Electrolyte and application
By using phosphate compounds containing halogenated phosphate, cyano and isocyano in the electrolyte, a stable electrode interface layer is formed, which solves the problems of structural instability and interface degradation of the battery under high temperature conditions, and significantly improves the The battery has high temperature cycling and storage performance and enhances safety.
Patent Information
- Application Number
- CN202411191590.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-08
AI Technical Summary
During the charging and discharging process of high voltage ternary positive electrode and silicon-based negative electrode, there are problems such as structural instability, large volume changes, and interface degradation, resulting in safety problems such as electrolyte decomposition, loss of active substances and thermal runaway in the battery under high temperature conditions, which affects the Its cycle performance and storage performance.
Use phosphate compounds containing halogenated phosphate, cyano and/or isocyano as electrolyte components to form stable LiF and Li3PO4-enriched SEI layer and CEI layer to inhibit electrolyte decomposition and interface reaction, and enhance battery High temperature cycle and storage performance.
Effectively suppress the high-temperature gas production of batteries under high-voltage and high temperature conditions, improve the high-temperature circulation performance, high-temperature storage performance and safety performance of batteries, extend the cycle life of the battery, and prevent the increase of the acidity and chromaticity of the electrolyte.
Smart Images

Figure BDA0005015256600000011 
Figure BDA0005015256600000021 
Figure BDA0005015256600000031
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of secondary batteries, in particular to an electrolyte and its application. Background Art
[0002] In the preparation of batteries, although high-voltage ternary positive electrodes and silicon-based negative electrodes have the advantages of high energy density, they still have problems such as structural instability, large volume changes, and interface degradation during the charging and discharging process. These problems are more serious under high temperature conditions, which can lead to safety issues such as electrolyte decomposition, active material loss, and thermal runaway. As a result, the prepared batteries have poor high-temperature cycle performance, poor high-temperature storage performance, and poor safety performance. Summary of the invention
[0003] Based on this, it is necessary to provide an electrolyte and application to address the above problems. When the electrolyte is applied to a battery, the battery can have excellent high-temperature cycle performance, high-temperature storage performance and safety performance.
[0004] An electrolyte comprises a solute and a non-aqueous solvent, and also comprises a phosphate compound, wherein the structural formula of the phosphate compound is as shown in formula (1):
[0005]
[0006] In formula (1), R 1 , R 2 , R 3 , R 4 are independently selected from cyano, isocyano, C1-C20 alkyl, C1-C20 haloalkyl, C6-C26 aryl, C6-C26 haloaryl or C6-C26 alkoxy, and R 1 , R 2 , R 3 , R 4 At least one of A is selected from cyano or isocyano; 1 , A 2 are independently selected from hydrogen, halogen, C1-C20 alkyl, C1-C20 haloalkyl, C6-C26 aryl or C6-C26 haloaryl, and A 1 and A 2 At least one of M is selected from halogen; M is selected from at least one of Li, Na or K.
[0007] In one embodiment, A 1 and A 2 At least one of them is selected from fluorine atoms, R 1 , R 2 , R 3 , R 4 At least one of the groups is selected from cyano, and at least one of the groups is selected from isocyano.
[0008] In one embodiment, the cyano group accounts for 1 / 6-1 / 2 of the terminal groups in the phosphate compound, the isocyano group accounts for 1 / 6-1 / 2 of the terminal groups in the phosphate compound, and the fluorine atom accounts for 1 / 6-1 / 3 of the terminal groups in the phosphate compound.
[0009] In one embodiment, the phosphate compound is selected from any one of the compounds having the structures shown in formula (2) to formula (8),
[0010]
[0011]
[0012] In one embodiment, the phosphate compound is selected from any one of the compounds having the structures shown in formula (9) to formula (15),
[0013]
[0014] In one of the embodiments, the mass fraction of the phosphate compound in the electrolyte is 0.05%-2.5%.
[0015] In one embodiment, the solute is selected from electrolyte lithium salt, and the mass fraction of the electrolyte lithium salt in the electrolyte is 10%-19%.
[0016] In one embodiment, the non-aqueous solvent is selected from carbonate and / or acetate.
