Nitrogen-substituted dicyclooctane quaternary ammonium salt lithium battery non-aqueous electrolyte additive and application thereof

By using nitrogen to replace bicyclooctane quaternary ammonium salt compounds as electrolyte additives in lithium-ion batteries, a solid electrolyte membrane is formed, which solves the problem of unstable lithium-ion batteries under high voltage and improves the cycle stability and resistance of the batteries High temperature reduces costs.

CN118919846APending Publication Date: 2024-11-08HUZHOU UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410965761.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing lithium-ion batteries are unstable at high voltages, resulting in intensified electrolyte decomposition, increased side reactions on the electrode surface, decreased circulation performance, and even safety accidents. It is necessary to develop high voltage and long-life electrolytes.

Method used

Nitrogen is used to replace bicyclooctane quaternary ammonium salt compounds as the nonaqueous electrolyte additive of lithium batteries to form a dense solid electrolyte membrane, inhibiting the contact reaction between the electrode and the electrolyte, and improving the cycle stability of the battery at high pressure, normal temperature and high temperature.

Benefits of technology

By forming a dense protective film, the electrolyte decomposition and electrode corrosion are reduced, the cycle stability of the battery is improved, and the cost of additives is reduced, and the lithium ion conduction ability and better high temperature resistance are achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919846A_ABST
    Figure CN118919846A_ABST
Patent Text Reader

Abstract

The invention relates to the field of lithium batteries, and discloses a nitrogen-substituted dicyclooctane quaternary ammonium salt lithium battery non-aqueous electrolyte additive and application thereof. The structure of the nitrogen-substituted dicyclooctane quaternary ammonium salt compound contains a nitrogen-substituted dicyclooctane quaternary ammonium salt cation and one or more organic anions; wherein the nitrogen-substituted dicyclooctane quaternary ammonium salt cation contains one or two nitrogen atoms, and hydrogen on the nitrogen is partially or completely substituted to form tertiary amine or quaternary ammonium. When the nitrogen-substituted dicyclooctane quaternary ammonium salt compound is used as a lithium battery non-aqueous electrolyte additive, a more compact and stable solid electrolyte membrane can be formed on the surface of an electrode, so that the cycling stability of the battery at high pressure, normal temperature and high temperature can be better improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of lithium batteries, and in particular to a nitrogen-substituted bicyclooctane quaternary ammonium salt lithium battery non-aqueous electrolyte additive and application thereof. Background Art

[0002] As promoting the development of new energy industry has become a social consensus, lithium-ion secondary batteries, mainly lithium-ion batteries, have become the primary candidates for energy storage and conversion devices due to their significant advantages such as high energy density, high power density, long cycle life and green environmental protection. However, with the continuous upgrading of electrical equipment, ordinary lithium-ion batteries can no longer meet the current needs of life and production, and are in urgent need of development in the direction of higher energy density, longer service life and higher safety performance. Although the energy density can be greatly improved by increasing the cut-off voltage of the battery, the system is unstable under high voltage, resulting in aggravated decomposition of the electrolyte, increased side reactions between decomposition products and electrode surfaces, decreased battery cycle performance, and even safety accidents. Therefore, it is necessary to develop high-voltage and long-life electrolytes.

[0003] At present, there are two main ideas for developing high-voltage electrolytes. One is to use organic molecules with low highest occupied molecular orbital (HOMO) energy levels substituted with strong electron-withdrawing groups such as fluorine and cyanide as solvents for electrolytes, thereby improving the oxidation resistance of the electrolyte. The other is to introduce electrolyte film-forming additives that can form a stable, low-impedance, uniform, high-ionic conductivity, and electronically insulating solid electrolyte film on the electrode surface, thereby preventing the electrolyte material from undergoing further electrochemical reactions on the electrode surface. Compared with the first method of using high-voltage resistant solvents, the second method has become the preferred solution for major theoretical research and practical applications due to its advantages such as small amount of additives, obvious effects, low cost, large selectivity, small impact on battery preparation process, and ease of industrialization.

[0004] According to the different chemical structures of the film-forming additives, they can be divided into carbonates / carbonyl esters, carboxylates, sulfonates, sulfuric acid / sulfites, anhydrides, nitriles, ethers, sulfones, borates, phosphates / phosphites, and salts. Among them, salt additives include salts whose cations are metal ions, and organic salts whose anions and cations are both organic ions. For example, the invention patent CN117613392B discloses a fluorinated complex lithium salt with a branched long-chain fluoroester structure, which can form a fluorine-containing protective layer on the graphite surface, and the complexed lithium ions are easy to decomplex and participate in the cycle during charging and discharging, and some lithium ions also cooperate with graphite in the gaps of the protective layer substrate to form a dense fluorine-containing composite protective layer, thereby greatly improving the cycle stability of the battery. It has been reported that organic salt compounds whose anions and cations are both organic ions are used as additives in electrodes. For example, invention patent CN105518916B discloses a compound whose anion is a five-membered ring and whose cation is a quaternary ammonium or imidazolium ion. When the compound is used as an additive in the preparation of the positive electrode, the ionic conductivity of the electrode can be significantly improved, thereby effectively improving the rate performance of the battery. However, organic salts whose anions and cations are both organic ions have not been reported to be used in electrolytes.

