or trithiocyanate in a solvent, stirring with ultrasound until completely dissolved, and using it to prepare an organic small molecule precursor solution; Step 3: taking a certain amount of a mixture of carbon nanotubes and polyvinyl pyrrolidone and dissolving it in a solvent in proportion and then ultrasonically dispersing it; Step 4: Mix the solutions in steps 1, 2 and 3, and stir evenly to obtain a mixed solution; Step 5, adding sublimed sulfur and a catalyst to the mixed solution obtained in step 4; and uniformly dispersing by ultrasonic stirring to obtain a mixed solution; Step 6: Disperse the mixed solution obtained in step 5 in the salt template and keep it warm at 235-265° C. for a certain period of time under Ar atmosphere; Step 7, the product solution after the heat preservation in step 6 is fully washed in a detergent and separated and dried; Step 8: Grind the dried material from step 7 and diffuse it under a certain temperature for more than 12 hours. After the diffusion is completed, the product is sieved to obtain a sulfide polymer molecular framework composite material.

[0014] As a preferred embodiment, in step 5, the catalyst includes potassium iodide, elemental iodine and iodophenyl diacetic acid.

[0015] The second purpose of the present invention is to provide a sulfide polymer molecular framework composite material, which is a layered material; the sulfide polymer molecular framework composite material is prepared from an organic polymer and an organic small molecule, wherein the organic polymer is polyacrylonitrile or polyacrylic acid resin, and the organic small molecule is used to connect the main structure of two organic polymer chains.

[0016] The third object of the present invention is to use the above-mentioned sulfide polymer molecular framework composite material in the preparation of battery positive electrode materials.

[0017] Compared with the prior art, the present invention has at least one of the following beneficial effects: First, the present invention optimizes the sulfide polymer molecular framework composite material, utilizes the characteristics of organic polymers, grafts small molecules of organic polymers onto the side chains of organic polymers, and successfully constructs a sulfide polymer molecular framework. After the polymer is expanded from the inside, more active sites are provided for sulfur and channels can be provided for the transmission of lithium ions to improve rate performance.

[0018] Second, the preparation process of the present invention uses polyacrylonitrile and polyacrylic acid as raw materials, which have a wide range of sources; the present invention uses the salt template method for synthesis, which has high preparation efficiency and can provide the possibility for large-scale production of electrodes. The preparation process of the present invention uses the carbon chain as the organic skeleton. The carbon chain is naturally stable and easy to combine with sulfur. By combining the sulfur chain with the carbon skeleton, a sulfide polymer electrode with good stability and adaptability to volume changes is constructed. Since ordinary sulfide polymers are prone to agglomeration, the sulfide polymer molecular framework constructed by bonding organic small molecules in the sulfide polymer can effectively solve this problem, thereby effectively improving the electrochemical performance and cycle life of the polymer, improving the rate performance of the material, and achieving high-rate charge / discharge.