[0017] In one embodiment, the electrolyte further includes an additive, the mass fraction of the additive in the electrolyte is 0.5%-5%, and the additive is selected from at least one of vinyl sulfate, tris(trimethylsilyl) phosphate, tris(trimethylsilyl) borate, lithium difluorooxalatoborate, vinylene carbonate, vinyl ethylene carbonate, fluoroethylene carbonate, and 1,3-propane sultone.
[0018] A secondary battery comprising the electrolyte as described above.
[0019] A vehicle using the secondary battery as described above.
[0020] In the electrolyte of the present invention, a phosphate compound containing a halogenated phosphate, a cyano group and / or an isocyano group is used, wherein the halogenated phosphate (such as a fluorophosphate) can form a stable LiF, Li 3 PO 4Enriched SEI layer, reduce battery impedance, improve battery cycle performance and high temperature performance; cyano group can promote the formation of a stable CEI layer on the surface of the high-voltage ternary positive electrode, and by forming a strong coordination with the transition metal, inhibit the dissolution of transition metal ions and enhance the thermal stability of the positive electrode; isocyano group can effectively remove water and acid, slow down the decomposition and consumption of the electrolyte, reduce gas production, form a stable interface film on the electrode surface, improve interface properties, and enhance the cycle life of the battery. Therefore, when the electrolyte of the present invention is applied to the battery, it can effectively suppress the high-temperature gas production phenomenon that occurs when the battery is under high-pressure and high-temperature conditions for a long time, so that the battery has excellent high-temperature cycle performance, high-temperature storage performance and safety performance.
[0021] In addition, when the electrolyte contains unstable additives (such as vinyl sulfate), the phosphate compound with a specific structure of the present invention can also effectively inhibit the increase of the acidity and chromaticity of the electrolyte. DETAILED DESCRIPTION
[0022] For ease of understanding of the present invention, the present invention will be described in more detail below. However, it should be understood that the present invention can be implemented in many different forms and is not limited to the embodiments or examples described herein. On the contrary, the purpose of providing these embodiments or examples is to make the understanding of the disclosure of the present invention more thorough and comprehensive.
[0023] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific implementation methods or embodiments, and are not intended to limit the present invention. The optional scope of the term "and / or" used herein includes any one of two or more related listed items, and also includes any and all combinations of related listed items, and the combinations include any two related listed items, any more related listed items, or all related listed items.
[0024] The electrolyte provided in the present application includes a solute and a non-aqueous solvent, and also includes a phosphate compound, the structural formula of the phosphate compound is shown in formula (1):
[0025]
[0026] In formula (1), R 1 , R 2 , R 3 , R 4 are independently selected from cyano, isocyano, C1-C20 alkyl, C1-C20 haloalkyl, C6-C26 aryl, C6-C26 haloaryl or C6-C26 alkoxy, and R 1 , R2 , R 3 , R 4 At least one of A is selected from cyano or isocyano; 1 , A 2 are independently selected from hydrogen, halogen, C1-C20 alkyl, C1-C20 haloalkyl, C6-C26 aryl or C6-C26 haloaryl, and A 1 and A 2 At least one of M is selected from halogen; M is selected from at least one of Li, Na or K.
[0027] In the electrolyte of the present invention, a phosphate compound containing a halogenated phosphate, a cyano group and / or an isocyano group is used, wherein the halogenated phosphate (such as a fluorophosphate) can form a stable LiF, Li 3 PO 4 Enriched SEI layer, reduce battery impedance, improve battery cycle performance and high temperature performance; cyano group can promote the formation of a stable CEI layer on the surface of the high-voltage ternary positive electrode, and by forming a strong coordination with the transition metal, inhibit the dissolution of transition metal ions and enhance the thermal stability of the positive electrode; isocyano group can effectively remove water and acid, slow down the decomposition and consumption of the electrolyte, reduce gas production, form a stable interface film on the electrode surface, improve interface properties, and enhance the cycle life of the battery. Therefore, when the electrolyte of the present invention is applied to the battery, it can effectively suppress the high-temperature gas production phenomenon that occurs when the battery is under high-pressure and high-temperature conditions for a long time, so that the battery has excellent high-temperature cycle performance, high-temperature storage performance and safety performance.