[0005] In summary, in order to solve the current technical problem of unstable high-voltage charging and discharging of lithium-ion batteries, it is urgent to systematically develop electrolyte organic salt additives with novel structures that can form a more solid electrode surface to form a stable solid electrolyte film, and apply them to batteries. Summary of the invention

[0006] In order to solve the above technical problems, the present invention provides a nitrogen-substituted bicyclooctane quaternary ammonium salt lithium battery non-aqueous electrolyte additive and its application. When the nitrogen-substituted bicyclooctane quaternary ammonium salt compound of the present invention is used as a lithium battery non-aqueous electrolyte additive, a more compact and stable solid electrolyte film can be formed on the electrode surface, thereby better improving the cycle stability of the battery under high pressure, normal temperature and high temperature.

[0007] The specific technical scheme of the present invention is: In the first aspect, the present invention provides a nitrogen-substituted bicyclooctane quaternary ammonium salt lithium battery non-aqueous electrolyte additive, the chemical structure of which is shown below: in: R1, R2, R3, R4, R5, R6 and R7 are selected from a linear or branched saturated hydrocarbon group having 1 to 4 carbon atoms, or a saturated hydrocarbon group in which all or part of the hydrogen atoms are replaced by halogen elements; The functional groups X and Y are selected from fluorine atoms, or linear or branched saturated hydrocarbon groups having 1 to 4 carbon atoms, saturated hydrocarbon groups containing oxygen atoms, saturated hydrocarbon groups in which all or part of the hydrogen atoms are replaced by halogen elements, saturated hydrocarbon groups in which all or part of the hydrogen atoms are replaced by halogen elements and containing oxygen atoms, and unsaturated hydrocarbon groups containing double bonds or triple bonds; G- is a fluorine-containing organic anion selected from tetrafluoroborate ([BF4] - ), trifluoromethanesulfonate ([SO3CF3] - ), fluorosulfonate ([SO3F] - ), hexafluorophosphate ([PF6] - ), bis(fluorosulfonyl)imide ([N(SO2F)2] - ), difluorophosphate ([PO2F2] - ), difluorooxalatoborate ([BF2(C2O4)] - ) and bis(oxalatoborate) ([B(C2O4)2] - ).

[0008] The structural characteristics of the nitrogen-substituted bicyclooctane quaternary ammonium salt compounds selected by the present invention are: the structure contains a nitrogen-substituted bicyclooctane quaternary ammonium salt cation and one or more organic anions; wherein the nitrogen-substituted bicyclooctane quaternary ammonium salt cation contains one or two nitrogens, and the hydrogen on the nitrogen is partially or completely replaced to form a tertiary amine (R1R2NR3) or a quaternary ammonium (R1R2NR3). + R3R4); fluorinated organic anions (G - ) including tetrafluoroborate (BF4 - ), hexafluorophosphate (PF6 - ), bis(fluorosulfonyl)imide ([N(SO2F)2] - ), difluorophosphate (PO2F2 - ), difluorooxalatoborate (BF2(C2O4) - ) and bis(oxalatoborate) (B(C2O4)2 - ) at least one of.

[0009] The present invention has found through research that when the compound having the above structural characteristics is used as a non-aqueous electrolyte additive for lithium batteries, a denser protective film (solid electrolyte membrane) can be formed on the electrode surface compared with conventional electrolyte additives, thereby better inhibiting the contact reaction between the electrode and the electrolyte, reducing electrolyte decomposition and corrosion of the electrode surface; at the same time, due to the high content of nitrogen-containing substances in such compounds, their solubility in organic electrolytes is lower, their high temperature resistance is better, and they have the characteristics of high lithium ion conductivity, etc.; under the combined effect of the above characteristics, the cycle stability of the battery under high pressure, room temperature and high temperature can be better improved.

[0010] In addition, unlike conventional lithium-ion complex organic anion salts, the anions and cations of the compounds of the present invention are all organic ions and do not contain lithium ions. This can not only significantly reduce the cost of additives (especially lithium resources are scarce and expensive) and even the cost of batteries, but also the dual organic ions give the structure of the compound higher design flexibility, and different organic functional groups can be selected to modify the function of the compound.

[0011] Preferably, R1, R2, R3, R4, R5, R6 and R7 are selected from -CH-, -CH2-, -CHCH3, -CHOCH3, -CF-, -CF2- and -CHCH=CH2.

