Modified electrospinning composite diaphragm, preparation method thereof and lithium battery comprising modified electrospinning composite diaphragm
Polyacrylonitrile/polyvinylidene fluoride nanofiber separators were prepared by electrospinning and heat treatment, and SiO2/GO composite layer was coated on its surface, which solved the problem of lithium dendrites in lithium batteries and improved the electrochemical performance of the batteries and safety, achieving stability and long life in high temperature environments.
Patent Information
- Application Number
- CN202411228488.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Lithium metal batteries are prone to form lithium dendrites during charging and discharging, resulting in short circuits of the battery, affecting its safety and cycle life. The existing diaphragm materials are insufficient mechanical strength, poor electrolyte absorption performance, and large interface impedance of the diaphragm, making it difficult to effectively suppress lithium branches. Growth of crystals.
Polyacrylonitrile/polyvinylidene fluoride nanofiber separators were prepared by electrospinning process, and coated with heat treatment and SiO2/GO composite solution to form a modified electrospin composite separator, which improves the mechanical strength and electrochemical performance of the separator and blocks lithium Dentite penetration.
It improves the electrochemical performance and safety stability of lithium batteries, enhances the dendrite resistance and cycle stability of the separator, maintains the mechanical properties in high temperature environments, and extends the service life of the battery.
Smart Images

Figure CN118920016A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium batteries, and in particular to a modified electrospun composite diaphragm and a preparation method thereof, and a lithium battery comprising the same. Background Art
[0002] Lithium metal batteries are considered to be a strong contender for the next generation of energy storage devices due to their high energy density and high capacity. However, lithium metal anodes are prone to form lithium dendrites during the charge and discharge process. These dendrites can penetrate the separator and cause battery short circuits, seriously affecting the safety and cycle life of the battery. Therefore, inhibiting the growth of lithium dendrites has become one of the key issues in improving the performance of lithium metal batteries.
[0003] At present, relevant technicians have suppressed the growth of lithium dendrites by optimizing diaphragm materials, developing functional coatings, and preparing multifunctional composite diaphragms. However, the diaphragm materials prepared by the above methods still have problems such as insufficient mechanical strength, poor electrolyte absorption performance, and large diaphragm interface impedance, which are not conducive to improving the electrochemical performance and safety and stability of lithium batteries.
[0004] Therefore, it is necessary to provide a solution for modifying the electrospun composite membrane to improve the electrochemical performance and safety stability of lithium batteries. Summary of the invention
[0005] In view of this, the present application provides a modified electrospun composite diaphragm and a preparation method thereof, and a lithium battery comprising the same, to solve the problem of how to improve the electrochemical performance and safety and stability of lithium batteries.
[0006] In order to achieve the above technical objectives, this application adopts the following technical solutions:
[0007] In a first aspect, the present application provides a method for preparing a modified electrospun composite membrane, comprising the following steps:
[0008] S1. Using polyacrylonitrile and polyvinylidene fluoride as raw materials, electrospinning is performed to obtain PAN / PVDF (polyacrylonitrile / polyvinylidene fluoride) nanofiber membrane;
[0009] S2. heat treating the PAN / PVDF nanofiber membrane to obtain a membrane matrix;
[0010] S3. Coat the SiO2 / GO composite solution on the surface of the membrane substrate and then dry it to obtain the modified electrospun composite membrane.
[0011] Preferably, in step S1, the process parameters of electrospinning are as follows: voltage is 16-20 KV, flow rate is 0.01-0.03 ml / min, and collection distance is 80-90 mm.
[0012] Preferably, in step S1, the mass ratio of polyacrylonitrile to polyvinylidene fluoride is 1-3:1.
[0013] Preferably, in step S2, the heat treatment temperature is 170-180° C., and the heat treatment time is 0.5-1 h.
[0014] Preferably, in step S3, the preparation method of the SiO2 / GO composite solution is: after mixing the SiO2 nanoparticles and the GO solution, ultrasonic stirring is performed to obtain the SiO2 / GO composite solution.
[0015] Preferably, in step S3, the mass ratio of SiO2 to GO is 2-3:1.
