Negative electrode protection layer and preparation method thereof, negative electrode and battery
By applying a negative electrode protective layer on the negative electrode of the battery, the pore-carrying reactants of the filler react with dead lithium to prevent dendrites from penetration, the problems of dendrites and dead lithium are solved, the battery performance and safety are improved, and self-discharge is avoided , delaying capacity attenuation.
Patent Information
- Application Number
- CN202411405218.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-10
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In the field of battery energy storage, dendrite growth and dead lithium formation during negative electrode deposition lead to unstable battery cycles, which may cause safety hazards and reduce electrochemical performance. The existing methods inhibit dendrite and dead lithium while being difficult to avoid self-discharge while inhibiting self-discharge. .
The negative electrode protective layer is used, including the matrix, filler and reactants. The matrix is for lithium ions to pass through. The filler has pores to carry reactants. The reactants can react with dead lithium, block dendrites and reduce dead lithium deposition, and avoid reactants from The electrode contact causes self-discharge.
Effectively inhibit dendrites' growth and formation of dead lithium, improve battery performance, delay capacity attenuation, enhance safety, avoid self-discharge, and improve battery capacity retention rate.
Smart Images

Figure CN118919731A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of battery technology, and in particular to a negative electrode protective layer and a preparation method thereof, a negative electrode and a battery. Background Art
[0002] In the field of battery energy storage, dendrite growth and dead lithium formation during the deposition process of the negative electrode have always been bottlenecks that plague its development and application. Specifically, the growth of dendrites on the electrode surface can cause instability at the interface between the electrode and the electrolyte during the battery cycle, and may even pierce the diaphragm to cause a short circuit inside the battery, thereby causing a safety hazard. Dead lithium refers to some inactivated lithium that appears at the electrode. These inactivated lithiums do not participate in the charge and discharge reactions, which can lead to reduced electrochemical performance of the battery. In response to this problem, by adding substances that can react with negative electrode lithium dendrites and dead lithium to the battery system, such as directly using I2 as an electrolyte additive, dendrite growth and dead lithium formation can be suppressed to a certain extent. However, this solution can lead to severe self-discharge, making it difficult for the battery to be used normally. Therefore, how to effectively regulate the growth of dendrites and the formation of dead lithium while suppressing self-discharge is crucial for practical applications. In view of this, the present application is hereby proposed. Summary of the invention
[0003] The present application provides a negative electrode protective layer and a preparation method thereof, a negative electrode and a battery. The negative electrode protective layer can effectively inhibit the growth of dendrites to improve battery performance.
[0004] An embodiment of the present application provides a negative electrode protective layer, comprising: a substrate, configured to allow lithium ions to pass through; a filler, at least partially embedded in the substrate, and having pores inside the filler; a reactant, loaded in the pores of the filler, and the reactant can react with dead lithium.
[0005] In some embodiments of the present application, the filler includes a rigid inorganic material that does not react with dead lithium.
[0006] In some embodiments of the present application, the rigid inorganic material includes at least one of halloysite, attapulgite, sepiolite, zeolite, diatomaceous earth, montmorillonite, chrysotile, and palygorskite.
[0007] In some embodiments of the present application, the reactant includes at least one of a halogen-containing substance, an organic compound, and a halogen derivative of an organic compound.
[0008] In some embodiments of the present application, the halogen-containing substance includes at least one of a halogen element and a metal halide.
[0009] In some embodiments of the present application, the halogen element includes iodine element.
[0010] In some embodiments of the present application, the metal halide includes at least one of halides of Li, Mg, Al, Ti, Sr, and Sn.
[0011] In some embodiments of the present application, the organic compound includes at least one of ferrocene, 10-methylphenothiazine, thianthrene, and 2,2,6,6-tetramethylpiperidinyl oxide.
[0012] In some embodiments of the present application, the material of the matrix includes a lithium-philic material, so that lithium ions can pass through the matrix.
[0013] In some embodiments of the present application, the material of the matrix includes a polymer, an organic solvent and a lithium salt, wherein the polymer includes a lithium-philic organic polymer.
[0014] In some embodiments of the present application, the organic polymer includes at least one of polyethylene oxide, polyvinylidene fluoride, polyacrylic acid, polyacrylonitrile, and polymethyl methacrylate.
[0015] In some embodiments of the present application, the organic solvent includes at least one of acetonitrile, nitrogen methyl pyrrolidone, dimethyl carbonate, dimethylacetamide, ethylene carbonate, ethylene glycol methyl ether, and ethyl acetate.
[0016] In some embodiments of the present application, the lithium salt includes at least one of lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethylsulfonyl)imide, lithium bis(oxalatoborate), lithium difluorooxalatoborate, and lithium tetrafluoroborate.
[0017] In some embodiments of the present application, the molar ratio of the polymer to the lithium salt is (10-100):1.
[0018] In some embodiments of the present application, the thickness of the negative electrode protection layer is 0.1-5 μm.
[0019] In some embodiments of the present application, the median particle size of the particles constituting the negative electrode protection layer is less than 5 μm.
[0020] In some embodiments of the present application, the porosity of the negative electrode protection layer is >30%.
[0021] Another embodiment of the present application provides a method for preparing a negative electrode protective layer, comprising the following steps: performing a first mixing treatment on a filler and a reactant so that the reactant is loaded in the pores of the filler to obtain a loaded filler; preparing a matrix material; performing a second mixing treatment on the loaded filler and the matrix material to obtain a mixed slurry; and obtaining the negative electrode protective layer after coating and drying the mixed slurry.
[0022] In some embodiments of the present application, the first mixing treatment includes: dissolving the reactants in a first solvent to form a reactant solution, adding a filler for uniform treatment to obtain a loaded crude product; washing the loaded crude product to remove the reactants deposited on the surface of the filler to obtain a loaded filler.