[0019] Third, the present invention also provides an application of a sulfide polymer molecular framework composite material; the battery positive electrode material prepared using the sulfide polymer molecular framework composite material of the present invention exhibits excellent electrochemical properties, for example, the composite material has a specific capacity of 1105.1 mAh / g at a current density of 0.3 C, and the capacity remains at 967.3 mAh / g after 100 cycles. At a current density of 5 C, it still has a reversible capacity of 726 mAh / g. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 The full XPS spectrum of the molecular framework of polyacrylonitrile grafted p-phenylenediamine sulfide polymer of Example 1 of the present invention; Figure 2 This is an XPS C1s high-resolution image of the molecular framework of the polyacrylonitrile grafted p-phenylenediamine sulfide polymer of Example 1 of the present invention; Figure 3 This is an XPS S2p high-resolution image of the molecular framework of the polyacrylonitrile grafted p-phenylenediamine sulfide polymer of Example 1 of the present invention; Figure 4 This is an XPS N1s high-resolution image of the molecular framework of the polyacrylonitrile grafted p-phenylenediamine sulfide polymer of Example 1 of the present invention; Figure 5 Fourier transform infrared spectra of the sulfide polymer molecular frameworks of Example 1, Comparative Example 1 and Comparative Example 2 of the present invention; Figure 6 The Raman spectra of the sulfide polymer molecular frameworks of Example 1, Comparative Example 1 and Comparative Example 2 of the present invention; Figure 7 This is a transmission electron microscope image of the molecular framework of the polyacrylonitrile grafted p-phenylenediamine sulfide polymer of Example 1 of the present invention; Figure 8 The cycling curve at a current density of 0.3 C when the polyacrylonitrile grafted p-phenylenediamine sulfide polymer molecular framework of Example 1 of the present invention is used as a positive electrode material for a lithium-sulfur battery; Fig. 9This is a rate performance diagram at current densities of 1 C, 2 C, 3 C, 4 C, and 5 C when the polyacrylonitrile grafted p-phenylenediamine sulfide polymer molecular framework of Example 1 of the present invention is used as a positive electrode material for a lithium-sulfur battery; Fig.10 The cycle curve at a current density of 0.3 C when the polyacrylonitrile sulfide polymer of Comparative Example 1 of the present invention is used as a positive electrode material for a lithium-sulfur battery; Fig.11 This is a rate performance diagram at current densities of 1 C, 2 C, 3 C, 4 C, and 5 C when the polyacrylonitrile sulfide polymer of Comparative Example 1 of the present invention is used as a positive electrode material for a lithium-sulfur battery; Fig.12 The cycle curve at a current density of 0.3 C when the p-phenylenediamine sulfide polymer of Comparative Example 2 of the present invention is used as a positive electrode material for a lithium-sulfur battery; Fig.13 This is a rate performance diagram at current densities of 1 C, 2 C, 3 C, 4 C, and 5 C when the p-phenylenediamine sulfide polymer of Comparative Example 2 of the present invention is used as a positive electrode material for a lithium-sulfur battery; Fig.14 This is the full XPS spectrum of the molecular framework of polyacrylic acid grafted trithiocyanate sulfopolymer according to Example 4 of the present invention; Fig.15 This is the XPS C1s high-resolution image of the molecular framework of polyacrylic acid grafted trithiocyanate sulfopolymer according to Example 4 of the present invention; Fig.16 This is the XPS N1s high-resolution image of the molecular framework of polyacrylic acid grafted trithiocyanate sulfopolymer according to Example 4 of the present invention; Fig.17 This is the XPS S2p high-resolution image of the molecular framework of polyacrylic acid grafted trithiocyanate sulfopolymer according to Example 4 of the present invention; Fig.18 The cycle curve at a current density of 0.3 C when the polyacrylic acid grafted trithiocyanate composite material of Example 4 of the present invention is used as a positive electrode material for a lithium-sulfur battery; Fig.19 The full XPS spectrum of the molecular framework of polyacrylic acid grafted 5-aminoisophthalic acid sulfide polymer of Example 5 of the present invention; Fig. 20 This is a high-resolution XPSC1s image of the molecular framework of the polyacrylic acid grafted 5-aminoisophthalic acid sulfide polymer of Example 5 of the present invention; Fig.21 This is a high-resolution XPSN1s image of the molecular framework of polyacrylic acid grafted 5-aminoisophthalic acid sulfide polymer of Example 5 of the present invention; Fig. 22 This is an XPSS2p high-resolution image of the molecular framework of polyacrylic acid grafted 5-aminoisophthalic acid sulfide polymer according to Example 5 of the present invention; Fig.23 The Fourier transform infrared spectrum of the polyacrylic acid grafted 5-aminoisophthalic acid sulfide polymer molecular framework of Example 5 of the present invention; Fig.24 The cycle curve at a current density of 0.3 C when the polyacrylic acid grafted 5-aminoisophthalic acid composite material of Example 5 of the present invention is used as a positive electrode material for a lithium-sulfur battery; Fig.25 The cycling curve at a current density of 0.3 C when the polyacrylonitrile grafted p-phenylenediamine sulfide polymer molecular framework of Example 2 of the present invention is used as a positive electrode material for a lithium-sulfur battery; Fig.26 The cycling curve at a current density of 0.3 C when the polyacrylonitrile grafted p-phenylenediamine sulfide polymer molecular framework of Example 3 of the present invention is used as a positive electrode material for a lithium-sulfur battery; Fig. 27 Schematic diagram of the preparation principle of Examples 1-3 of the present invention.

[0021] The Chinese meanings of the horizontal and vertical axes in the figure are: Intensity means intensity; Binding energy means bond energy; Wavenumber means wavelength; Raman shfit means Raman spectrum; Cycle number means the number of cycles; Specific capacity means specific capacity. DETAILED DESCRIPTION

[0022] In order to make the technical means, creative features, objectives and beneficial effects achieved by the present invention easy to understand, the present invention is further explained below in conjunction with specific implementation methods.

[0023] In addition, in order to better illustrate the present invention, numerous specific details are given in the specific embodiments below. Those skilled in the art should understand that the present invention can also be implemented without certain specific details. In other embodiments, methods, means, equipment and steps well known to those skilled in the art are not described in detail in order to highlight the main purpose of the present invention.

[0024] Example 1 In this example, polyacrylonitrile grafted p-phenylenediamine sulfide polymer molecular framework (abbreviated as: PAN@PPD@S) is prepared, and the preparation steps are as follows: (1) Preparation of polyacrylonitrile (PAN) precursor solution: 0.3 g of polyacrylonitrile (PAN) (150,000 g mol -1 ) was dissolved in 8 mL of N, N-dimethylformamide solution and stirred evenly; (2) Preparation of organic small molecule precursor solution: 0.4732 g of p-phenylenediamine (PPD) was dissolved in 8 mL of N,N-dimethylformamide solution and ultrasonically stirred until completely dissolved; wherein the mass ratio of polyacrylonitrile (PAN) to p-phenylenediamine (PPD) was 1:1.53; wherein the purity of p-phenylenediamine used in this example was 97%; (3) Dissolve a mixture of 0.05 g carbon nanotubes (CNT) and 0.01 g polyvinyl pyrrolidone (PVP) in 5 ml N, N-dimethylformamide solution and disperse by ultrasonication; (4) Mix the solutions in steps (1), (2) and (3) and stir to obtain a mixed solution; (5) Add 3.0 g of sublimated sulfur to the mixed solution obtained in step (4), and stir thoroughly with ultrasonic to disperse it evenly; (6) Disperse the mixed solution obtained in step (5) in 70 g of KCl salt template and keep it at 235 °C for 3 h under Ar atmosphere; (7) Dissolve the product after heat preservation in step (6) in 800 mL of a mixed solution of water and anhydrous ethanol, wash thoroughly, centrifuge and dry; wherein the volume ratio of water to anhydrous ethanol is 4:1; (8) The dried material in step (7) was ground and then diffused in a reactor at 160°C for 12 h. After the mixture was dried, the product was sieved through a 300-mesh sieve to obtain an organic polymer-organic small molecule sulfur; polymer molecular framework composite material PAN@PPD@S. The product mass was 2.478 g, and the mass yield was 65.8%.