[0012] Preferably, X and Y are selected from -F, -CH3, -CF3, -CH2Cl, -CH2CF3 and -CHCH=CH2.

[0013] Preferably, the G - Selected from tetrafluoroborate (BF4 - ), trifluoromethanesulfonate ([SO3CF3] - ), fluorosulfonate ([SO3F] - ) and hexafluorophosphate (PF6 - ) at least one of.

[0014] Preferably, the chemical structural formula of the nitrogen-substituted bicyclooctane quaternary ammonium salt lithium battery non-aqueous electrolyte additive is one of the following: In a second aspect, the present invention provides a non-aqueous electrolyte for lithium-ion batteries, which includes a nitrogen-substituted bicyclooctane quaternary ammonium salt-based lithium battery non-aqueous electrolyte additive, an organic solvent and a lithium salt.

[0015] Preferably, the nitrogen-substituted bicyclooctane quaternary ammonium salt lithium battery non-aqueous electrolyte additive accounts for 0.2-2% of the total mass of the non-aqueous electrolyte, and more preferably, accounts for 0.5-1% of the total mass of the non-aqueous electrolyte.

[0016] Preferably, the organic solvent is selected from at least one of cyclic carbonates, linear carbonates, cyclic carboxylates, linear carboxylates, sulfones, ethers and fluoroethers; further preferably selected from at least one of methyl propylene carbonate, ethyl propylene carbonate, ethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, 2,2,2-trifluoroethyl methyl carbonate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl pivalate, ethyl pivalate, butyl acetate, dimethyl sulfoxide, ethyl methyl sulfoxide, dioxolane, dimethoxypropane, and 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether.

[0017] Preferably, the organic solvent accounts for 40-90% of the total mass of the non-aqueous electrolyte.

[0018] Preferably, the lithium salt is selected from at least one of LiPF6, LiN(SO2F)2(LiFSI), LiN(SO2CF3)2, LiCF3SO3, LiC(SO2CF3)3, LiPF2(C2O4)2, LiPF2O2(LFP), LiBF4, LiB(C2O4)2 and LiBF2(C2O4)(LiODFB).

[0019] Preferably, the lithium salt accounts for 10-20% of the total mass of the non-aqueous electrolyte.

[0020] Preferably, the non-aqueous electrolyte further comprises other additives, selected from at least one of carbonates, halogenated carbonates, sulfates, sulfites, halogenated carboxylates, phosphates, halogenated phosphates, borates, nitrile compounds, silanes and phosphazenes; further preferably selected from vinylene carbonate (VC), vinyl ethylene carbonate (VEC), vinylene sulfate, vinyl sulfate (DTD), vinyl sulfite (ES), fluoroethylene carbonate (FEC), adiponitrile (AN), succinonitrile (SN), 1, At least one of 2-bis(2-cyanoethoxy)ethane (DENE), 1,3,6-hexanetrinitrile (HTCN), tris(trimethylsilyl)borate (TMSB), tris(trimethylsilyl)phosphite (TMSPi), tris(trimethylsilyl)phosphate (TMSPa), hexamethyldisilazane (HMDS), triethyl phosphate, tripropyl phosphate, tris(2,2,2-trifluoroethyl)phosphate, trivinyl phosphate, triallyl phosphate, tripropargyl phosphate and pentafluoroethoxyphosphazene; Preferably, the other additives account for 0.5-15% of the total mass of the non-aqueous electrolyte.

[0021] In a third aspect, the present invention provides the use of the above-mentioned nitrogen-substituted bicyclooctane quaternary ammonium salt lithium battery non-aqueous electrolyte additive in promoting the formation of an electrode solid electrolyte film on the surface of a lithium ion battery electrode.

[0022] In a fourth aspect, the present invention provides a lithium-ion battery, comprising a positive electrode, a negative electrode, a separator and the above-mentioned lithium-ion battery non-aqueous electrolyte.

[0023] Compared with the prior art, the beneficial effects of the present invention are: (1) When the nitrogen-substituted bicyclooctane quaternary ammonium salt compounds of the present invention are used as additives for non-aqueous electrolytes of lithium batteries, a denser protective film (solid electrolyte film) can be formed on the electrode surface, thereby better inhibiting the contact reaction between the electrode and the electrolyte, reducing the decomposition of the electrolyte and the corrosion of the electrode surface; at the same time, the content of nitrogen-containing substances in such compounds is relatively high, so that their solubility in organic electrolytes is lower, their high temperature resistance is better, and they have the characteristics of high lithium ion conductivity; under the combined effect of the above characteristics, the cycle stability of the battery under high voltage, room temperature and high temperature can be better improved.