[0016] Preferably, the thickness ratio of the membrane matrix to the film layer after the SiO2 / GO composite solution is dried is 5:2-3.
[0017] In a second aspect, the present application provides a modified electrospun composite membrane.
[0018] In a third aspect, the present application provides a lithium battery comprising a modified electrospun composite membrane.
[0019] In a fourth aspect, the present application provides an application of a lithium battery in the automotive and / or aerospace fields.
[0020] The beneficial effects of the present application are as follows: the present application can prepare a PAN / PVDF nanofiber separator with high porosity and good electrolyte absorption performance through the electrospinning process of step S1, which is conducive to the efficient transmission and uniform deposition of lithium ions and improves the electrochemical performance of the battery. The heat treatment of step S2 causes cross-linking and crystallization between the PAN / PVDF nanofiber separators, which is conducive to improving the mechanical strength and thermal stability of the separator, effectively blocking the penetration of lithium dendrites and maintaining the profile unchanged in an environment of 180°C and above, and ultimately improving the safety and stability of the battery; through step S3, SiO2 / GO is coated on the separator substrate as a modified layer, the conductivity and lithium-philic functional groups of graphene can regulate the uniform deposition of lithium ions, and the chemical reaction of SiO2 with lithium dendrites can eliminate the growth of lithium dendrites, improve the anti-dendrite ability and electrochemical performance of the separator, and at the same time, the SiO2 / GO of the present application has good compatibility with the substrate, will not increase the interface impedance of the separator, and ultimately improve the cycle stability and capacity retention rate of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 Microscopic images of PAN / PVDF nanofibers before and after heat treatment. DETAILED DESCRIPTION
[0022] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0023] The present application provides a method for preparing a modified electrospun composite membrane, comprising the following steps:
[0024] S1. Using polyacrylonitrile and polyvinylidene fluoride as raw materials, electrospinning was performed to obtain PAN / PVDF nanofiber membrane;
[0025] S2. heat treating the PAN / PVDF nanofiber membrane to obtain a membrane matrix;
[0026] S3. Coat the SiO2 / GO composite solution on the surface of the membrane substrate and then dry it to obtain the modified electrospun composite membrane.
[0027] The present application can prepare a PAN / PVDF (polyvinylidene fluoride) nanofiber diaphragm with high porosity and good electrolyte absorption performance through the electrospinning process of step S1, which is conducive to the efficient transmission and uniform deposition of lithium ions, and improves the rate performance of the battery. The heat treatment of step S2 causes cross-linking and crystallization between the PAN / PVDF nanofiber diaphragms, which is conducive to improving the mechanical strength and thermal stability of the diaphragm, effectively blocking the penetration of lithium dendrites and maintaining the profile unchanged in an environment of 180°C and above, and ultimately improving the safety and stability of the battery. Through step S3, SiO2 / GO is coated on the diaphragm substrate as a modified layer, the conductivity and lithium-philic functional groups of graphene can regulate the uniform deposition of lithium ions, and the chemical reaction of SiO2 with lithium dendrites can eliminate the growth of lithium dendrites, improve the anti-dendrite ability and electrochemical performance (cycle life, coulomb efficiency and safety performance) of the diaphragm, and at the same time, the SiO2 / GO of the present application has good compatibility with the substrate, will not increase the interface impedance of the diaphragm, and ultimately improve the cycle stability and capacity retention rate of the battery.
[0028] In the present application, in step S1, the process parameters of electrospinning are as follows: voltage is 16-20KV, flow rate is 0.01-0.03ml / min, and collection distance is 80-90mm.
[0029] In step S1, the process of preparing PAN / PVDF nanofiber membrane by electrospinning is as follows: dissolving PAN and PVDF in a solvent to obtain a mixed solution; the solvent includes one or more of DMF and THF; placing the mixed solution in an electrospinning device, adjusting the voltage, flow rate, and collection distance, and performing an electrospinning process to prepare a PAN / PVDF nanofiber membrane.