[0028] In addition, isocyanate can react with trace amounts of water in the electrolyte, inhibiting the generation of LiPF 6 hydrolysis reaction to avoid the production of PF 5 Therefore, when the electrolyte contains unstable additives (such as vinyl sulfate), the phosphate compound with a specific structure of the present invention can also effectively inhibit the increase of the acidity and chromaticity of the electrolyte.
[0029] It can be understood that in the present invention, according to R 1 , R 2 , R 3 , R 4 , A 1 and A 2 The performance of phosphate compounds, the performance of electrolytes, and thus the performance of batteries can be regulated by different substituents.
[0030] In the present invention, the halogen is selected from any one of a fluorine atom, a chlorine atom, a bromine atom and an iodine atom, and is preferably a fluorine atom.
[0031] In the present invention, the halogen in the C1-C20 haloalkyl group and the C6-C26 haloaryl group is selected from at least one of a fluorine atom, a chlorine atom, a bromine atom or an iodine atom, and is preferably a fluorine atom.
[0032] Optionally, A 1 and A 2 At least one of them is selected from fluorine atoms, R 1 , R 2 , R 3 , R 4 In the above, at least one is selected from cyano and at least one is selected from isocyano. In this way, the phosphate compound structure contains cyano, isocyano and fluorophosphate at the same time. Under the synergistic effect of the three, the high temperature cycle performance, high temperature storage performance and safety performance of the electrolyte can be further improved.
[0033] Furthermore, when the phosphate compound structure contains cyano, isocyano and fluorophosphate at the same time, the cyano accounts for 1 / 6-1 / 2 of the terminal groups in the phosphate compound, the isocyano accounts for 1 / 6-1 / 2 of the terminal groups in the phosphate compound, and the fluorine atom accounts for 1 / 6-1 / 3 of the terminal groups in the phosphate compound. By setting it in this way, by controlling the content of the three, the synergistic effect of the three can be fully exerted, and the comprehensive performance of the battery can be better improved.
[0034] It should be noted that in the present invention, the ratio of cyano, isocyano and fluorine atoms to the terminal groups in the phosphate compound is the number of cyano, isocyano and fluorine atoms to the terminal group R in the phosphate compound. 1 , R 2 , R 3 , R 4 , A 1 and A 2 ratio of the total number of .
[0035] Optionally, the phosphate compound is selected from any one of the compounds having the structures shown in formula (2) to formula (8),
[0036]
[0037] In the present invention, M in the compounds having the structures shown in the above formulae (2) to (8) is preferably Li.
[0038] Optionally, the phosphate compound is selected from any one of the compounds having the structures shown in formula (9) to formula (15),
[0039]
[0040] Optionally, the mass fraction of the phosphate compound in the electrolyte is 0.05%-2.5%, preferably 0.2%-1.5%. In this way, by controlling the content of the phosphate compound, when the electrolyte is applied to the battery, it can better form stable CEI and SEI films at the positive and negative electrodes, inhibit the side reaction between the positive electrode and the electrolyte, optimize the water-acid environment, prevent gas generation, and inhibit the increase of interface resistance, thereby further improving the cycle performance and thermal stability of the battery.
[0041] It should be noted that the preparation method of the phosphate compound in the present invention can refer to the following steps: reacting a silane compound containing a cyanide group, a compound containing an isocyanate and a catalyst to obtain an intermediate product, then dissolving the intermediate product and the M source in an organic solvent, followed by toluene precipitation to obtain a phosphate compound as shown in formula (1), wherein the M source is selected from a sodium salt, a lithium salt or a potassium salt, the catalyst is preferably oxalyl chloride, and the organic solvent is preferably acetonitrile.
[0042] For example, trimethylsilyl cyanide, methyl-2,4-diisocyanate and oxalyl chloride are reacted to obtain an intermediate product, and then the intermediate product and LiPF 6 The product is dissolved in acetonitrile and then precipitated with toluene to obtain a phosphate compound as shown in formula (13).