[0024] (2) Compared with conventional lithium ion complex organic anion salts, the anions and cations of the compounds of the present invention are all organic ions and do not contain lithium ions. This can not only significantly reduce the cost of additives and even the cost of batteries, but also the dual organic ions give the structure of the compound a higher design flexibility, and different organic functional groups can be selected to modify the function of the compound. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 The battery cycle stability diagram (specific capacity-cycle number curve diagram) of Example 11 and Comparative Example 5.

[0026] Figure 2 The battery cycle stability diagram (specific capacity-cycle number curve diagram) of Example 13 and Comparative Example 7. DETAILED DESCRIPTION

[0027] The present invention will be further described below in conjunction with the embodiments.

[0028] Overall embodiment A nitrogen-substituted bicyclooctane quaternary ammonium salt lithium battery non-aqueous electrolyte additive, the chemical structure of which is as follows: in: R1, R2, R3, R4, R5, R6 and R7 are selected from a linear or branched saturated hydrocarbon group having 1 to 4 carbon atoms, or a saturated hydrocarbon group in which all or part of the hydrogen atoms are replaced by halogen elements; The functional groups X and Y are selected from fluorine atoms, or linear or branched saturated hydrocarbon groups having 1 to 4 carbon atoms, saturated hydrocarbon groups containing oxygen atoms, saturated hydrocarbon groups in which all or part of the hydrogen atoms are replaced by halogen elements, saturated hydrocarbon groups in which all or part of the hydrogen atoms are replaced by halogen elements and containing oxygen atoms, and unsaturated hydrocarbon groups containing double bonds or triple bonds; G- is an anion selected from tetrafluoroborate ([BF4] - ), trifluoromethanesulfonate ([SO3CF3] - ), fluorosulfonate ([SO3F] - ), hexafluorophosphate ([PF6]- ), bis(fluorosulfonyl)imide ([N(SO2F)2] - ), difluorophosphate ([PO2F2] - ), difluorooxalatoborate ([BF2(C2O4)] - ) and bis(oxalatoborate) ([B(C2O4)2] - ).

[0029] In some embodiments, R1, R2, R3, R4, R5, R6 and R7 are selected from -CH-, -CH2-, -CHCH3, -CHOCH3, -CF-, -CF2- and -CHCH=CH2.

[0030] In some embodiments, X and Y are selected from -F, -CH3, -CF3, -CH2Cl, -CH2CF3, and -CHCH=CH2.

[0031] In some embodiments, the G- is selected from tetrafluoroborate (BF4 - ), trifluoromethanesulfonate ([SO3CF3] - ), fluorosulfonate ([SO3F] - ) and hexafluorophosphate (PF6 - ) at least one of.

[0032] In some preferred embodiments, the chemical structural formula of the nitrogen-substituted bicyclooctane quaternary ammonium salt lithium battery non-aqueous electrolyte additive is one of the following: A non-aqueous electrolyte for lithium ion batteries comprises a nitrogen-substituted bicyclooctane quaternary ammonium salt lithium battery non-aqueous electrolyte additive, an organic solvent and a lithium salt.

[0033] In some embodiments, the nitrogen-substituted bicyclooctane quaternary ammonium salt lithium battery non-aqueous electrolyte additive accounts for 0.2-2% of the total mass of the non-aqueous electrolyte, and more preferably, accounts for 0.5-1% of the total mass of the non-aqueous electrolyte.

[0034] In some embodiments, the organic solvent is selected from at least one of cyclic carbonates, linear carbonates, cyclic carboxylates, linear carboxylates, sulfones, ethers and fluoroethers; further preferably selected from at least one of methyl propylene carbonate, ethyl propylene carbonate, ethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, 2,2,2-trifluoroethyl methyl carbonate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl pivalate, ethyl pivalate, butyl acetate, dimethyl sulfoxide, ethylmethyl sulfoxide, dioxolane, dimethoxypropane, and 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether.

[0035] In some embodiments, the organic solvent accounts for 40-90% of the total mass of the non-aqueous electrolyte.

[0036] In some embodiments, the lithium salt is selected from at least one of LiPF6, LiN(SO2F)2(LiFSI), LiN(SO2CF3)2, LiCF3SO3, LiC(SO2CF3)3, LiPF2(C2O4)2, LiPF2O2(LFP), LiBF4, LiB(C2O4)2 and LiBF2(C2O4)(LiODFB).

[0037] In some embodiments, the lithium salt accounts for 10-20% of the total mass of the non-aqueous electrolyte.