[0030] The present application adjusts the electrospinning process parameters to ensure that the porosity of the modified electrospun composite membrane is ≥75% and the electrolyte absorption performance is ≥552%, so as to ensure the uniform deposition and efficient transmission of lithium ions.
[0031] In some embodiments, in step S1, the mass ratio of polyacrylonitrile to polyvinylidene fluoride is 1-3:1.
[0032] In some embodiments, in step S2, the heat treatment temperature is 170-180° C., and the heat treatment time is 0.5-1 h.
[0033] At the above heat treatment temperature, it is more conducive to cross-linking and crystallization between the nanofibers to improve the mechanical strength of the diaphragm.
[0034] The heat treatment step of step S2 is: placing the PAN / PVDF nanofiber membrane in a vacuum oven and heat treating it at 170-180°C for 0.5-1h to obtain a membrane matrix. After the heat treatment, the tensile strength and thermal dimensional stability of the membrane matrix are significantly improved.
[0035] In some embodiments, in step S3, the preparation method of the SiO2 / GO composite solution is: after mixing the SiO2 nanoparticles and the GO solution, ultrasonic stirring is performed to obtain the SiO2 / GO composite solution.
[0036] In some embodiments, in step S3, the coating method is: soaking the membrane substrate into the SiO2 / GO composite solution, and then taking it out. The taken-out membrane is dried in a drying oven to obtain a modified electrospun composite membrane.
[0037] Coating in the above manner is beneficial for SiO2 / GO to be evenly distributed on the surface of the diaphragm substrate.
[0038] In some embodiments, in step S3, the mass ratio of SiO2 to GO is 2-3:1.
[0039] In some embodiments, the thickness ratio of the membrane substrate to SiO2 / GO is 5:2-3.
[0040] In a second aspect, the present application provides a modified electrospun composite membrane.
[0041] In a third aspect, the present application provides a lithium battery comprising a modified electrospun composite membrane.
[0042] In a fourth aspect, the present application provides an application of a lithium battery in the automotive and / or aerospace fields.
[0043] The lithium battery of the present application has the advantages of high thermal stability (resistant to deformation at 180°C), high safety, good cycle stability and capacity retention rate, and can meet the demand for high temperature resistance of lithium batteries in the automotive and / or aerospace fields.
[0044] The present solution is further described below through specific embodiments.
[0045] Example 1
[0046] A method for preparing a modified electrospun composite membrane comprises the following steps:
[0047] S1. A 10 wt% solution (PAN: PVDF = 3: 1) was placed in an electrospinning device, the voltage was adjusted to 18 KV, the flow rate was 0.02 ml / min, the collection distance was 90 mm, and electrospinning was performed to obtain a PAN / PVDF nanofiber membrane;
[0048] S2. The PAN / PVDF nanofiber membrane was placed in a vacuum oven and heat treated at 170°C for 0.5 h to obtain a membrane matrix;
[0049] S3. Ultrasonic dispersion of SiO2 particles in GO solution to obtain SiO2 / GO composite solution, coating the SiO2 / GO composite solution on the diaphragm substrate, and drying the solution in a drying oven at 70°C to obtain a modified electrospun composite diaphragm.
[0050] Example 2
[0051] A method for preparing a modified electrospun composite membrane comprises the following steps:
[0052] S1. Place a solution with a concentration of 8 wt% (PAN: PVDF = 3: 1) in an electrospinning device, adjust the voltage to 18 KV, the flow rate to 0.02 ml / min, and the collection distance to 90 mm for electrospinning to obtain a PAN / PVDF nanofiber membrane;
[0053] S2. The PAN / PVDF nanofiber membrane was placed in a vacuum oven and heat treated at 170°C for 0.5 h to obtain a membrane matrix;
[0054] S3. Ultrasonic dispersion of SiO2 particles in GO solution to obtain SiO2 / GO composite solution, coating the SiO2 / GO composite solution on the diaphragm substrate, and drying the solution in a drying oven at 70°C to obtain a modified electrospun composite diaphragm.