[0025] The organic polymer-organic small molecule sulfur polymer molecular framework composite material PAN@PPD@S obtained in Example 1 is used to prepare a PAN@PPD@S lithium-sulfur battery. In this application example, the PAN@PPD@S positive electrode composite material, carbon black (Super-P) and polyvinylidene fluoride (PVDF) are mixed in a mass ratio of 7:2:1 to prepare the positive electrode, and the fully mixed slurry is evenly coated on aluminum foil. The active material (PAN@PPD@S positive electrode composite material) loading amount is 1-3 mg / cm 2 The following tests used an active substance loading of 1.2 mg / cm 2 Aluminum foil was then vacuum dried at 60 °C for 12 h. In addition, metallic lithium was used as the negative electrode, and the electrolyte was LiN (CF 3 SO 2 ) 2 (1 M) and LiNO 3(0.1 M) in a mixed solvent of 1,3-dioxypolyalkane and dimethyl ether, the volume ratio of 1,3-dioxypolyalkane and dimethyl ether in the mixed solvent is 1:1. The separator used is a microporous polypropylene film (Celgard 2400). The electrochemical performance tests performed below were performed after assembling CR2025 coin cells in an Ar-filled glove box.

[0026] In this example 1, a PAN@PPD@S cathode composite material was prepared using a salt template. In order to study the chemical state of the prepared PAN@PPD@S sulfide polymer molecular framework, we performed XPS characterization on it. The results are as follows: Figure 1-4 The XPS spectrum of the PAN@PPD@S sulfide polymer molecular framework ( Figure 1 ) It can be seen that its main components are C, N, O and S elements. Figure 2 As shown in the high-resolution XPS C 1S of the PAN@PPD@S sulfide polymer molecular framework, the characteristic peak at 284.7 eV corresponds to the typical CC bond. It should be pointed out that the typical C≡N bond in the PAN raw material does not appear, and the peaks at 285.7 eV and 286.3 eV correspond to the characteristic peaks of the typical CN bond and CS bond. This result shows that the C≡N bond is opened and CN and CS bonds are formed during the preparation of the sulfide polymer. In the XPS high-resolution S 2P ( Figure 3 ), the peaks at 163.5 eV and 164.8 eV correspond to S 2p3 / 2 and S2p1 / 2 of SS bonds, respectively, and the peaks at 161.3 eV and 162.2 eV correspond to CS bonds, again proving that sulfur was successfully grafted into the polymer. In the high-resolution XPS N1s, the characteristic peak at 399.9 eV corresponds to the CNC bond, 398.7 eV is the characteristic peak of SCN, and 397.8 eV corresponds to the -NH- bond ( Figure 4 ) This result indicates that during the preparation process, the C≡N bond in the raw material PAN is broken and combines with the amine group and sulfur molecule of PPD to build a molecular framework.

[0027] In Raman spectroscopy ( Figure 6 ), at 1338 cm -1 and 1562 cm -1 Two strong peaks appeared at 1338 cm -1 The absorption peak at 1562 cm represents the Sp3 CC bond from the material in the disordered structure. -1 The peak at 386 cm shows the Sp2 C=C bond of the material, while the peak at 386 cm −1 and 111 cm −1 、131 cm −1The peaks on the left and right confirm the formation of CS / NS and SS bonds, respectively. −1 The weak peak at 472 cm -1 The peaks around the center are attributed to the SCN bonds in the molecular framework, indicating the successful construction of PAN@PPD@S. Figure 7 This is the TEM image of the PAN@PPD@S positive electrode material prepared in Example 1. The PAN@PPD@S material synthesized using a salt template has a well-dispersed nanosheet structure with uniform pore distribution. Figure 8 The discharge specific capacities of the PAN@PDD@S electrode material at 0.3 C for the first and 100th cycles are 1105.1 mAhg -1 and 967.3 mAh g -1 9 In order to study the charge and discharge performance of PAN@PPD@S cathode materials at high rates, the rate performance of PAN@PPD@S was tested in the range of 1 C to 5 C. It was found that the capacities of PAN@PPD@S electrode at 1 C, 2 C, 3 C, 4 C and 5 C were 969, 886, 800, 753 and 726 mAh g, respectively. -1 Even at 5.0C rate, the PAN@PPD@S electrode still achieved 726 mAh g -1 The high discharge specific capacity is based on the successful construction of the sulfide polymer molecular framework.