[0023] In some embodiments of the present application, the first mixing treatment further includes: adding a second solvent after the uniform treatment until the reactant is precipitated and deposited on the surface or in the pores of the filler, and obtaining a loaded crude product through solid-liquid separation; wherein the solubility of the reactant in the first solvent is greater than the solubility in the second solvent.
[0024] In some embodiments of the present application, the uniform treatment includes ultrasonic dispersion and / or vacuum stirring.
[0025] In some embodiments of the present application, the vacuum stirring time is 20-40 minutes.
[0026] In some embodiments of the present application, the washing treatment includes washing the loaded crude product using the first solvent and the second solvent respectively.
[0027] In some embodiments of the present application, the first solvent includes anhydrous ethanol and / or acetone, and the second solvent includes water.
[0028] In some embodiments of the present application, the concentration of the reactant in the reactant solution is 0.01-0.5 mol / L.
[0029] In some embodiments of the present application, the amount of the filler added is 1-10 wt % of the reactant solution.
[0030] In some embodiments of the present application, the method for preparing the matrix material includes: dissolving a polymer in an organic solvent, and adding a lithium salt to mix to obtain the matrix material.
[0031] In some embodiments of the present application, in the second mixing process, the amount of the loaded filler is 0.5-10 wt % of the total mass of the polymer and the lithium salt.
[0032] Yet another embodiment of the present application provides a negative electrode, comprising a negative electrode current collector and any one of the negative electrode protection layers described above, wherein the negative electrode protection layer is disposed on the surface of the negative electrode current collector.
[0033] Yet another embodiment of the present application provides a battery, comprising the negative electrode described above.
[0034] According to the embodiment of the present application, the negative electrode protection layer provided includes a substrate, a filler and a reactant, wherein the substrate can be selected as a material through which lithium ions can pass smoothly, so that lithium ions can pass through the entire negative electrode protection layer via the substrate, thereby performing a normal charge and discharge reaction. The filler and the substrate are nested with each other, and the filler can be used to physically block the growth of dendrites to prevent dendrites from piercing the negative electrode protection layer and affecting battery performance. The reactant is selected as a substance that can react with dead lithium, so that if lithium dendrites and dead lithium are generated at the negative electrode, the effect of suppressing lithium dendrites and removing dead lithium can be achieved by reacting the reactant with lithium metal. In addition, the filler can also provide pores for accommodating reactants. When the reactant is placed in the pores, the filler itself can play an isolating role to avoid problems such as self-discharge caused by direct contact between the reactant and the negative electrode material or the negative electrode current collector. Therefore, the negative electrode protection layer provided in the embodiment of the present application loads the reactants in the filler, which can not only block the penetration of dendrites, but also react with dead lithium, reduce the deposition of dead lithium, remove dead lithium, and reduce the large-area contact between the reactants and the electrodes, avoiding the spontaneous reaction of the reactants with the electrodes and preventing the problem of battery self-discharge.
[0035] According to the method for preparing the negative electrode protective layer provided in the embodiment of the present application, before the base material is mixed with the filler and the reactant to prepare the negative electrode protective layer, the filler is first mixed with the reactant to prepare a loaded filler loaded with the reactant, so that as much reactant as possible can be loaded in the filler, so as to improve the effect of inhibiting dendrites and removing dead lithium. In addition, the prepared negative electrode protective layer loads the reactant in the filler, which can not only prevent dendrites from penetrating, but also react with dead lithium to reduce dead lithium deposition; at the same time, it can reduce the contact between the reactant and the electrode to avoid self-discharge.
[0036] According to the negative electrode provided in the embodiment of the present application, since a negative electrode protective layer is provided, the negative electrode can avoid the occurrence of dendrites and dead lithium, which is beneficial to improving the electrochemical performance of the negative electrode. At the same time, it can also avoid self-discharge and has good safety.
[0037] The battery provided according to the embodiment of the present application can reduce the generation of dendrites and dead lithium, thereby achieving the functions of improving the capacity retention rate of the battery, delaying capacity decay, etc., and can also avoid self-discharge and has better safety.
[0038] Additional technical solutions and advantages of the present application will be partially given in the following description, and partially become apparent from the following description, or be understood through the practice of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] In order to more clearly illustrate the specific implementation methods of the present application or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without paying any creative work.
[0040] Figure 1 A schematic diagram of the structure of a negative electrode protective layer and its coating on a negative electrode current collector provided in some embodiments of the present application.
[0041] Figure 2 Schematic diagram of the microstructure of a modified negative electrode sheet with a negative electrode protective layer on the surface provided in Example 1 of the present application.
[0042] Figure 3 This is a schematic diagram of the negative electrode protective layer obtained in Comparative Example 6 of the present application.
[0043] Among them, 100, substrate; 200, filler; 300, reactant; 400, negative electrode current collector. DETAILED DESCRIPTION
[0044] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values 1 and 2 are listed, and if the maximum range values 3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0045] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0046] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0047] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0048] If there is no special explanation, the "include" and "comprising" mentioned in this application represent open-ended or closed-ended expressions. For example, the "include" and "comprising" may represent that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0049] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0050] For battery systems based on lithium-based negative electrodes, if dendrites and dead lithium are generated during the negative electrode deposition process, it will not only lead to rapid loss of active lithium and serious side reactions causing electrolyte dryness, but also easily cause safety accidents. Therefore, it is crucial to regulate the growth of negative electrode dendrites.
[0051] Please refer to Figure 1 As shown, the embodiment of the present application provides a negative electrode protection layer, including a substrate 100, which is configured to allow lithium ions to pass through; a filler 200, which is at least partially embedded in the substrate 100, and has pores inside the filler 200; a reactant 300, which is loaded in the pores of the filler 200, and the reactant 300 can react with dead lithium. Exemplarily, the negative electrode protection layer provided in the embodiment of the present application can be used to be arranged on the surface of the negative electrode material or the negative electrode current collector 400, so as to effectively inhibit the growth of dendrites and the formation of dead lithium.