[0038] In some embodiments, the non-aqueous electrolyte further comprises other additives, selected from at least one of carbonates, halogenated carbonates, sulfates, sulfites, halogenated carboxylates, phosphates, halogenated phosphates, borates, nitrile compounds, silanes and phosphazenes; further preferably selected from vinylene carbonate (VC), vinyl ethylene carbonate (VEC), vinylene sulfate, vinyl sulfate (DTD), vinyl sulfite (ES), fluoroethylene carbonate (FEC), adiponitrile (AN), succinonitrile (SN), 1 , at least one of 2-bis(2-cyanoethoxy)ethane (DENE), 1,3,6-hexanetrinitrile (HTCN), tris(trimethylsilyl)borate (TMSB), tris(trimethylsilyl)phosphite (TMSPi), tris(trimethylsilyl)phosphate (TMSPa), hexamethyldisilazane (HMDS), triethyl phosphate, tripropyl phosphate, tris(2,2,2-trifluoroethyl)phosphate, trivinyl phosphate, triallyl phosphate, tripropargyl phosphate and pentafluoroethoxyphosphazene; In some embodiments, the other additives account for 0.5-15% of the total mass of the non-aqueous electrolyte.

[0039] A lithium-ion battery, comprising a positive electrode, a negative electrode, a separator and the above-mentioned lithium-ion battery non-aqueous electrolyte. There is no limitation on its structure, and there is no specific limitation on its processing and manufacturing process. Exemplarily, the structure of the battery is selected from any one of a button battery, a soft pack, an aluminum shell, a steel shell, a plastic shell and a cylindrical 18650 type.

[0040] The materials of the positive electrode, the negative electrode and the separator may be those known in the art.

[0041] In some embodiments, the positive electrode active material may be selected from at least one of the following materials: lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium iron phosphate and lithium manganese phosphate, but is not limited to the above materials.

[0042] In some embodiments, the negative electrode material may be selected from at least one of metallic lithium, graphite, mesophase carbon microspheres, amorphous carbon, lithium titanium oxide, lithium vanadium oxide, silicon-based materials, tin-based materials, and transition metal oxides, but is not limited to the above materials. In some embodiments, the graphite includes artificial graphite and natural graphite; the amorphous carbon includes hard carbon and soft carbon.

[0043] In some embodiments, the diaphragm is selected from polyolefin melt-stretched diaphragms; or the diaphragm is selected from diaphragms with at least one of PET (polyethylene terephthalate), polyvinylidene fluoride, aramid and polyamide as the base material; or it is selected from diaphragms coated with polyolefins on a high softening point porous matrix material, but is not limited to the above materials.

[0044] Specific Examples and Comparative Examples In order to make the purpose, technical scheme and beneficial technical effects of the present invention clearer, the present invention is further described in detail below in conjunction with specific examples and comparative examples. It should be understood that the specific embodiments described in this specification are only for explaining the present invention, not for limiting the present invention. The formula, proportion, etc. of the embodiments can be selected according to local conditions without substantial effect on the results.

[0045] (1) In all the following examples and comparative examples, lithium nickel manganese oxide (LiNi 0.5 Mn 1.5 O4) positive electrode was prepared according to the following method: The active material lithium nickel manganese oxide, binder (PVDF) and conductive agent (Super P) were mixed in a mass ratio of 95:2:3, and N-methylpyrrolidone (NMP) solvent was added and stirred to prepare a slurry. The slurry was evenly coated on an aluminum foil (thickness of 12 μm) current collector, coated on one side, and the surface density was controlled to be 15.0±0.5 mg / cm 2 The coated electrode was baked in a blast oven at 100°C for 2 hours. Then roller pressed to control the compaction density to 3.4g / cm 3 The rolled electrode was cut into electrode pieces with a diameter of 16 mm using a slicer, placed in a vacuum drying oven at 60°C for 24 hours, and transferred to a glove box for later use.

[0046] (2) In all the following examples and comparative examples, the graphite negative electrode was prepared according to the following method: The graphite active material, thickener sodium carboxymethyl cellulose (CMC), binder styrene butadiene rubber (SBR), and conductive agent (Super P) were mixed in a mass ratio of 94.5:1.5:2:2, and deionized water was added and stirred to prepare a slurry. The slurry was evenly coated on the copper foil (thickness of 6 μm) current collector (single-sided coating), and the surface density was 4.5±0.2 mg / cm 2Then it was dried in an oven at 105℃ for 2 hours. After completion, it was cold pressed and the compacted density was 1.6g / cm 3 , cut into electrodes with a diameter of 18 mm, put them into the vacuum drying oven at 60°C for 24 hours, and transfer them to the glove box for use.

[0047] (3) In all the following examples and comparative examples, the diaphragms were prepared according to the following method: The purchased polypropylene (PP) diaphragm was cut into diaphragm sheets with a diameter of 19 mm by a slicer, dried in a vacuum drying oven at 50° C. for 12 hours, and transferred to a glove box for use.

[0048] (4) In all the following examples and comparative examples, the electrolyte was prepared according to the following method: In a glove box with an argon atmosphere, mix the organic solvents according to the ratio, and add the nitrogen-substituted bicyclooctane quaternary ammonium salt compound and other electrolyte additives (if any). After mixing, place in the built-in refrigerator (8°C) of the glove box for 1 hour. Slowly dissolve the lithium salt in the mixed organic solvent and mix well to obtain an electrolyte.