[0028] Example 2 In this example, polyacrylonitrile grafted p-phenylenediamine sulfide polymer molecular framework (abbreviated as: PAN@PPD@S) is prepared, and the preparation steps are as follows: (1) Preparation of PAN precursor solution: 0.3 g of polyacrylonitrile (PAN) (150,000 g mol -1 ) was dissolved in 8 mL of N, N-dimethylformamide solution and stirred evenly; (2) Preparation of organic small molecule precursor solution: 0.3155 g of p-phenylenediamine (PPD) was dissolved in 8 ml of N,N-dimethylformamide solution and ultrasonically stirred until completely dissolved; the solution was prepared according to a molar mass ratio of polyacrylonitrile (PAN) to p-phenylenediamine (PPD) of 1:1.02; the purity of p-phenylenediamine used in this example was 97%.

[0029] (3) Dissolve a mixture of 0.05 g carbon nanotubes (CNT) and 0.01 g polyvinyl pyrrolidone (PVP) in 5 ml N, N-dimethylformamide solution and disperse by ultrasonication; (4) Mix the solutions in steps (1), (2) and (3) and stir to obtain a mixed solution; (5) Add 3.0 g of sublimed sulfur to the mixed solution obtained in step (4), and stir and disperse the mixture by ultrasonic stirring to obtain a mixed solution; (6) Disperse the mixed solution obtained in step (5) in 70 g of KCl salt template and keep it at 235 °C for 3 h under Ar atmosphere; (7) Dissolve the product after heat preservation in step (6) in 800 mL of a mixed solution of water and anhydrous ethanol, wash thoroughly, centrifuge and dry, wherein the volume ratio of water to anhydrous ethanol is 4:1; (8) The dried material in step (7) was ground and diffused in a reactor at 160°C for 12 h. After the mixture was dried, the product was sieved through a 300-mesh sieve to obtain an organic polymer-organic small molecule sulfide polymer molecular framework composite material PAN@PPD@S. The mass of the composite material product was 1.847 g, and the mass yield was 51.1%.

[0030] Example 3 In this embodiment, polyacrylonitrile grafted p-phenylenediamine sulfide polymer molecular framework (abbreviated as: PAN@PPD@S) is prepared, and the method steps are as follows: (1) Preparation of PAN precursor solution: 0.3 g of polyacrylonitrile (PAN) (150,000 g mol -1 ) was dissolved in 8 mL of N, N-dimethylformamide solution and stirred evenly; (2) Preparation of organic small molecule precursor solution: 0.6310 g of p-phenylenediamine (PPD) was dissolved in 8 ml of N,N-dimethylformamide solution and ultrasonically stirred until completely dissolved; the solution was prepared according to a mass ratio of polyacrylonitrile (PAN) to p-phenylenediamine (PPD) of 1:2.04. The purity of p-phenylenediamine used in this example was 97%.

[0031] (3) Dissolve a mixture of 0.05 g carbon nanotubes (CNT) and 0.01 g polyvinyl pyrrolidone (PVP) in 5 ml N, N-dimethylformamide solution and disperse by ultrasonication; (4) Mix the solutions in steps (1), (2) and (3) and stir to obtain a mixed solution; (5) Add 3.0 g of sublimed sulfur to the mixed solution obtained in step (4), and stir and disperse the mixture by ultrasonic stirring to obtain a mixed solution; (6) Disperse the mixed solution obtained in step (5) in 70 g of KCl salt template and keep it at 235 °C for 3 h under Ar atmosphere; (7) Dissolve the product after heat preservation in step (6) in a mixed solution of water and anhydrous ethanol (800 mL), wash thoroughly, centrifuge and dry, wherein the volume ratio of water to anhydrous ethanol is 4:1; (8) The dried material in step (7) was ground and then diffused in a reactor at 160°C for 12 h. After the mixture was dried, the product was sieved through a 300-mesh sieve to obtain an organic polymer-organic small molecule sulfur polymer molecular framework composite material PAN@PPD@S. The mass of the composite material product was 2.147 g, and the mass yield was 54.6%.

[0032] In this scheme, the organic polymer-organic small molecule sulfur polymer molecular framework composite material PAN@PPD@S obtained in Example 2 and Example 3 is used to prepare PAN@PPD@S lithium-sulfur battery, which is the same as the preparation test steps and control parameters of the above Example 1. The only difference is that the corresponding PAN@PPD@S positive electrode composite materials prepared in each example are used respectively.