[0052] Specifically, the negative electrode protective layer includes a substrate 100, a filler 200 and a reactant 300, wherein the substrate 100 can be selected as a material through which lithium ions can pass smoothly, so that lithium ions can pass through the entire negative electrode protective layer via the substrate 100, thereby performing a normal charge and discharge reaction. The filler 200 and the substrate 100 are nested with each other, and the filler 200 can be used to physically block the growth of dendrites to prevent dendrites from piercing the negative electrode protective layer and affecting the battery performance. The reactant 300 is selected as a substance that can react with dead lithium, so that if lithium dendrites and dead lithium are generated at the negative electrode, the reactant 300 can be used to react with lithium metal to achieve the effect of inhibiting lithium dendrites and removing dead lithium. In addition, the filler 200 can also provide pores for accommodating the reactant 300. When the reactant 300 is placed in the pores, the filler 200 itself can play an isolating role to avoid the reactant 300 from directly contacting the negative electrode material or the negative electrode current collector 400 to cause self-discharge and other problems.
[0053] Therefore, the negative electrode protection layer provided in the embodiment of the present application loads the reactant 300 in the filler 200, which can not only block the penetration of dendrites, but also react with dead lithium, reduce the deposition of dead lithium, remove dead lithium, and reduce the large-area contact between the reactant 300 and the electrode, avoiding the spontaneous reaction of the reactant 300 with the electrode, and preventing the problem of battery self-discharge.
[0054] In order to further improve the performance of the negative electrode protection layer, the material selection of the filler 200 may be optimized.
[0055] In some embodiments, the filler 200 includes a rigid inorganic material that does not react with dead lithium. Since the filler 200 and the substrate 100 are nested with each other, there is a certain probability that the filler 200 contacts the electrode. Therefore, in order to avoid serious self-discharge of the battery, the filler 200 is preferably a material that does not react with dead lithium. In particular, the filler 200 is more preferably a rigid inorganic material, wherein a rigid inorganic material refers to an inorganic material that has little or no deformation under force, and the use of a rigid inorganic material with higher strength is more conducive to preventing dendrite growth.
[0056] Further, in some embodiments, the rigid inorganic material includes at least one of halloysite, attapulgite, sepiolite, zeolite, diatomite, montmorillonite, chrysotile, and palygorskite. The selected material has sufficient internal pores, which is conducive to increasing the loading amount of the reactant 300 in the filler 200, while effectively avoiding the contact between the reactant 300 and the electrode; and the selected material has a high structural strength, which can effectively block the growth of dendrites, thereby minimizing the penetration of dendrites through the negative electrode protective layer.
[0057] Since the reactant 300 can directly react with the dead lithium to remove the dead lithium, the selection of the type of the reactant 300 is also crucial.
[0058] In some embodiments, the reactant 300 includes at least one of a halogen-containing substance, an organic compound, and a halogen derivative of an organic compound. In this case, the reactant 300 can fully undergo an oxidation-reduction reaction with the dead lithium, remove the dead lithium, and avoid the formation of dead lithium, which leads to battery capacity decay and shortened cycle life.
[0059] Exemplarily, in some embodiments, the halogen-containing substance includes at least one of a halogen element and a metal halide; in some embodiments, the halogen element includes an iodine element; in some embodiments, the metal halide includes at least one of a halide of Li, Mg, Al, Ti, Sr, and Sn, for example, the metal halide may be at least one of LiI, MgI2, AlI3, TiI4, SrI2, and SnI4; in particular, when the reactant 300 includes an iodine element, the chemical reaction that occurs at this time includes: 2Li + I2→ 2LiI. In some embodiments, the organic compound includes at least one of ferrocene, 10-methylphenothiazine, thianthracene, and 2,2,6,6-tetramethylpiperidinyl oxide. Selecting the above-mentioned suitable reactant 300 so that its redox potential is within the battery charge and discharge window (such as 3-4.3V) can more fully remove dead lithium and further avoid the influence of dead lithium on battery performance.
[0060] It should also be noted that the type of material of the substrate 100 will also affect the performance of the negative electrode protective layer. In some embodiments, the material of the substrate 100 includes a lithium-philic material so that lithium ions can pass through the substrate 100. Among them, the lithium-philic material refers to a material that can easily interact with lithium ions, and in this embodiment, it refers to a material that can allow lithium ions to pass through. The selection of a lithium-philic material allows lithium ions to pass through the negative electrode protective layer smoothly, which is conducive to the normal progress of the charge and discharge reaction.
[0061] In some embodiments, the material of the matrix 100 includes a polymer, an organic solvent, and a lithium salt, wherein the polymer includes a lithium-philic organic polymer.
[0062] Exemplarily, in some embodiments, the organic polymer includes at least one of polyethylene oxide (PEO), polyvinylidene fluoride (PVDF), polyacrylic acid (PAA), polyacrylonitrile (PAN), and polymethyl methacrylate (PMMA). In some embodiments, the organic solvent includes at least one of acetonitrile, nitrogen methyl pyrrolidone (NMP), dimethyl carbonate (DMC), dimethylacetamide (DMAC), ethylene carbonate (EC), ethylene glycol methyl ether (EMC), and ethyl acetate (EA). In some embodiments, the lithium salt includes at least one of lithium hexafluorophosphate (LiPF6), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethylsulfonyl)imide (LiTFSI), lithium bis(oxalatoborate) (LiBOB), lithium difluorooxalatoborate (LiDFOB), and lithium tetrafluoroborate (LiBF4). By selecting the above-mentioned suitable matrix 100 material, the influence of the negative electrode protective layer on the lithium ion transmission rate can be reduced, which is conducive to ensuring the battery performance.