[0055] Example 3
[0056] A method for preparing a modified electrospun composite membrane comprises the following steps:
[0057] S1. A 12 wt% solution (PAN: PVDF = 3: 1) was placed in an electrospinning device, the voltage was adjusted to 18 KV, the flow rate was 0.02 ml / min, the collection distance was 90 mm, and electrospinning was performed to obtain a PAN / PVDF nanofiber membrane;
[0058] S2. The PAN / PVDF nanofiber membrane was placed in a vacuum oven and heat treated at 180°C for 0.5 h to obtain a membrane matrix;
[0059] S3. Ultrasonic dispersion of SiO2 particles in GO solution to obtain SiO2 / GO composite solution, coating the SiO2 / GO composite solution on the diaphragm substrate, and drying the solution in a drying oven at 70°C to obtain a modified electrospun composite diaphragm.
[0060] Comparative Example 1
[0061] A method for preparing a composite diaphragm, the other contents are the same as those of Example 1, except that the voltage is adjusted to 22KV, the flow rate is 0.04ml / min, the collection distance is 70mm,
[0062] Comparative Example 2
[0063] A method for preparing a composite diaphragm, the other contents are the same as those of Example 1, and the heat treatment temperature of step S2 is 150°C.
[0064] Comparative Example 3
[0065] A method for preparing a composite diaphragm, the other contents are the same as those of Example 1, and the heat treatment temperature of step S2 is 200°C.
[0066] Comparative Example 4
[0067] A method for preparing a composite diaphragm, the other contents of which are the same as those of Example 1, excluding the heat treatment process of step S2.
[0068] Comparative Example 5
[0069] A method for preparing a composite diaphragm, the other contents are the same as those of Example 1, excluding step S3.
[0070] Comparative Example 6
[0071] A method for preparing a composite membrane, the other contents are the same as those of Example 1, and the SiO2 / GO composite solution is replaced by a GO solution of equal concentration.
[0072] Comparative Example 7
[0073] A method for preparing a composite membrane, the other contents are the same as those of Example 1, and the SiO2 / GO composite solution is replaced by a SiO2 solution of equal concentration.
[0074] Test and Evaluation
[0075] The mechanical strength, electrolyte absorption rate, porosity, dimensional stability and anti-dendrite ability of the composite membranes obtained in various embodiments and comparative examples were tested, and the results are shown in Table 1.
[0076] The test content and methods are as follows:
[0077] Mechanical strength: Use a thickness gauge to measure the thickness of the diaphragm and record it as A. Place the diaphragm on a cutting machine and cut it into strips with a width of 10 mm. Then, draw lines at 10 cm intervals on the diaphragm cut into strips, and then clamp the diaphragm on the universal tester. After entering the relevant parameters, start measuring. When the diaphragm is broken, the tensile strength will be displayed, and the tensile strength can be read. High mechanical strength of the diaphragm can effectively improve the anti-dendrite ability.
[0078] Electrolyte absorption rate: Soak the dry diaphragm in liquid electrolyte for 2 hours, and calculate the absorption rate (E%) of the diaphragm electrolyte by measuring the difference in diaphragm weight before and after the test. The electrolyte absorption of the diaphragm is calculated by the formula: W1 is the weight of the dry diaphragm, and W2 is the wet weight after wiping the liquid electrolyte on the diaphragm surface with filter paper.
[0079]
[0080] Porosity: The porosity of the membrane was measured by the n-butanol method. The dried membrane was cut into a circular shape with a diameter of 2.0 cm. The circular membrane with a dry weight Md was immersed in n-butanol for 2 h, and then the n-butanol on the surface was removed with filter paper to obtain the wet weight Mw. The porosity (P%) of the membrane was calculated using the following formula: Where ρ is the density of n-butanol and V is the volume of the dry membrane.
[0081]
[0082] Dimensional stability: The diaphragm was cut into a circle with a diameter of 1.5 cm and placed at 150°C, 170°C, 180°C and 200°C for 0.5 hours. The thermal shrinkage behavior was observed according to the change in area size and the profile deformation temperature was recorded.