[0033] Example 4 This embodiment provides a polyacrylic acid grafted trithiocyanate sulfide polymer molecular framework composite material (abbreviated as: TTCA@S@PAA), and the preparation steps are as follows: (1) Preparation of PAA precursor solution: 0.2 g polyacrylic acid (PAA) (450,000 g mol -1 ) were dissolved in 10 g of anhydrous ethanol solution and stirred evenly; (2) Preparation of organic small molecule precursor solution: Dissolve 0.0432 g of thiocyanuric acid (thiocyanuric acid, TTCA) in 5 ml of N,N-dimethylformamide solution and stir ultrasonically until completely dissolved; the mass ratio of polyacrylic acid (PAA) to thiocyanuric acid (TTCA) is 1:0.21; the purity of thiocyanuric acid used in this example is 97%; (3) Dissolve a mixture of 0.05 g carbon nanotubes (CNT) and 0.01 g polyvinyl pyrrolidone (PVP) in 5 ml anhydrous ethanol and disperse by ultrasonication; (4) Mix the solutions in steps (1), (2) and (3) and stir to obtain a mixed solution; (5) Add 3.0 g of sublimated sulfur, 0.15 g of potassium iodide, 0.11 g of elemental iodine and 0.15 g of iodophenyl diacetic acid catalyst to the mixed carbon nanotube (CNT) solution obtained in step (4), and stir and disperse the mixture by ultrasonic stirring to obtain a mixed solution; (6) Disperse the mixed solution obtained in step (5) in 70 g of KCl salt template and keep it at 260 °C under Ar atmosphere; (7) Dissolve the product after heat preservation in step (6) in a mixed solution of water and anhydrous ethanol (800 mL), wash thoroughly, centrifuge and dry, wherein the volume ratio of water to anhydrous ethanol is 4:1; (8) The dried material in step (7) was ground and then diffused in a reactor at 160°C for 12 h. After the mixture was dried, the product was sieved through a 300-mesh sieve to obtain an organic polymer-organic small molecule sulfide polymer molecular framework composite material TTCA@S@PAA. The mass of the composite material product was 2.147 g, and the mass yield was 66.2%.

[0034] The positive electrode was prepared by mixing the TTCA@S@PAA positive electrode composite material prepared in Example 4, carbon black (Super-P) and polyvinylidene fluoride (PVDF) in a mass ratio of 7:2:1. The fully mixed slurry was evenly coated on an aluminum foil. The active material (TTCA@S@PAA positive electrode composite material) loading amount was 1-3 mg / cm 2 The following tests used a loading of 1.2 mg / cm 2 Aluminum foil was then vacuum dried at 60 °C for 12 h. In addition, metallic lithium was used as the negative electrode, and the electrolyte was LiN (CF 3 SO 2 ) 2 (1 M) and LiNO 3 (0.1 M), the volume ratio of 1,3-dioxypolyalkane and dimethyl ether in the mixed solvent is 1:1. The separator used is a microporous polypropylene film (Celgard 2400). The electrochemical performance tests performed below were performed after assembling CR2025 coin cells in an Ar-filled glove box.

[0035] The polyacrylic acid grafted trithiocyanate (TTCA@S@PAA) sulfide polymer molecular framework composite material was assembled into a lithium-sulfur battery to test the electrochemical performance. As shown in the figure, at a current density of 0.3 C, the specific capacity can reach 1100.5 mAh / g, and after 100 cycles, the capacity remains at 1001.5 mAh / g.

[0036] Example 5 This embodiment provides a polyacrylic acid grafted 5-aminoisophthalic acid sulfide polymer molecular framework composite material (abbreviated as: 5-AIPA@S@PAA), and the preparation steps are as follows: (1) Preparation of PAA precursor solution: 0.2 g polyacrylic acid (PAA) (450,000 g mol -1 ) were dissolved in 10 g of anhydrous ethanol solution and stirred evenly; (2) Preparation of organic small molecule precursor solution: Dissolve 0.1284 g of 5-aminoisophthalic acid (5-AIPA) in 5 ml of N,N-dimethylformamide solution and stir with ultrasonic until completely dissolved; the mass ratio of PAA to 5-aminoisophthalic acid (5-AIPA) is 1:0.61; wherein the purity of 5-aminoisophthalic acid used in this example is 98%; (3) Dissolve a mixture of 0.05 g carbon nanotubes (CNT) and 0.01 g polyvinyl pyrrolidone (PVP) in 5 ml anhydrous ethanol and disperse by ultrasonication; (4) Mix the solutions in steps (1), (2) and (3) and stir to obtain a mixed solution; (5) Add 3.0 g of sublimed sulfur, 0.15 g of potassium iodide, 0.11 g of elemental iodine and 0.15 g of iodophenyl diacetic acid catalyst to the mixed solution in step (4), and stir and disperse them evenly with ultrasonic stirring to obtain a mixed solution; (6) Disperse the mixed solution in step (5) in 70 g of KCl salt template and keep it at 260 °C for 3 hours under Ar atmosphere; (7) dissolving the product after heat preservation in step (6) in a mixed solution (800 mL) of water and anhydrous ethanol in a volume ratio of 4:1, washing the mixture thoroughly and drying the mixture; (8) The dried material in step (7) was ground and then diffused in a reactor at 160°C for 12 h. After the mixture was dried, the product was sieved through a 300-mesh sieve to obtain an organic polymer-organic small molecule sulfide polymer molecular framework composite material 5-AIPA@S@PAA. The mass of the composite material product was 1.674 g, and the mass yield was 50.2%.

[0037] The positive electrode was prepared by mixing the 5-PAIPA@S@PAA positive electrode composite material prepared in Example 5, carbon black (Super-P) and polyvinylidene fluoride (PVDF) in a mass ratio of 7:2:1. The fully mixed slurry was evenly coated on an aluminum foil. The active material (5-PAIPA@S@PAA positive electrode composite material) loading amount was 1-3 mg / cm 2 The following tests used an active substance loading of 1.5 mg / cm 2 Aluminum foil was used and then vacuum dried at 60 °C for 12 h. In addition, metallic lithium was used as the negative electrode and the electrolyte was LiN (CF 3 SO 2 ) 2 (1 M) and LiNO 3(0.1 M), the volume ratio of 1,3-dioxypolyalkane and dimethyl ether in the mixed solvent is 1:1, and the separator used is a microporous polypropylene film (Celgard 2400). The electrochemical performance tests performed below were performed after assembling CR2025 coin cells in an Ar-filled glove box.