[0063] Specifically, the organic solvent included in the matrix 100 of the embodiment of the present application is mainly used as a medium to mix the polymer with the lithium salt and the filler 200 loaded with reactants evenly, so as to facilitate the preparation of the negative electrode protective layer. The role of the lithium salt is mainly to provide enough lithium ions inside the polymer to increase the internal ion migration rate, that is, the ion conductivity. If the lithium salt is not added, the ion conductivity of the negative electrode protective layer will be very poor. Therefore, the matrix 100 can at least play the following three roles: 1. As an adhesive for inorganic fillers, it can be stably adhered to the negative electrode; 2. As an ion-conducting medium, lithium ions are quickly transported inside; 3. The polymer can also prevent substances that react with dead lithium, such as I2, from entering the electrolyte, resulting in self-discharge. In fact, substances that react with lithium will be connected to the dangling bonds above (such as the ether bonds of PEO and the F bonds of PVDF) in the part in contact with the polymer, and slowly diffuse to the surroundings, which can also prevent them from entering the electrolyte.
[0064] In some embodiments, the molar ratio of the polymer to the lithium salt is (10-100): 1. For example, the molar ratio of the polymer to the lithium salt can be 10: 1, 20: 1, 30: 1, 40: 1, 50: 1, 60: 1, 70: 1, 80: 1, 90: 1, 100: 1 or any value between (10-100): 1. Thus, by doping the matrix 100 with an appropriate amount of lithium salt, it is beneficial to further improve the lithium ion transfer rate, thereby improving the battery performance.
[0065] In addition, the thickness of the negative electrode protective layer will also affect its application effect. In some embodiments, the thickness of the negative electrode protective layer is 0.1-5μm. For example, the thickness of the negative electrode protective layer can be 0.1μm, 0.2μm, 0.5μm, 1μm, 1.5μm, 2μm, 2.5μm, 3μm, 3.5μm, 4μm, 4.5μm, 5μm or any value between 0.1-5μm. If the thickness of the negative electrode protective layer is too large, it will affect the lithium ion transmission effect and reduce the battery performance, and it will also take up space and cause the battery size to be larger and more expensive; if the thickness of the negative electrode protective layer is too small, the inhibitory effect on dendrites and dead lithium is insufficient. In the embodiment of the present application, the thickness of the negative electrode protective layer is controlled within the above-mentioned appropriate range, which can not only effectively inhibit the growth of dendrites and the formation of dead lithium, but also try to avoid the influence on the lithium ion transmission effect, and can effectively provide the comprehensive performance of the battery when used in the battery.
[0066] In some embodiments, the median particle size of the particles constituting the negative electrode protection layer is less than 5 μm, wherein the median particle size can be obtained by counting the particles in the SEM image of the negative electrode protection layer using software such as ImageJ.
[0067] In some embodiments, the porosity of the negative electrode protective layer is >30%. Wherein, the porosity refers to the percentage of the pore volume in the negative electrode protective layer to the total volume of the negative electrode protective layer in the natural state. Specifically, the porosity can be obtained by nitrogen adsorption and desorption (gas replacement method) test, or it can also be obtained by drainage method (applicable to macropores). Exemplarily, in some embodiments, the steps of testing the porosity by nitrogen adsorption and desorption are as follows: first, the negative electrode protective layer sample is heated and degassed under vacuum conditions to remove the gas adsorbed on the surface of the sample. After the sample is cooled to room temperature, helium is backfilled and the sample weight is weighed. The sample tube is installed on the analysis station and a nitrogen adsorption and desorption test is performed at a temperature of 77K. The pore size distribution and pore volume are obtained by BJH (Barrett-Joyner-Halenda) analysis. The instrument model used is: Micromeritics ASAP2020.
[0068] Another embodiment of the present application provides a method for preparing a negative electrode protective layer, comprising the following steps: performing a first mixing treatment on a filler 200 and a reactant 300 so that the reactant 300 is loaded in the pores of the filler 200 to obtain a loaded filler 200; preparing a matrix 100 material; performing a second mixing treatment on the loaded filler 200 and the matrix 100 material to obtain a mixed slurry; and obtaining a negative electrode protective layer after coating and drying the mixed slurry.
[0069] According to the preparation method provided in the embodiment of the present application, before the matrix 100 material is mixed with the filler 200 and the reactant 300 to prepare the negative electrode protection layer, the filler 200 is first mixed with the reactant 300 to prepare the loaded filler 200 loaded with the reactant 300, so that the filler 200 can be loaded with as much reactant 300 as possible, so as to improve the effect of removing dead lithium. In addition, the prepared negative electrode protection layer loads the reactant 300 in the filler 200, which can not only prevent dendrite penetration, but also react with dead lithium to reduce dead lithium deposition; at the same time, it can reduce the contact between the reactant 300 and the electrode to avoid self-discharge.
[0070] It should be noted that when the negative electrode protective layer is used in a battery, the mixed slurry in the above step can be directly coated on the surface of the negative electrode material or the negative electrode current collector 400, and then dried to obtain an electrode with a negative electrode protective layer. For example, the mixed slurry can be fully stirred and dispersed, and then coated on the surface of the negative electrode material or the negative electrode current collector 400, and the solvent is fully volatilized at room temperature, and then vacuum dried at 30-50°C to obtain a surface-modified negative electrode sheet.
[0071] In some embodiments, the first mixing process for preparing the loaded filler 200 includes: dissolving the reactant 300 in the first solvent to form a reactant 300 solution, adding the filler 200 for uniform treatment, and obtaining a loaded crude product through solid-liquid separation; illustratively, in this article, the means of solid-liquid separation may include filtration, centrifugation, etc. Then, the loaded crude product is washed to remove the reactant 300 deposited on the surface of the filler 200, and the loaded filler 200 is obtained.
[0072] In some embodiments, the first mixing treatment also includes: adding a second solvent after uniform treatment until the reactant 300 is precipitated and deposited on the surface or in the pores of the filler 200, and obtaining a loaded crude product through solid-liquid separation; wherein the solubility of the reactant 300 in the first solvent is greater than that in the second solvent.