[0049] (5) In all the following examples and comparative examples, the electrolyte was prepared according to the following method: In a glove box with an argon atmosphere, a CR2032-type button lithium-ion battery was assembled in the order of positive electrode shell, positive electrode sheet, separator, negative electrode sheet, electrolyte, gasket, spring and negative electrode shell.

[0050] (6) In all the following examples and comparative examples, the batteries were tested as follows: At an ambient temperature of 25°C, charge and discharge the battery in the voltage range of 3.5-4.95V. During the first charge and discharge, charge to 4.95V at a constant current of 0.1C, and then discharge to 3.5V at a constant current of 0.1C after being set aside.

[0051] At 25°C, the battery was charged at 1C constant current to 4.95V, then charged at 4.95V constant voltage to a cut-off current of 0.05C, left for 10 minutes, then discharged at 1C constant current to 3.5V, and left for 10 minutes. This charge and discharge process was repeated 100 times, and the discharge capacity was recorded each time.

[0052] Capacity retention after 100 cycles (%) = 100th discharge capacity / 1st discharge capacity × 100% Among them, in the preparation process of the above-mentioned battery, the names and abbreviations of some of the electrolyte organic solvents, lithium salts and additives involved are shown in Table 1 and the previous text (general embodiment part), and the specific formula of the selected electrolyte involved is shown in Table 2 and Table 3 below, and the content of each substance is the weight percentage calculated based on the total weight of the electrolyte.

[0053] Table 1: Names and abbreviations of some electrolyte solvents, lithium salts and additives Chinese naming abbreviation Ethylene carbonate EC Propylene carbonate PC Diethyl carbonate DEC Ethyl methyl carbonate EMC Vinylene carbonate VC Propyl Propionate PP Fluoroethylene carbonate FEC 1,1,2,2-Tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether HFE Propylene-1,3-sultone PST 1,3,6-Hexanetrinitrile HTCN Tetraethylammonium tetrafluoroborate ETB Lithium hexafluorophosphate <![CDATA[LiPF6]]> Lithium difluorooxalate borate LiODFB Lithium difluorophosphate LFP Lithium tetrafluoroborate <![CDATA[LiBF4]]> Table 2: Electrolyte formulations for various examples Table 3: Electrolyte formulas of various comparative examples The structures of the nitrogen-substituted bicyclooctaneamine and quaternary ammonium salt involved in the above comparative examples are as follows: (5) Test results The battery performance of the batteries in the above cases is shown in Table 4 below.

[0054] Table 4: Different electrolytes and corresponding battery performance Data analysis (1) By comparing Example 1 with Comparative Example 1, it can be found that, compared with the basic electrolyte containing only an organic solvent and a lithium salt (Comparative Example 1), after adding the nitrogen-substituted bicyclooctane quaternary ammonium salt A-1 (Example 1) of the present invention to the battery electrolyte, the capacity retention rate of the battery after 100 cycles is increased from 7.8% to 75.7%, and the cycle stability is greatly improved, which proves that the nitrogen-substituted bicyclooctane quaternary ammonium salt can indeed improve the internal stability of the battery and extend the cycle life.

[0055] Similarly, comparing the basic electrolyte containing only solvent and lithium salt (Comparative Example 5) with the electrolyte containing nitrogen-substituted bicyclooctane quaternary ammonium salt C-1 (Example 11), Figure 1 As shown, it can be clearly found that the capacity retention rate can be improved from 12.9% to 85.7%, and the improvement effect is also very significant.

[0056] Similarly, Example 13 containing both nitrogen-substituted bicyclooctane quaternary ammonium salt C-2 and other additives FEC is compared with Comparative Example 7 containing only FEC without C-2. Figure 2 As shown, the capacity retention rate of Example 13 is 90.4%, while that of Comparative Example 7 is only 66.4%.

[0057] Similarly, by comparing the electrolyte of Comparative Example 6 and Example 12 of the nitrogen-substituted bicyclooctane quaternary ammonium salt C-2, it can be found that the capacity retention of Example 12 is also significantly higher than that of Comparative Example 6.

[0058] The above comparison can fully prove that whether or not additional additives are used, the use of the nitrogen-substituted bicyclooctane quaternary ammonium salt of the present invention can effectively improve the cycle stability of the battery.

[0059] (2) By comparing Example 1 and Comparative Example 2, it can be found that when the additive used in Comparative Example 2 is not the nitrogen-substituted bicyclooctane quaternary ammonium salt of the present invention but the nitrogen-substituted heterocyclooctane DB-1, the cycle stability is far less than that of Example 1 (75.7%) containing the nitrogen-substituted bicyclooctane quaternary ammonium salt A-1. The reason may be that although the structure of DB-1 is similar to that of A-1, the former is a tertiary amine, while the latter is a quaternary ammonium salt containing anions, and the two are essentially different in nature. It is generally believed that the amine compound DB-1 is not easy to decompose into a film in the battery, and it is also unable to play the role of the salt structure like A-1 in forming a film on the electrode surface to play a protective effect and improve the lithium ion conductivity.