[0038] In order to further explore the molecular structure of 5-AIPA@S@PAA, XPS test was carried out. Fig.19 The XPS spectrum shown shows obvious signals of S 2p, C 1s, N 1s, and O 1s. The O 1s peak is due to the adsorption of O in the atmosphere on the surface of the material during transportation and measurement. 2 or CO 2 After peak fitting, it can be seen that the high-resolution C 1s peak is divided into 4 peaks ( Fig. 20 ), SC=N at 288.4 eV, CS at 285.5 eV, CC / C=C / CN at 284.6 eV, and CN at 286.5 eV. Fig.21 As shown, the high-resolution N 1s spectrum also has three peaks at 398.0 eV, 399.8 eV, and 401.3 eV, which are C=N, CN, and SC=N bonds, respectively. Fig. 22 The high-resolution S 2p peaks in the graph are at 163.3 and 164.5 eV, which are the S 2p of C-S bond, respectively. 3 / 2 and S 2p 1 / 2 , the peaks at 165.5 and 166.7 eV can be attributed to the S 2p of C-C bonds 3 / 2 and S 2p 1 / 2 , the peak at 168.5 eV is the SO bond.

[0039] To further explore the molecular structure of 5-AIPA@S@PAA, FT-IR spectroscopy tests were performed, such as Fig.23 There is no CH in the FT-IR spectrum of 5-AIPA@S@PAA. 2 At 804 cm ‒1 The torsion peak at 1711 cm ‒1 The stretching peak at 2500 cm ‒1 The stretching peak at 1623 cm ‒1 A clear peak of 5-AIPA@S@PAA was observed at 874 cm ‒1 The peak is the vibration of the CS bond, indicating that the S element is successfully bonded to the PAA carbon skeleton.

[0040] The polyacrylic acid grafted 5-aminoisophthalic acid cathode composite material was assembled into a lithium-sulfur battery to test the electrochemical performance, such as Fig.24 As shown in Figure 2, at a current density of 0.3 C, the specific capacity can reach 1150 mAh g -1 After 100 cycles, the capacity remains at 1059 mAh g -1 .

[0041] Comparative Example 1 In this comparative example, a polyacrylonitrile and sulfide polymer composite material (abbreviated as: PAN@S) is prepared, and the steps are as follows: (1) Preparation of PAN precursor solution: Prepare PAN and p-phenylenediamine in a ratio of 1:1. Add 0.3 g of PAN (150,000 g mol -1 ) was dissolved in 8 mL of N, N-dimethylformamide solution and stirred evenly; (2) A mixture of 0.05 g CNT and 0.01 g PVP was dissolved in 5 ml N, N-dimethylformamide solution and dispersed by ultrasonication. (3) mixing the solutions in steps (1) and (2), and stirring to obtain a mixed solution; (4) Add 3.0 g of sublimated sulfur to the mixed solution obtained in step (3), and stir thoroughly with ultrasonic stirring to disperse the mixture evenly; (5) Disperse the mixed solution in step (4) in 70 g of KCl salt template and keep it at 235 °C for 3 h under Ar atmosphere; (7) dissolving the product after heat preservation in step (5) in a mixed solution (800 mL) of water and anhydrous ethanol in a volume ratio of 4:1, washing thoroughly, centrifuging, and drying; (8) The dried material in step (7) was ground and diffused in a reactor at 160°C for 12 h. After the mixture was dried, the product was sieved through a 300-mesh sieve to obtain a polyacrylonitrile and sulfur composite material of 1.73 g with a mass yield of 52.0%.

[0042] The method for preparing PAN@S lithium-sulfur battery in this comparative example is as follows: The positive electrode was prepared by mixing PAN@S positive electrode composite material, carbon black (Super-P) and polyvinylidene fluoride (PVDF) in a mass ratio of 7:2:1. The fully mixed slurry was evenly coated on aluminum foil. The active material (PAN@S positive electrode composite material) loading was 1.3 mg / cm 2 The test was then carried out at 60 °C under vacuum for 12 h. In addition, metallic lithium was used as the negative electrode, and the electrolyte was composed of LiN (CF 3 SO 2 ) 2 (1 M) and LiNO 3(0.1 M) in a mixed solvent of 1,3-dioxypolyalkane and dimethyl ether, the volume ratio of 1,3-dioxypolyalkane and dimethyl ether in the mixed solvent is 1:1. The separator used is a microporous polypropylene film (Celgard 2400). The electrochemical performance tests performed below were performed after assembling CR2025 coin cells in an Ar-filled glove box.