[0043] In the present invention, in the electrolyte, the selection of the solute type is adjusted according to the selection of the specific type of M ions in the phosphate compound. For example, when the M ions in the phosphate compound are potassium ions, the solute is potassium salt, and the electrolyte is used for potassium ion batteries; when the M ions in the phosphate compound are sodium ions, the solute is sodium salt, and the electrolyte is used for sodium ion batteries; when the M ions in the phosphate compound are lithium ions, the solute is lithium salt, and the electrolyte is used for lithium ion batteries.
[0044] The solute in the present invention is selected from electrolyte lithium salt, and the mass fraction of the electrolyte lithium salt in the electrolyte is 10%-19%, preferably 10%-18.75%.
[0045] Furthermore, the electrolyte lithium salt is selected from at least one of lithium hexafluorophosphate, lithium bis(oxalatoborate), lithium bis(fluorosulfonyl imide) and lithium bis(trifluoromethylsulfonyl imide).
[0046] Optionally, the non-aqueous solvent is selected from carbonates and / or acetates, preferably carbonates and acetates, wherein the carbonate is selected from at least one of ethylene carbonate, propylene carbonate, diethyl carbonate or ethyl methyl carbonate, and the acetate is selected from ethyl acetate and / or propyl acetate.
[0047] Optionally, the electrolyte further includes an additive, the mass fraction of the additive in the electrolyte is 0.5%-5%, and the additive is selected from at least one of vinyl sulfate, tris(trimethylsilyl) phosphate, tris(trimethylsilyl) borate, lithium difluorooxalatoborate, vinylene carbonate, vinyl ethylene carbonate, fluoroethylene carbonate, and 1,3-propane sultone. Such an arrangement can synergize with phosphate compounds to further improve the cycle stability of the battery.
[0048] In one embodiment, the method for preparing the electrolyte of the present invention comprises the following steps:
[0049] S1, purifying the non-aqueous solvent to remove impurities and water;
[0050] S2, adding the solute to the solvent obtained in step S1 at room temperature and stirring evenly;
[0051] S3, adding a phosphate compound and stirring evenly to obtain an electrolyte.
[0052] In step S1, purification, impurity removal and water removal are preferably carried out by treating with at least one of molecular sieves, activated carbon, calcium hydride, lithium hydride, anhydrous calcium oxide, calcium chloride, phosphorus pentoxide, alkali metals or alkaline earth metals.
[0053] Optionally, in step S3, an additive is also added.
[0054] Meanwhile, the present invention also provides a secondary battery comprising the electrolyte as described above.
[0055] In one embodiment, the secondary battery may be a lithium ion battery, a sodium ion battery or a potassium ion battery.
[0056] Specifically, when the electrolyte of the present invention is applied to a lithium-ion battery, the lithium secondary battery includes a positive electrode sheet, a negative electrode sheet and the electrolyte described above, wherein the positive electrode sheet includes a positive electrode active material that embeds or de-embeds lithium ions, a conductive agent, a current collector, and a binder that combines the positive electrode active material and the conductive agent with the current collector; the negative electrode sheet includes a negative electrode active material that can embed or de-embed lithium ions, a conductive agent, a current collector, and a binder that combines the negative electrode active material and the conductive agent with the current collector.
[0057] In addition, the present invention also provides a vehicle using the secondary battery as described above.
[0058] The electrolyte and its application will be further described below by the following specific examples. However, it will be understood by those skilled in the art that the following examples are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. If no specific conditions are specified in the examples, the conditions are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be obtained commercially.
[0059] It should be noted that the structural formulas of the phosphate compounds in the embodiments and comparative examples of the present invention are respectively shown in the following formulas (9) to (17):
[0060]
[0061]
[0062] Example 1
[0063] Cyclic carbonate solvent ethylene carbonate (EC) and linear carbonate solvent ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) were mixed in a mass ratio of 3:5:2, and purified by molecular sieve to remove impurities and water to obtain a mixed solvent. Then, conductive lithium hexafluorophosphate (LiPF) was added to the mixed solvent at room temperature. 6 ), a phosphate compound having a structure as shown in formula (9) and vinyl sulfate, and stirred evenly to obtain an electrolyte, wherein the mass fraction of lithium hexafluorophosphate in the electrolyte is 12.5%, the mass fraction of the phosphate compound in the electrolyte is 0.8%, and the mass fraction of vinyl sulfate in the electrolyte is 1.5%.