[0083] Table 1 Performance test results of composite diaphragm
[0084]
[0085] By comparing Example 1, Example 2, and Example 3, it can be found that the porosity and electrolyte absorption performance of the electrospinning membrane are generally closely related to the solution concentration. When the solution concentration is high, the viscosity and surface tension of the spinning solution increase, resulting in an increase in the fiber diameter, thereby reducing the porosity of the membrane. This smaller porosity may reduce the absorption performance of the membrane to the electrolyte. However, if the solution concentration is too low, the formability of the fiber may deteriorate, resulting in an uneven pore structure, which will also affect the absorption of the electrolyte. Therefore, the solution concentration needs to be within a reasonable range to achieve higher porosity and good electrolyte absorption performance.
[0086] By comparing Example 1 and Comparative Example 1, it can be found that excessively high voltage may cause irregular accumulation of fibers on the collector, resulting in uneven pore structure, which may affect the electrolyte absorption performance. Higher flow rates and short collection distances usually lead to an increase in fiber diameter and a decrease in porosity, thereby weakening the electrolyte absorption capacity.
[0087] Compare Example 1 with Comparative Example 2, Comparative Example 3, and Comparative Example 4. It can be found that different heat treatment temperatures have a significant effect on the tensile strength, porosity, and electrolyte absorption performance of the electrospinning membrane. As the heat treatment temperature increases, the fibers may melt or crystallize, so that the bonding force between the fibers is enhanced, thereby increasing the tensile strength of the membrane. However, too high a temperature may cause the fibers to shrink excessively or break, which in turn reduces the tensile strength. Moderate heat treatment can allow the fibers to bond to each other, improve structural stability, and maintain a certain porosity; while high temperature treatment may cause the fibers to melt, fill the pores, and reduce the porosity. Lower heat treatment temperatures generally help maintain a higher porosity, thereby improving electrolyte absorption capacity; but if the heat treatment temperature is too high, the porosity decreases, and the electrolyte absorption performance will also decrease accordingly.
[0088] Therefore, the heat treatment temperature needs to be precisely controlled to optimize the mechanical properties, porosity, and electrolyte absorption properties of the electrospun separators.
[0089] Compare Example 1 with Comparative Example 5, Comparative Example 6, and Comparative Example 7. It can be found that coating SiO2 / GO on the electrospinning membrane has a significant effect on the performance. Coating SiO2 / GO can generally improve the mechanical strength of the membrane. SiO2 generally has good hydrophilicity and may increase the absorption of the electrolyte.
[0090] The composite diaphragms obtained in the embodiments and comparative examples were prepared into lithium batteries, and the electrochemical performance and safety stability of the lithium batteries were tested. The results are shown in Table 2.
[0091] Cyclic test: At room temperature, the initial capacity of batteries with different separators was tested at a rate of 0.2C. At a rate of 2C, the capacity retention rate of batteries with different separators after 500 cycles was tested.
[0092] Table 2 Performance test results of lithium batteries
[0093]
[0094] The initial capacity of batteries with different separators at 0.2C rate is closely related to electrolyte absorption. Good electrolyte absorption capacity can ensure that the electrolyte fully infiltrates the electrode material, promote ion conduction and electrochemical reactions, and thus increase the initial capacity of the battery. If the separator or electrode does not absorb the electrolyte sufficiently, the active sites in the electrode material cannot be effectively utilized, resulting in a decrease in initial capacity. Therefore, optimizing electrolyte absorption performance is an important factor in improving the initial capacity of the battery.
[0095] The capacity retention rate of the battery after 500 cycles at 2C rate is closely related to the mechanical properties of the diaphragm and the coating layer. The good mechanical properties of the diaphragm can effectively inhibit the penetration of lithium dendrites, thereby extending the battery life. The coated SiO2 or GO layer can further enhance the strength and stability of the diaphragm, provide additional protection, prevent dendrites from piercing the diaphragm, and improve the battery's anti-dendrite ability and capacity retention rate.