[0073] In this embodiment, since the solubility of the reactant 300 in the first solvent is greater than that in the second solvent, when the reactant 300 is dissolved in the first solvent, the reactant 300 can be dissolved as much as possible in the reactant 300 solution. After the filler 200 is added, the filler 200 can be fully contacted with the sufficient reactant 300 contained in the reactant 300 solution, especially the reactant 300 can be filled into the pores of the filler 200. Then the second solvent is added, and the reactant 300 is placed in the solvent formed by the mixture of the first solvent and the second solvent. Since the solubility of the reactant 300 in the second solvent is low, the solubility of the reactant 300 in the mixed solvent is low, so that the reactant 300 will precipitate from the solvent in a solid form and deposit on the surface and pores of the filler 200. Then the reactant 300 deposited on the surface of the filler 200 is washed and removed, and the loaded filler 200 that only loads the reactant 300 in the internal pores of the filler 200 can be obtained. Therefore, the reactant 300 can be effectively loaded in the internal pores of the filler 200 in the above manner, so as to facilitate the coordination of the reactant 300 and the filler 200 to achieve the effect of inhibiting the growth of dendrites and the generation of dead lithium.
[0074] It should be understood that the main purpose of removing the reactant 300 on the surface of the filler 200 in the above step is to avoid the self-discharge problem caused by the reactant 300 on the surface of the filler 200 contacting the electrode.
[0075] It can be seen from the above that the selection of the types of the first solvent and the second solvent has a significant impact on the loading effect of the filler 200 .
[0076] Exemplarily, in some embodiments, the first solvent includes anhydrous ethanol, and the second solvent includes water such as deionized water. Since anhydrous ethanol and water can be mutually soluble in any proportion, the first solvent and the second solvent have good compatibility at this time. Thus, in the process of gradually adding the second solvent to the first solvent, the second solvent can be quickly mixed with the first solvent, so as to facilitate the reactants 300 everywhere in the mixed solvent to be precipitated and deposited on different parts of the filler 200, thereby improving the uniformity of the deposition of the reactants 300 in the filler 200, and then helping to improve the reaction efficiency of the reactants 300 in the filler 200 with dead lithium. In addition, the amount of the second solvent added to the first solvent can also be arbitrarily controlled, so as to facilitate the solubility of the reactants 300 in the mixed solvent, so as to control the reactants 300 to be as completely precipitated as possible and deposited in the filler 200, thereby improving the reactant 300 loading of the filler 200.
[0077] In some embodiments, the concentration of reactant 300 in the reactant 300 solution is 0.01-0.5 mol / L. If the concentration of reactant 300 is too high, it will exceed the upper limit of the loading amount of filler 200, which is easy to cause waste; if the concentration of reactant 300 is too low, the loading amount of filler 200 is insufficient, and it is difficult to achieve the expected effect of the negative electrode protective layer. In this embodiment, by controlling the appropriate concentration of reactant 300, it can not only avoid the problem of waste of reactant 300, but also make the filler 200 load as much reactant 300 as possible, which is conducive to improving the performance of the negative electrode protective layer.
[0078] In some embodiments of the present application, the amount of filler 200 added is 1-10wt% of the solution of reactant 300. For example, the amount of filler 200 added can be 1wt%, 2wt%, 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt% or any value between 1-10wt% of the solution of reactant 300.
[0079] In some embodiments, the uniform treatment includes ultrasonic dispersion and / or vacuum stirring, which can fully mix the filler 200 and the reactant 300 solution, thereby facilitating controlling the reactant 300 in the reactant 300 solution to be fully deposited in the pores of the filler 200 in the subsequent steps.
[0080] Illustratively, the uniform treatment may include: firstly ultrasonically dispersing, and then vacuuming and continuing stirring, which can further improve the mixing effect.
[0081] In some embodiments, the vacuum stirring time is 20-40 minutes; for example, the vacuum stirring time can be 20 minutes, 22 minutes, 25 minutes, 28 minutes, 30 minutes, 32 minutes, 35 minutes, 38 minutes, 40 minutes or any value between 20 minutes and 40 minutes. Within the above appropriate time range, it is conducive to more complete mixing.
[0082] In order to fully remove the reactants 300 deposited on the surface of the filler 200, in some embodiments, the washing process includes washing the loaded crude product with a first solvent and a second solvent, respectively. Since the reactants 300 deposited in the pores of the filler 200 are difficult to wash away, while the reactants 300 deposited on the surface of the filler 200 are easier to wash away, all reactants 300 deposited on the surface of the filler 200 can be basically removed by washing with the first solvent. At this time, only a small part of the reactants 300 deposited in the pores of the filler 200 is lost, which will not have much impact on the performance of the negative electrode protective layer. Then, washing with the second solvent can remove the residual first solvent and avoid excessive dissolution of the reactants 300 deposited in the pores of the filler 200 into the first solvent to cause losses.
[0083] For example, the loaded crude product can be washed with anhydrous ethanol and deionized water respectively to remove the reactants 300 deposited on the surface of the inorganic filler 200, and then dried at 30-50°C to obtain the loaded filler 200 with the reactants 300 loaded therein.
[0084] In some embodiments, the preparation method of the matrix 100 material includes: dissolving a polymer in an organic solvent, and adding a lithium salt to mix to obtain the matrix 100 material; wherein the matrix 100 material refers to a material formed by mixing raw materials required to form the matrix 100.
[0085] For example, a certain amount of polymer may be dissolved in an organic solvent first, and then lithium salt may be added, and the molar ratio of lithium salt to polymer may be controlled to be 1:10-100, and the matrix 100 material may be obtained after sufficient stirring.
[0086] In some embodiments, in the second mixing process, the amount of the load filler 200 is 0.5-10wt% of the total mass of the polymer and the lithium salt. If the amount of the load filler 200 is too much, after the negative electrode protective layer is formed, the load filler 200 will block the transmission of lithium ions, resulting in a reduction in the efficiency of lithium ion transmission and affecting battery performance; if the amount of the load filler 200 is too little, the load filler 200 has poor inhibitory effect on dendrites and cleaning effect on dead lithium. In this embodiment, by controlling the amount of the load filler 200, the lithium ion transmission rate and the inhibitory effect on dendrites and dead lithium can be well balanced, which has good practicality.