[0064] Example 2
[0065] The difference between Example 2 and Example 1 is that the phosphate compound with the structure shown in formula (10) is used, and the other conditions are the same to obtain an electrolyte.
[0066] Example 3
[0067] The only difference between Example 3 and Example 1 is that a phosphate compound having a structure as shown in formula (11) is used, and the other conditions are the same to obtain an electrolyte.
[0068] Example 4
[0069] The only difference between Example 4 and Example 1 is that a phosphate compound having a structure as shown in formula (12) is used, and the other conditions are the same to obtain an electrolyte.
[0070] Example 5
[0071] The only difference between Example 5 and Example 1 is that a phosphate compound having a structure as shown in formula (13) is used, and the other conditions are the same to obtain an electrolyte.
[0072] Example 6
[0073] The only difference between Example 6 and Example 1 is that a phosphate compound having a structure as shown in formula (14) is used, and the other conditions are the same to obtain an electrolyte.
[0074] Example 7
[0075] The only difference between Example 7 and Example 1 is that a phosphate compound having a structure as shown in formula (15) is used, and the other conditions are the same to obtain an electrolyte.
[0076] Example 8
[0077] The only difference between Example 8 and Example 1 is that the mass fraction of lithium hexafluorophosphate in the electrolyte is 10%, the mass fraction of the phosphate compound in the electrolyte is 0.05%, and the mass fraction of vinyl sulfate in the electrolyte is 0.5%. The other conditions are the same, and an electrolyte is obtained.
[0078] Example 9
[0079] The only difference between Example 9 and Example 1 is that the mass fraction of lithium hexafluorophosphate in the electrolyte is 18.75%, the mass fraction of the phosphate compound in the electrolyte is 2.5%, the mass fraction of vinyl sulfate in the electrolyte is 5%, and the other conditions are the same to obtain an electrolyte.
[0080] Example 10
[0081] Compared with Example 1, Example 10 differs only in that the mass fraction of the phosphate compound in the electrolyte is 3%, and the other conditions are the same to obtain an electrolyte.
[0082] Embodiment 11
[0083] The only difference between Example 11 and Example 1 is that lithium bis(fluorosulfonyl)imide is used instead of lithium hexafluorophosphate, and 1,3-propane sultone is used instead of vinyl sulfate. The other conditions are the same to obtain an electrolyte.
[0084] Example 12
[0085] The only difference between Example 12 and Example 1 is that lithium bis(oxalatoborate) and lithium hexafluorophosphate are used as lithium salts, wherein the mass fraction of lithium bis(oxalatoborate) in the electrolyte is 2.5%, and the mass fraction of lithium hexafluorophosphate is 10%; tri(trimethylsilyl) phosphate is used instead of vinyl sulfate, and other conditions are the same to obtain an electrolyte.
[0086] Embodiment 13
[0087] The only difference between Example 13 and Example 1 is that vinyl sulfate is not added, and the other conditions are the same to obtain an electrolyte.
[0088] Comparative Example 1
[0089] The only difference between Comparative Example 1 and Example 1 is that a phosphate compound having a structure as shown in formula (16) is used, and the other conditions are the same to obtain an electrolyte.
[0090] Comparative Example 2
[0091] The only difference between Comparative Example 2 and Example 1 is that a phosphate compound having a structure as shown in formula (17) is used, and the other conditions are the same to obtain an electrolyte.
[0092] Comparative Example 3
[0093] Compared with Example 1, Comparative Example 3 differs only in that no phosphate compound is added, and other conditions are the same to obtain an electrolyte.
[0094] Comparative Example 4
[0095] The only difference between Comparative Example 4 and Example 12 is that no phosphate compound is added, and the other conditions are the same to obtain an electrolyte.