[0060] Similarly, by comparing Example 6 containing the nitrogen-substituted bicyclooctane quaternary ammonium salt B-1 of the present invention and containing the nitrogen-substituted bicyclooctane quaternary ammonium salt DB-2 (Comparative Example 3) not of the present invention, it can be found that the capacity retention rate of Example 6 (87.4%) is significantly higher than that of Comparative Example 3 (63.3%). The reason may be that although the cation of DB-2 is completely consistent with the nitrogen-substituted bicyclooctane quaternary ammonium salt B-1 of the present invention, the anion of DB-2 is a chloride ion, which is not involved in the present invention. In the existing literature and patent reports, there are few successful cases of chloride ions as additive structural units, and it is also unknown whether chloride ions can participate in the formation of the electrode surface passivation film.

[0061] Similarly, by comparing Example 8 containing the nitrogen-substituted bicyclooctane quaternary ammonium salt B-2 of the present invention and Comparative Example 4 containing tetraethylammonium tetrafluoroborate ETB (a structure not of the present invention), it can be found that the capacity retention rate of Example 8 (90.0%) is higher than that of Comparative Example 4 (77.2%). The reason may be that the cation of tetraethylammonium tetrafluoroborate ETB is tetraethylammonium, not the nitrogen-substituted bicyclooctane quaternary ammonium salt structure of the present invention, and even if it can participate in the formation of the passivation film (solid electrolyte film), it cannot form a dense, strong and stable passivation film like the nitrogen-substituted bicyclooctane quaternary ammonium salt, so the battery cycle stability is reduced.

[0062] The above comparison proves that even though the chemical structure of the additive in the comparative example is similar to that of the nitrogen-substituted bicyclooctane quaternary ammonium salt of the present invention, it still cannot achieve the effect similar to that of the nitrogen-substituted bicyclooctane quaternary ammonium salt of the present invention because it does not fully possess the characteristics of the compound of the present invention.

[0063] (3) By comparing Example 2 with Example 3, it can be found that Example 3 uses the nitrogen-substituted bicyclooctane quaternary ammonium salt A-5 without alkenyl structure, while Example 2 uses the nitrogen-substituted bicyclooctane quaternary ammonium salt A-3 containing an alkenyl structure. Under the same condition of small addition amount (0.2%), since A-3 has higher unsaturation, higher π bond chemical activity, and is more likely to participate in the formation of the passivation film, the capacity retention rate (78.0%) of the battery of Example 2 (containing A-3) is higher than that of Example 3 (containing A-5) (71.9%), that is, the alkenyl functional group plays an important role in promoting the film formation of the nitrogen-substituted bicyclooctane quaternary ammonium salt.

[0064] (4) By comparing Example 4 with Example 5, it can be found that the components contained in the electrolytes of the two are exactly the same, but the amount of nitrogen-substituted bicyclooctane quaternary ammonium salt added in Example 4 is 2%, while that in Example 5 is higher at 3%. It is possible that the high content leads to a too thick passivation film formed, which increases the battery impedance and hinders the release and insertion of lithium ions, which is not conducive to the long-term cycle of the battery. Therefore, the cycle stability of the battery in Example 5 (capacity retention rate after 100 cycles is 70.1%) is worse than that in Example 4 (capacity retention rate after 100 cycles is 80.3%). This shows that the higher the amount of nitrogen-substituted bicyclooctane quaternary ammonium salt added in the present invention, the better.

[0065] (5) By comparing Example 6 with Example 7, it can be found that Example 7 only contains nitrogen-substituted bicyclooctane quaternary ammonium salt B-1 but no additional lithium salt LFP, and it is found that the capacity retention rate of Example 7 (72.5%) is lower than that of Example 6 (87.4%). The possible reason is that the nitrogen-substituted bicyclooctane quaternary ammonium salt and LFP in Example 6 produce a synergistic effect, which plays a role in forming an electrode passivation film with lower impedance, stronger lithium ion conductivity and higher stability, so the battery stability of Example 6 is higher.

[0066] (6) By comparing Example 8 with Example 6, and Example 10 with Example 6, it can be found that whether it is a battery using a bicyclooctane quaternary ammonium salt in which the hydrogen on the alkyl group connected to the nitrogen cation is replaced by a fluorine atom (such as B-2 in Example 8, a single cation contains three fluorine atoms), or a battery using a bicyclooctane quaternary ammonium salt in which the hydrogen on the octane in the structure is replaced by fluorine (such as B-4 in Example 10, a single cation contains nine fluorine atoms), the battery has a higher capacity retention rate after cycling than the battery using a bicyclooctane quaternary ammonium salt with less fluorine substitution (such as B-1 in Example 6, a single cation contains only one fluorine atom). This shows that reasonable fluorine substitution can make the effect of stabilizing the battery cycle capacity of the bicyclooctane quaternary ammonium salt more obvious.