[0087] Another embodiment of the present application provides a negative electrode, comprising a negative electrode current collector and a negative electrode protection layer of any of the above embodiments, wherein the negative electrode protection layer is disposed on the surface of the negative electrode current collector 400. Figure 1 As shown, the negative electrode protection layer can be stacked with the negative electrode current collector 400. For example, the negative electrode current collector 400 can be copper foil, aluminum foil, composite current collector, etc. For example, the negative electrode can also include a lithium metal negative electrode material, and the negative electrode protection layer is arranged on the surface of the negative electrode material or the negative electrode current collector 400 that contacts the electrolyte to play a protective role.
[0088] The negative electrode protection layer includes a substrate 100 and a filler 200 loaded with a reactant 300 that can react with dead lithium, which can not only prevent dendrites from penetrating, but also achieve the effect of removing dead lithium. In addition, since the reactant 300 is loaded in the filler 200, it will not spontaneously react with the negative electrode material and / or the negative electrode current collector 400, and can avoid causing serious self-discharge problems. Therefore, due to the provision of the negative electrode protection layer, the negative electrode can avoid the occurrence of dendrites and dead lithium, which is beneficial to improving the electrochemical performance of the negative electrode, and can also avoid self-discharge, and has good safety.
[0089] Another embodiment of the present application provides a battery, comprising the negative electrode of the above embodiment. Exemplarily, the battery assembly method comprises: assembling the positive electrode, the separator, and the negative electrode of the above embodiment into a battery. Among them, the positive electrode material can be a ternary positive electrode (NCM), lithium cobalt oxide (LCO), lithium iron phosphate (LFP), lithium nickel manganese oxide (LNMO), lithium-rich manganese-based material (LMR), etc. The separator can be a PP or PE separator. The negative electrode is a modified negative electrode provided in an embodiment of the present application. The electrolyte can be an ether electrolyte, for example, the molar ratio of LiFSI:DME:TTE is 1:1.2:3.
[0090] The battery of this embodiment can reduce the generation of dendrites and dead lithium, thereby achieving the functions of improving the capacity retention rate of the battery, delaying capacity decay, etc., and can also avoid self-discharge, and has better safety.
[0091] The following examples describe the disclosure of the present application in more detail, and these examples are merely illustrative, as it will be apparent to those skilled in the art that various modifications and variations are made within the scope of the disclosure of the present application. Unless otherwise stated, all reagents and raw materials used in the following examples are commercially available or synthesized according to conventional methods, and the instruments used in the examples are commercially available.
[0092] Example 1 This embodiment provides a negative electrode protective layer and a preparation method thereof, and a negative electrode, comprising the following steps: I2 was dissolved in anhydrous ethanol to prepare a 0.1 mol / L reactant solution, and then halloysite was added as a filler in an amount of 5 wt% of the mass of the reactant solution. After ultrasonication for 30 minutes, vacuum stirring was continued for 30 minutes, and then deionized water was added to the solution until I2 was completely separated and deposited in the filler. The solution was filtered and rinsed with anhydrous ethanol and deionized water respectively to remove I2 deposited on the surface of the filler, and dried at 40°C to obtain a halloysite-loaded filler loaded with I2.
[0093] The PEO polymer was dissolved in an acetonitrile solvent, and lithium salt LiTFSI was added, with the molar ratio of the lithium salt to the polymer being 1:20, and the matrix material was obtained by fully stirring.
[0094] A certain amount of the above-mentioned halloysite-loaded filler is added to the matrix material, the amount of which is 5wt% of the mass of the lithium salt and the polymer, and after being fully stirred and dispersed, it is coated on the surface of an 8μm copper foil with a coating thickness of 1μm. The solvent is fully evaporated at room temperature, and then vacuum dried at 40°C to obtain a modified negative electrode sheet with a negative electrode protective layer on the surface, with a median particle size of ~0.5μm and a porosity of 36%. Figure 2 shown.
[0095] This embodiment also provides a battery. The battery assembly includes: weighing NCM811, conductive carbon, and PVDF according to a mass ratio of 96.5:2:1.5 and mixing them evenly, adding NMP to fully homogenize to prepare a uniform slurry, and coating it on aluminum foil with a coating amount of 20 mg / cm 2 , after drying, roller pressing treatment, compaction density 3.0g / cm 3 , a positive electrode sheet with a flat surface was obtained; the negative electrode used the modified negative electrode sheet with a negative electrode protective layer on the surface; the separator used a PE double-sided coated ceramic separator (12μm+2μm+2μm); the electrolyte was an ether electrolyte, and the molar ratio of LiFSI:DME:TTE was 1:1.2:3. Then the positive electrode sheet, the negative electrode sheet and the separator were assembled, and then the electrolyte was added, and the battery was left to stand at 45°C for 24h and the performance of the obtained battery was tested. The test results are shown in Table 1 below.
[0096] Example 2 The difference between this embodiment and embodiment 1 is that I2 is dissolved in anhydrous ethanol to prepare a 0.01 mol / L reactant solution, and the remaining steps are the same as those of embodiment 1. The coating thickness is 1 μm, the median particle size is ~0.5 μm, and the porosity is 38%.
[0097] Example 3 The difference between this embodiment and embodiment 1 is that I2 is dissolved in anhydrous ethanol to prepare a 0.5 mol / L reactant solution, and the remaining steps are the same as those of embodiment 1. The coating thickness is 1 μm, the median particle size is ~0.5 μm, and the porosity is 35%.
[0098] Example 4 The difference between this embodiment and embodiment 1 is that a certain amount of the above-mentioned halloysite-loaded filler is added to the base material, and the added amount is 0.5wt% of the mass of the lithium salt and the polymer, and the remaining steps are the same as those of embodiment 1. The coating thickness is 1μm, the median particle size is ~0.5μm, and the porosity is 31%.