[0096] The electrolytes of Examples 1-13 and Comparative Examples 1-4 were divided into three parts respectively, wherein one part of the electrolytes of Examples 1-13 and Comparative Examples 1-4 was used to prepare LiNi 0.6 Co 0.2 Mn 0.2 O 2 / graphite silicon soft package battery, and then the corresponding battery was cycled in a high temperature environment of 45°C, the charge and discharge cycle performance was tested at a 1C rate, and the high temperature storage performance was tested at a high temperature environment of 60°C for 14 days, as follows:
[0097] LiNi 0.6 Co 0.2 Mn 0.2 O 2 Preparation method of graphite silicon soft package battery: First, 96wt% LiNi 0.6 Co 0.2 Mn 0.2 O 2 (NCM622), 1wt% polyvinylidene fluoride (PVDF), and 3wt% conductive carbon black (SP) are prepared into a solid solute, and then 30wt% N-methylpyrrolidone (NMP) and 70wt% solid solute are uniformly mixed, and the mixture is coated on a current collector aluminum foil, dried, and rolled to obtain LiNi0.6 Co 0.2 Mn 0.2 O 2 positive electrode sheet; secondly, 94wt% artificial graphite, 3% silicon oxide, 0.5wt% single-walled carbon nanotubes, 1wt% carboxymethyl cellulose (CMC), 0.5wt% styrene-butadiene rubber (SBR), and 1wt% acrylic resin (PAA) are prepared into a solid solute, and then 45wt% water and 55wt% solid solute are uniformly mixed, and the mixture is coated on a current collector copper foil, dried, and rolled to obtain a graphite silicon negative electrode sheet; then a separator is placed between the positive and negative electrode sheets, and a LiNi 0.6 Co 0.2 Mn 0.2 O 2 / Graphite silicon soft pack battery cell.
[0098] Battery high temperature storage experiment: The corresponding battery obtained above was subjected to 5 charge and discharge cycle tests at room temperature at a charge and discharge rate of 1C, and finally charged to full power at a rate of 1C. The 1C capacity Q, battery internal resistance T 0 and battery thickness H 0 The fully charged battery was stored at 60°C for 14 days and the 1C discharge capacity Q was recorded. 1 、Battery internal resistance T 1 and thickness H 1 Then charge and discharge the battery at room temperature at a rate of 1C for 5 weeks, and select the one with the highest discharge capacity as the discharge capacity Q 2 , the experimental data of battery high temperature storage capacity retention rate, capacity recovery rate, thickness change rate, internal resistance change rate, etc. are calculated, and the results are recorded as shown in Table 1 and Table 2; Among them, internal resistance change rate (%) = (T 1 -T 0 ) / T 0 ×100; thickness change rate (%) = (H 1 -H 0 ) / H 0 ×100; Capacity retention rate (%) = Q 1 / Q×100; Capacity recovery rate (%) = Q 2 / Q×100.
[0099] Table 1
[0100]
[0101] It can be seen from the data in Table 1 that, compared with Comparative Examples 1-4, after adding phosphate compounds containing fluorophosphate, cyano and / or isocyano in the structure in the embodiments of the present invention, the 45°C high-temperature cycle capacity retention rate is significantly improved, and after 14 days of high-temperature storage at 60°C, the capacity retention and recovery rate are effectively improved, especially in Example 5, where the phosphate compound structure contains fluorophosphate, cyano and isocyano at the same time, and the effect is more obvious through the synergistic effect between the three.
[0102] Table 2
[0103]
[0104] As shown in Table 2, compared with Comparative Examples 1-4, after adding phosphate compounds containing fluorophosphate, cyano and / or isocyano groups in the structure in the embodiments of the present invention, the expansion rate and internal resistance change rate of the battery are significantly reduced after being stored at 60°C for 14 days. Therefore, in the present invention, by adding phosphate compounds containing a specific structure, the impedance of the battery cell can be effectively reduced, and the high-temperature gas generation phenomenon that occurs when the battery is under high-voltage and high-temperature conditions for a long time can be effectively suppressed.