[0043] Comparative Example 2 In this comparative example, a composite material of p-phenylenediamine and sulfur (referred to as PPD@S) is prepared, and the steps are as follows: (1) Preparation of organic small molecule precursor solution: Dissolve 0.6310 g of p-phenylenediamine in 8 ml of N,N-dimethylformamide solution and stir by ultrasonic until completely dissolved; (2) Dissolve a mixture of 0.05 g CNT and 0.01 g PVP in 5 ml N, N-dimethylformamide solution and disperse by ultrasonication; (3) Mix the solutions in steps (1) and (2), and stir to obtain a mixed solution; (4) Add 3.0 g of sublimated sulfur to the mixed solution in step (3) and stir thoroughly with ultrasonic to disperse evenly; (5) Disperse the mixed solution in step (4) in 70 g of KCl salt template and keep it at 235 °C for 3 h under Ar atmosphere; (6) The product after incubation was dissolved in a mixed solution (800 mL) of water and anhydrous ethanol in a volume ratio of 4:1, washed thoroughly, centrifuged and dried; (7) The dried material in step (6) was ground and then diffused in a reactor at 160°C for 12 h. After the mixture was dried, the product was sieved through a 300-mesh sieve to obtain a composite material of p-phenylenediamine and sulfur (1.83 g) with a mass yield of 50.6%.

[0044] The method for preparing the PPD@S lithium-sulfur battery in this comparative example is as follows: The positive electrode was prepared by mixing PPD@S positive electrode composite material, carbon black (Super-P) and polyvinylidene fluoride (PVDF) in a mass ratio of 7:2:1. The fully mixed slurry was evenly coated on aluminum foil. The active material (PPD@S positive electrode composite material) loading was 1.2 mg / cm 2 , and then dried in vacuum at 60 °C for 12 h. In addition, metallic lithium was used as the negative electrode, and the electrolyte was LiN (CF 3 SO 2 ) 2 (1 M) and LiNO 3(0.1 M), the volume ratio of 1,3-dioxypolyalkane and dimethyl ether in the mixed solvent is 1:1. The separator used is a microporous polypropylene film (Celgard 2400). The electrochemical performance tests performed below were performed after assembling CR2025 coin cells in an Ar-filled glove box.

[0045] By comparing Example 1, Comparative Example 1 and Comparative Example 2, the cycle performance under 0.3 C is as follows Figure 8 , 10 , 12, among which PAN@PDD@S electrode exhibits the highest capacity and the best cycle stability, with the discharge specific capacity of 1105 mAh g after the first and 100th cycles, respectively. -1 and 967 mAh g -1 The capacity decay per cycle is only 0.12%. In contrast, the initial discharge capacity of PAN@S and PPD@S electrode materials is only 1005 mAh g -1 and 1002 mAh -1 , the capacity retention rate after 100 cycles is less than 74% and 69%. In order to study the effect of the molecular framework on the rate performance of the sulfide polymer, the rate performance of Comparative Example 1, Comparative Example 1 and Comparative Example 2 was tested in the range of 1C to 5C. The test results are as follows Fig. 9 , 11 , 13. The capacity of PAN@PPD@S electrode is significantly higher than that of PAN@S and PPD@S, with the capacities of 969, 886, 800 and 753 at 1 C, 2 C, 3 C and 4 C, respectively. Even at 5 C rate, PAN@PPD@S electrode still achieved 726 mAh g -1 However, the capacity of PAN@S and PPD@S electrodes at a high rate of 5 C is only 489 mAh g -1 and 339 mAhg -1 When the rate is restored to 1 C, the discharge specific capacity of the PAN@PPD@S electrode can almost be restored to the initial value, indicating that the PAN@PPD@S electrode material has good electrochemical reversibility and a stable structure. The electrochemical performance tests in the above embodiments and comparative examples of this scheme are performed after assembling CR2025 coin cells in an Ar-filled glove box (the current and specific capacity can be calculated based on the mass loading of sulfur in the cathode).

[0046] In the above embodiments, the parts not described in detail are prior art. In this solution, small organic molecules are used to connect organic polymers to construct a molecular framework to provide ion channels for lithium ion transmission. The preparation method of the present invention has a wide range of raw materials and a simple preparation process. The prepared material has a high actual specific capacity for the positive electrode of a lithium-sulfur battery. The present invention uses widely available polyacrylonitrile and polyacrylic acid as raw materials, and then uses p-phenylenediamine, trithiocyanate, and 5-aminoisophthalic acid as organic small molecules to connect the polymer skeleton. Not only does it increase the sulfur content of the material and overcome the shuttling effect of polysulfides during the cycle, the carbon chain as a natural flexible skeleton can also adapt to the volume expansion of the sulfur positive electrode. The successful construction of the molecular framework can also provide a channel for the transmission of lithium ions and improve the rate performance.

[0047] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technician familiar with this profession can make some changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the technical solution of the present invention.