[0099] Example 5 The difference between this embodiment and embodiment 1 is that a certain amount of the above-mentioned halloysite-loaded filler is added to the base material, and the added amount is 10wt% of the mass of the lithium salt and the polymer, and the remaining steps are the same as those of embodiment 1. The coating thickness is 1μm, the median particle size is ~0.5μm, and the porosity is 44%.
[0100] Example 6 The difference between this embodiment and embodiment 1 is that I2 is replaced by ferrocene, including: dissolving ferrocene in acetone to prepare a 0.1 mol / L reactant solution, then adding halloysite as a filler, the addition amount is 5wt% of the mass of the reactant solution, after ultrasonication for 30 minutes, vacuuming and stirring for 30 minutes, filtering, and washing with acetone to remove ferrocene deposited on the surface of the filler, drying at 40°C to obtain a ferrocene-loaded halloysite filler, and the rest is the same as embodiment 1. The coating thickness is 1μm, the median particle size is ~0.5μm, and the porosity is 35%.
[0101] Example 7 The difference between this embodiment and embodiment 1 is that I2 is replaced by 10-methylphenothiazine, including: dissolving 10-methylphenothiazine in acetone to prepare a 0.1 mol / L reactant solution, then adding halloysite as a filler in an amount of 5wt% of the mass of the reactant solution, ultrasonicating for 30 minutes, vacuuming and stirring for 30 minutes, filtering, rinsing with acetone to remove 10-methylphenothiazine deposited on the surface of the filler, drying at 40°C, and obtaining a halloysite-loaded filler loaded with 10-methylphenothiazine, and the rest is the same as embodiment 1. The coating thickness is 1μm, the median particle size is ~0.5μm, and the porosity is 35%.
[0102] Example 8 The difference between this embodiment and embodiment 1 is that the halloysite is replaced by attapulgite of equal mass, and the rest is the same as embodiment 1. The coating thickness is 1 μm, the median particle size is ~1 μm, and the porosity is 33%.
[0103] Example 9 The difference between this embodiment and embodiment 1 is that the halloysite is replaced by sepiolite of equal mass, and the rest is the same as embodiment 1. The coating thickness is 1 μm, the median particle size is ~2 μm, and the porosity is 38%.
[0104] Comparative Example 1 The difference between this comparative example and Example 1 is that I2 is not added to the negative electrode protective layer. The coating thickness is 1 μm, the median particle size is ~0.5 μm, and the porosity is 37%.
[0105] Comparative Example 2 The difference between this comparative example and Example 1 is that halloysite is not added to the negative electrode protective layer, that is, a certain amount of I2 is directly added to the base material, and the added amount is 5wt% of the mass of the lithium salt and the polymer. The coating thickness is 1μm, there are no obvious particles, and the porosity is 3%.
[0106] Comparative Example 3 The difference between this comparative example and Example 1 is that I2 is dissolved in anhydrous ethanol to prepare a 0.005 mol / L reactant solution. The coating thickness is 1 μm, the median particle size is ~0.5 μm, and the porosity is 35%.
[0107] Comparative Example 4 The difference between this comparative example and Example 1 is that I2 is dissolved in anhydrous ethanol to prepare a 1 mol / L reactant solution. The coating thickness is 1 μm, the median particle size is ~0.5 μm, and the porosity is 36%.
[0108] Comparative Example 5 The difference between this comparative example and Example 1 is that a certain amount of the above-mentioned halloysite-loaded filler is added to the base material, and the added amount is 0.1wt% of the mass of the lithium salt and the polymer. The coating thickness is 1μm, the median particle size is ~0.5μm, and the porosity is 18%.
[0109] Comparative Example 6 The difference between this comparative example and Example 1 is that a certain amount of the above-mentioned halloysite-loaded filler is added to the base material, and the added amount is 20wt% of the mass of the lithium salt and the polymer. The coating thickness is 1μm, the median particle size is ~0.5μm, and the porosity is 53%.
[0110] Table 1. Electrochemical performance of batteries corresponding to each embodiment and comparative example
[0111] Among them, battery capacity recovery rate = the amount of electric energy that can be released after charging / battery initial capacity × 100%.
[0112] Table 1 compares the electrochemical properties of Examples 1-9 and Comparative Examples 1-6. It can be seen that Examples 1-9 all show similar performance. Compared with Comparative Example 1 in which I2 is not added, the capacity retention rate after 50 cycles is increased from less than 60% to more than 87%, which is similar to Comparative Example 2 in which only I2 is added. This shows that I2 in the protective layer can react with dead lithium, so that the lithium that has lost its activity and is difficult to be reused and solidified in the dead lithium is converted back into lithium ions that can be transported between the positive and negative electrodes, playing the role of activating dead lithium, thereby delaying capacity decay. From the perspective of capacity retention after full charge and standing, the capacity recovery rate of Comparative Example 1 without I2 is 95.2%, while that of Comparative Example 2 with only I2 added is only 76.6%. This is because I2 contacts the negative pole with a large area, which causes it to spontaneously react with the deposited lithium, resulting in severe self-discharge. Although the capacity retention rate in Examples 1-9 is lower than that in Comparative Example 1, it is much higher than that in Comparative Example 2, indicating that the scheme in the present invention can effectively inhibit the spontaneous reaction of I2 with the negative pole and inhibit self-discharge. In terms of capacity recovery rate, Comparative Example 1 is 99.3%, and the capacity is basically fully recovered, while Examples 1-9 and Comparative Example 2 both reach more than 100% (the main reason is that the substances reacting with lithium release and activate some inactive lithium components, namely dead lithium, so the capacity recovery will be higher than 100%), indicating that although I2 will cause self-discharge, it has little effect on the subsequent cycle of the battery, and even helps to recover the capacity. In Comparative Example 3, due to the reduction of I2 concentration, the load of I2 in the halloysite is reduced, and the capacity retention rate after 50 cycles of Comparative Example 1 is reduced, and the capacity retention rate after full charge and standing is improved. The electrochemical performance of Comparative Example 4 is not much different from that of Example 1, but in the actual operation process, I2 cannot be completely dissolved in ethanol, which will lead to the problem of insufficient utilization of experimental materials. Comparative Example 5 reduces the halloysite content, and the I2 content it carries is correspondingly reduced, so the capacity retention rate after 50 cycles is reduced, but the capacity retention rate after full charge and standing is improved. In Comparative Example 6, the content of halloysite is increased, and the content of organic components is relatively low, and the organic components play a bonding role, resulting in poor flexibility and adhesion. Figure 3 As shown, the negative electrode protective layer obtained in Comparative Example 6 is easily detached.