[0105] At the same time, the remaining two electrolytes corresponding to Examples 1-13 and Comparative Examples 1-4 were stored at room temperature and at a high temperature of 45°C, respectively, and the acidity and chromaticity of the electrolytes stored for 7 days, 15 days, 30 days, and 60 days were tested respectively; the instrument for the acidity test was a potentiometric titrator, the acidity test method was a triethylamine potentiometric titration method, and the chromaticity was tested using a colorimeter; the chromaticity recording results are shown in Table 3; the acidity recording results are shown in Table 4.
[0106] Table 3
[0107]
[0108] As can be seen from Table 3, it is not difficult to find from the results of room temperature storage and 45°C high temperature storage that after adding phosphate compounds containing fluorophosphate, cyano and / or isocyano in the structure in the embodiments of the present invention, the increase in the chromaticity of the electrolyte can be effectively suppressed, especially when containing additives such as vinyl sulfate that are likely to increase the chromaticity of the electrolyte, it can play a significant inhibitory role.
[0109] Table 4
[0110]
[0111] As can be seen from Table 4, the results of room temperature storage and 45°C high temperature storage show that the addition of phosphate compounds containing fluorophosphate, cyano and / or isocyano groups in the structure in the embodiments of the present invention can effectively inhibit the increase in electrolyte acidity; especially when containing additives such as vinyl sulfate, tris(trimethylsilyl) phosphate, tris(trimethylsilyl) borate that are prone to increase the acidity of the electrolyte, it can play a significant inhibitory role.
[0112] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0113] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. An electrolyte comprising a solute and a non-aqueous solvent, It is characterized in that Also included are phosphate compounds, the structural formula of the phosphate compound is as shown in formula (1): In formula (1), R 1 , R 2 , R 3 , R 4 are independently selected from cyano, isocyano, C1-C20 alkyl, C1-C20 haloalkyl, C6-C26 aryl, C6-C26 haloaryl or C6-C26 alkoxy, and R 1 , R 2 , R 3 , R 4 At least one of A is selected from cyano or isocyano; 1 , A 2 are independently selected from hydrogen, halogen, C1-C20 alkyl, C1-C20 haloalkyl, C6-C26 aryl or C6-C26 haloaryl, and A 1 and A 2 At least one of M is selected from halogen; M is selected from at least one of Li, Na or K.
2. The electrolyte according to claim 1, It is characterized in that A 1 and A 2 At least one of them is selected from fluorine atoms, R 1 , R 2 , R 3 , R 4 At least one of the groups is selected from cyano, and at least one of the groups is selected from isocyano.
3. The electrolyte according to claim 2, It is characterized in that The cyano group accounts for 1 / 6-1 / 2 of the terminal groups in the phosphate compound, the isocyano group accounts for 1 / 6-1 / 2 of the terminal groups in the phosphate compound, and the fluorine atom accounts for 1 / 6-1 / 3 of the terminal groups in the phosphate compound.
4. The electrolyte according to claim 1, It is characterized in that The phosphate compound is selected from any one of the compounds having the structures shown in formula (2) to formula (8), 5. The electrolyte according to claim 4, It is characterized in that The phosphate compound is selected from any one of the compounds having the structures shown in formula (9) to formula (15), 6. The electrolyte according to claim 1, It is characterized in that The mass fraction of the phosphate compound in the electrolyte is 0.05%-2.5%.
7. The electrolyte according to claim 1, It is characterized in that The solute is selected from electrolyte lithium salt, and the mass fraction of the electrolyte lithium salt in the electrolyte is 10%-19%.
8. The electrolyte according to claim 1, It is characterized in that The non-aqueous solvent is selected from carbonates and / or acetates.
9. The electrolyte according to any one of claims 1 to 8, It is characterized in that The electrolyte also includes an additive, the mass fraction of the additive in the electrolyte is 0.5%-5%, and the additive is selected from at least one of vinyl sulfate, tri(trimethylsilyl) phosphate, tri(trimethylsilyl) borate, lithium difluorooxalatoborate, vinylene carbonate, vinyl ethylene carbonate, fluoroethylene carbonate, and 1,3-propane sultone.
10. A secondary battery comprising the electrolyte according to any one of claims 1 to 9.
11. A vehicle using the secondary battery according to claim 10.