[0067] (7) By comparing Example 14 and Example 15, it can be found that when Example 14 uses the nitrogen-substituted bicyclooctane quaternary ammonium salt of the present invention and additional HFE and PST as additives, the capacity retention rate after cycling (95.0%) of Example 14 is significantly improved compared with Example 15 (capacity retention rate after 100 cycles is 79.1%) without other additives such as HFE and PST. This shows that the reasonable use of other additives can achieve synergistic effects with the nitrogen-substituted bicyclooctane quaternary ammonium salt, thereby further improving the cycle stability of the battery.

[0068] The raw materials and equipment used in the present invention, unless otherwise specified, are all commonly used raw materials and equipment in the art; the methods used in the present invention, unless otherwise specified, are all conventional methods in the art.

[0069] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A nitrogen-substituted bicyclooctane quaternary ammonium salt lithium battery non-aqueous electrolyte additive, characterized in that: The chemical structure is shown below: R1, R2, R3, R4, R5, R6 and R7 are selected from a linear or branched saturated hydrocarbon group having 1 to 4 carbon atoms, or a saturated hydrocarbon group in which all or part of the hydrogen atoms are replaced by halogen elements; The functional groups X and Y are selected from fluorine atoms, or linear or branched saturated hydrocarbon groups having 1 to 4 carbon atoms, saturated hydrocarbon groups containing oxygen atoms, saturated hydrocarbon groups in which all or part of the hydrogen atoms are replaced by halogen elements, saturated hydrocarbon groups in which all or part of the hydrogen atoms are replaced by halogen elements and containing oxygen atoms, and unsaturated hydrocarbon groups containing double bonds or triple bonds; G- is selected from the group consisting of tetrafluoroborate, trifluoromethanesulfonate, fluorosulfonate, hexafluorophosphate, bisfluorosulfonimide, difluorophosphate, difluorooxalatoborate and bisoxalatoborate.

2. The nitrogen-substituted bicyclooctane quaternary ammonium salt lithium battery non-aqueous electrolyte additive according to claim 1, characterized in that: The R1, R2, R3, R4, R5, R6 and R7 are selected from -CH-, -CH2-, -CHCH3, -CHOCH3, -CF-, -CF2- and -CHCH=CH2.

3. The nitrogen-substituted bicyclooctane quaternary ammonium salt lithium battery non-aqueous electrolyte additive according to claim 1, characterized in that: The X and Y are selected from -F, -CH3, -CF3, -CH2Cl, -CH2CF3 and -CHCH=CH2.

4. The nitrogen-substituted bicyclooctane quaternary ammonium salt lithium battery non-aqueous electrolyte additive according to claim 1, characterized in that: The G- is selected from at least one of tetrafluoroborate, trifluoromethanesulfonate, fluorosulfonate and hexafluorophosphate.

5. The nitrogen-substituted bicyclooctane quaternary ammonium salt lithium battery non-aqueous electrolyte additive according to claim 1, characterized in that: The chemical structure is one of the following:

6. Use of the nitrogen-substituted bicyclooctane quaternary ammonium salt lithium battery non-aqueous electrolyte additive according to any one of claims 1 to 5 in lithium ion battery non-aqueous electrolyte.

7. The use according to claim 6, characterized in that: The non-aqueous electrolyte comprises a nitrogen-substituted bicyclooctane quaternary ammonium salt lithium battery non-aqueous electrolyte additive, an organic solvent and a lithium salt.

8. The use according to claim 6 or 7, characterized in that: The nitrogen-substituted bicyclooctane quaternary ammonium salt lithium battery non-aqueous electrolyte additive accounts for 0.2-2% of the total mass of the non-aqueous electrolyte.

9. The use according to claim 7, characterized in that: The organic solvent is selected from at least one of cyclic carbonates, linear carbonates, cyclic carboxylates, linear carboxylates, sulfones, ethers and fluoroethers; The lithium salt is selected from at least one of LiPF6, LiN(SO2F)2, LiN(SO2CF3)2, LiCF3SO3, LiC(SO2CF3)3, LiPF2(C2O4)2, LiPF2O2, LiBF4, LiB(C2O4)2 and LiBF2(C2O4).

10. The use according to claim 7, characterized in that: The non-aqueous electrolyte further comprises other additives, selected from at least one of carbonates, halogenated carbonates, sulfates, sulfites, halogenated carboxylates, phosphates, halogenated phosphates, borates, nitrile compounds, silanes and phosphazenes; The other additives account for 0.5-15% of the total mass of the non-aqueous electrolyte.