[0113] The various technical features described above can be combined arbitrarily. Although all possible combinations of these technical features are not described, any combination of these technical features should be considered to be covered by this specification as long as there is no contradiction in such combination.
[0114] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.
Claims
1. A negative electrode protective layer, It is characterized in that include: A substrate configured to allow lithium ions to pass through; A filler, at least partially embedded in the matrix, and having pores inside the filler; A reactant is loaded in the pores of the filler, and the reactant can react with dead lithium.
2. The negative electrode protective layer according to claim 1, It is characterized in that The filler includes a rigid inorganic material that does not react with dead lithium; Optionally, the rigid inorganic material includes at least one of halloysite, attapulgite, sepiolite, zeolite, diatomaceous earth, montmorillonite, chrysotile, and palygorskite.
3. The negative electrode protective layer according to claim 1, It is characterized in that The reactant includes at least one of a halogen-containing substance, an organic compound, and a halogen derivative of an organic compound; Optionally, the halogen-containing substance includes at least one of a halogen element and a metal halide; Optionally, the halogen element comprises iodine element; Optionally, the metal halide includes at least one of halides of Li, Mg, Al, Ti, Sr, and Sn; Optionally, the organic compound includes at least one of ferrocene, 10-methylphenothiazine, thianthrene, and 2,2,6,6-tetramethylpiperidinyl oxide.
4. The negative electrode protective layer according to claim 1, It is characterized in that The material of the matrix includes a lithium-philic material so that lithium ions can pass through the matrix; Optionally, the material of the matrix includes a polymer, an organic solvent and a lithium salt, wherein the polymer includes a lithium-philic organic polymer; Optionally, the organic polymer includes at least one of polyethylene oxide, polyvinylidene fluoride, polyacrylic acid, polyacrylonitrile, and polymethyl methacrylate; Optionally, the organic solvent includes at least one of acetonitrile, nitrogen methyl pyrrolidone, dimethyl carbonate, dimethylacetamide, ethylene carbonate, ethylene glycol methyl ether, and ethyl acetate; Optionally, the lithium salt includes at least one of lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethylsulfonyl)imide, lithium bis(oxalatoborate), lithium difluorooxalatoborate, and lithium tetrafluoroborate; Optionally, the molar ratio of the polymer to the lithium salt is (10-100):
1.
5. The negative electrode protective layer according to claim 1, It is characterized in that The thickness of the negative electrode protective layer is 0.1-5 μm; and / or The median particle size of the particles constituting the negative electrode protective layer is less than 5 μm; and / or The porosity of the negative electrode protection layer is greater than 30%.
6. A method for preparing a negative electrode protective layer, It is characterized in that The following steps are involved: Performing a first mixing process on the filler and the reactant so that the reactant is loaded in the pores of the filler to obtain a loaded filler; Formulating matrix materials; Performing a second mixing process on the loaded filler and the matrix material to obtain a mixed slurry; The negative electrode protective layer is obtained after the mixed slurry is coated and dried.
7. The method for preparing the negative electrode protective layer according to claim 6, It is characterized in that The first mixing treatment includes: dissolving the reactant in a first solvent to form a reactant solution, adding a filler to perform a uniform treatment to obtain a loaded crude product; washing the loaded crude product to remove the reactant deposited on the surface of the filler to obtain a loaded filler; Optionally, the first mixing treatment further comprises: adding a second solvent after the uniform treatment until the reactant is precipitated and deposited on the surface or in the pores of the filler, and obtaining a loaded crude product through solid-liquid separation; wherein the solubility of the reactant in the first solvent is greater than that in the second solvent; Optionally, the uniform treatment includes ultrasonic dispersion and / or vacuum stirring; Optionally, the vacuum stirring time is 20-40 minutes; Optionally, the washing treatment comprises washing the loaded crude product using the first solvent and the second solvent respectively; Optionally, the first solvent includes anhydrous ethanol and / or acetone, and the second solvent includes water; Optionally, the reactant concentration in the reactant solution is 0.01-0.5 mol / L; Optionally, the filler is added in an amount of 1-10 wt % of the reactant solution.
8. The method for preparing the negative electrode protective layer according to claim 6, It is characterized in that The preparation method of the matrix material comprises: dissolving a polymer into an organic solvent, and adding a lithium salt to mix to obtain the matrix material; Optionally, in the second mixing process, the amount of the loaded filler is 0.5-10 wt % of the total mass of the polymer and the lithium salt.
9. A negative electrode, It is characterized in that It comprises a negative electrode current collector and a negative electrode protective layer prepared by the preparation method of the negative electrode protective layer according to any one of claims 1 to 5 or the negative electrode protective layer according to any one of claims 6 to 8, wherein the negative electrode protective layer is arranged on the surface of the negative electrode current collector.
10. A battery, It is characterized in that Comprising the negative electrode as claimed in claim 9.
Citation Information
Patent Citations
Metal lithium negative electrode for lithium battery and lithium battery
CN111224068A
Lithium metal negative electrode, preparation method thereof and related lithium metal battery and device
CN114530589A
Ceramic coating and application thereof in lithium ion battery diaphragm
CN118523037A
Anode for lithium secondary battery, and manufacturing method therefor
WO2023177204A1
KR20190068065A