[0096] The present application can prepare a PAN / PVDF nanofiber diaphragm with high porosity and good electrolyte absorption performance through the electrospinning process of step S1, which is conducive to the efficient transmission and uniform deposition of lithium ions and improves the electrochemical performance of the battery. The heat treatment of step S2 causes cross-linking and crystallization between the PAN / PVDF nanofiber diaphragms, which is conducive to improving the mechanical strength and thermal stability of the diaphragm, effectively blocking the penetration of lithium dendrites and maintaining the profile unchanged in an environment of 180°C and above, ultimately improving the safety and stability of the battery. Through step S3, SiO2 / GO is coated on the diaphragm substrate as a modified layer, the conductivity and lithium-philic functional groups of graphene can regulate the uniform deposition of lithium ions, and the chemical reaction of SiO2 with lithium dendrites can eliminate the growth of lithium dendrites, improve the anti-dendrite ability and electrochemical performance of the diaphragm, and at the same time, the SiO2 / GO of the present application has good compatibility with the substrate, will not increase the interface impedance of the diaphragm, and ultimately improve the cycle stability and capacity retention rate of the battery.
[0097] Figure 1The microscopic images of PAN / PVDF nanofibers before and after heat treatment show that after heat treatment, a cross-linked structure is generated at the fiber joints, which can effectively improve the tensile strength. And the cross-sectional image of the composite membrane after coating SiO2 / GO on the heat-treated PAN / PVDF, the coating layer is evenly covered on the membrane surface. Among them, Figure (a) is a PAN / PVDF nanofiber membrane without heat treatment, it can be found that the fibers are cross-arranged without connection. Figure (b) is a heat-treated PAN / PVDF nanofiber membrane, and a cross-linked structure is generated between the fibers. Figure (c) is the cross-sectional morphology of the composite membrane, showing the thickness of the coating layer and the fiber layer. Figures (d), (e) and (f) are elemental images of the coating layer of the composite membrane cross-section, it can be found that the C, O, and Si elements are evenly distributed.
[0098] The above are only preferred specific implementations of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.
Claims
1. A method for preparing a modified electrospun composite membrane, characterized in that: The following steps are involved: S1. Using polyacrylonitrile and polyvinylidene fluoride as raw materials, electrospinning was performed to obtain PAN / PVDF nanofiber membrane; S2. heat treating the PAN / PVDF nanofiber membrane to obtain a membrane matrix; S3. Coating the SiO2 / GO composite solution on the surface of the membrane substrate, and then drying to obtain the modified electrospun composite membrane.
2. The method for preparing the modified electrospun composite membrane according to claim 1, characterized in that: In step S1, the process parameters of the electrospinning are as follows: voltage is 16-20 KV, flow rate is 0.01-0.03 ml / min, and collection distance is 80-90 mm.
3. The method for preparing the modified electrospun composite membrane according to claim 1, characterized in that: In step S1, the mass ratio of polyacrylonitrile to polyvinylidene fluoride is 1-3:
1.
4. The method for preparing the modified electrospun composite membrane according to claim 1, characterized in that: In step S2, the heat treatment temperature is 170-180°C, and the heat treatment time is 0.5-1h.
5. The method for preparing the modified electrospun composite membrane according to claim 1, characterized in that: In step S3, the preparation method of the SiO2 / GO composite solution is: after mixing SiO2 nanoparticles and GO solution, ultrasonic stirring is performed to obtain the SiO2 / GO composite solution.
6. The method for preparing the modified electrospun composite membrane according to claim 5, characterized in that: In step S3, the mass ratio of SiO2 to GO is 2-3:
1.
7. The method for preparing the modified electrospun composite membrane according to claim 1, characterized in that: The thickness ratio of the membrane substrate to the film layer after the SiO2 / GO composite solution is dried is 5:2-3.
8. A modified electrospun composite membrane obtained by the preparation method according to any one of claims 1 to 7.
9. A lithium battery, characterized in that: It comprises the modified electrospun composite membrane as claimed in claim 8.
10. Use of the lithium battery according to claim 9 in the automotive and / or aerospace fields.
Citation Information
Patent Citations
Lithium ion battery hybrid separation membrane preparation method
CN108172736A
Cited By
Ultrafast-charge electrostatic spinning lithium battery diaphragm, preparation method and application
CN120601074A