Claims

1. A method for preparing a sulfide polymer molecular framework composite material, characterized in that: The steps include: Step 1: dissolving a certain amount of organic polymer polyacrylonitrile or polyacrylic acid resin in a solvent and stirring the mixture to prepare an organic polymer precursor solution; Step 2: dissolving a certain amount of organic small molecules in a solvent, stirring by ultrasonic until completely dissolved, to prepare an organic small molecule precursor solution; Step 3: taking a certain amount of a mixture of carbon nanotubes and polyvinyl pyrrolidone and dissolving it in a solvent in proportion and then ultrasonically dispersing it; Step 4: Mix the solutions obtained in steps 1, 2 and 3, and stir them evenly to obtain a mixed solution; Step 5, adding sublimed sulfur and a catalyst to the mixed solution obtained in step 4, or adding sublimed sulfur to the mixed solution obtained in step 4; stirring and dispersing by ultrasonication to obtain a mixed solution; Step 6: Disperse the mixed solution obtained in step 5 in the salt template and keep it at 235-265° C. for a certain period of time under Ar atmosphere; Step 7, the product solution after the heat preservation in step 6 is fully washed in a detergent and separated and dried; Step 8: Grind the dried material from step 7 and diffuse it for a certain time under certain temperature conditions. After the diffusion is completed, the product is sieved to obtain a sulfide polymer molecular framework composite material.

2. The method for preparing the sulfide polymer molecular framework composite material according to claim 1, characterized in that: The mass ratio of the polyacrylonitrile in step 1 to the organic small molecule in step 2 is 1:1-2.

1.

3. The method for preparing the sulfide polymer molecular framework composite material according to claim 1, characterized in that: The mass ratio of the polyacrylic acid resin in step one to the organic small molecule in step two is 1:0.2-0.

65.

4. The method for preparing the sulfide polymer molecular framework composite material according to claim 1, characterized in that: In the step seven, the detergent is a mixed solution of water and anhydrous ethanol, wherein the volume ratio of water to anhydrous ethanol is 4:

1.

5. The method for preparing the sulfide polymer molecular framework composite material according to claim 1, characterized in that: In step seven, the drying conditions are as follows: the drying temperature range is 55-65° C. under vacuum conditions, and the drying time is 10-15 h.

6. The method for preparing the sulfide polymer molecular framework composite material according to claim 1, characterized in that: The steps include: Step 1: dissolving a certain amount of polyacrylonitrile in N,N-dimethylformamide and stirring evenly to prepare an organic polymer precursor solution; Step 2: dissolving a certain amount of p-phenylenediamine in N,N-dimethylformamide solution, stirring by ultrasonic until completely dissolved, for preparing an organic small molecule precursor solution; Step 3: Take a certain amount of a mixture of carbon nanotubes and polyvinyl pyrrolidone and dissolve it in N, N-dimethylformamide according to a certain proportion, and then disperse it by ultrasonic. Step 4: Mix the solutions obtained in steps 1, 2 and 3, and stir them evenly to obtain a mixed solution; Step 5, adding sublimed sulfur to the mixed solution obtained in step 4, and uniformly dispersing by ultrasonic stirring to obtain a mixed solution; Step 6: Disperse the mixed solution obtained in step 5 in the salt template and keep it warm at 235-265° C. for a certain period of time under Ar atmosphere; Step 7, the product solution after the heat preservation in step 6 is fully washed in a detergent and separated and dried; Step 8: Grind the dried material obtained in step 7 and diffuse it under a certain temperature for more than 12 hours. After the diffusion is completed, the product is sieved to obtain a sulfide polymer molecular framework composite material.

7. The method for preparing the sulfide polymer molecular framework composite material according to claim 1, characterized in that: The steps include: Step 1: dissolving a certain amount of organic polymer polyacrylic acid resin in a solvent and stirring the mixture evenly to prepare an organic polymer precursor solution; Step 2: dissolving a certain amount of 5-aminoisophthalic acid or trithiocyanate in a solvent, stirring with ultrasound until completely dissolved, and using it to prepare an organic small molecule precursor solution; Step 3: taking a certain amount of a mixture of carbon nanotubes and polyvinyl pyrrolidone and dissolving it in a solvent in proportion and then ultrasonically dispersing it; Step 4: Mix the solutions in steps 1, 2 and 3, and stir evenly to obtain a mixed solution; Step 5, adding sublimed sulfur and a catalyst to the mixed solution obtained in step 4; and uniformly dispersing by ultrasonic stirring to obtain a mixed solution; Step 6: Disperse the mixed solution obtained in step 5 in the salt template and keep it warm at 235-265° C. for a certain period of time under Ar atmosphere; Step 7, the product solution after the heat preservation in step 6 is fully washed in a detergent and separated and dried; Step 8: Grind the dried material obtained in step 7 and diffuse it under a certain temperature for more than 12 hours. After the diffusion is completed, the product is sieved to obtain a sulfide polymer molecular framework composite material.

8. The method for preparing the sulfide polymer molecular framework composite material according to claim 7, characterized in that: In the step 5, the catalyst includes potassium iodide, elemental iodine and iodophenyl diacetic acid.

9. Sulfur polymer molecular framework composite material, characterized in that: The sulfide polymer molecular framework composite material is a lamellar material; the sulfide polymer molecular framework composite material is prepared from an organic polymer and organic small molecules, wherein the organic polymer is polyacrylonitrile or polyacrylic acid resin, and the organic small molecules are used to connect the main structure of two organic polymer chains.

10. Use of the sulfide polymer molecular framework composite material according to claim 9 in preparing battery positive electrode materials.

Citation Information

Cited By

  • Composite sulfur positive electrode material and preparation method and application thereof

    CN119864402A