Electro-absorption modulated semiconductor laser and preparation method and application thereof
By adopting a two-stage grating layer structure and SAG growth method in the electrical absorption modulated semiconductor laser, the limitations of the electrical absorption modulator capacitance and light reflection on the laser are solved, and high modulation bandwidth and stable optical performance are achieved.
Patent Information
- Application Number
- CN202410972745.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-19
AI Technical Summary
The modulation bandwidth of existing electrical absorption modulation semiconductor lasers is limited by the device capacitance of the electrical absorption modulator and the parasitic parameters introduced by the package, and the light reflection between DFB and EA affects the laser state and signal quality.
An electrical absorption modulated semiconductor laser is designed, using a two-stage grating layer structure, with the grating of the L1 region short and the grating of the L2 region long and the optical coupling coefficient of the L1 region is greater than 1.2 times the optical coupling coefficient of the L2 region. The grating layer of the laser is grown by the SAG method. Reduce light reflection affects laser mode.
The stability of the luminescence mode and the stability of the light-current-voltage curve are achieved, the peaks and valleys of chirp and frequency response are reduced, signal quality is improved, and process flow is simplified.
Smart Images

Figure CN118920268A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of optoelectronic devices, and in particular relates to an electro-absorption modulated semiconductor laser and a preparation method and application thereof. Background Art
[0002] Electroabsorption modulated semiconductor laser (EML) is a key device commonly used in modern high-speed optical communication systems. It has the characteristics of high bandwidth, low chirp, high modulation depth and compact structure. It is a hot spot in the current research of optoelectronic integrated devices and the mainstream direction of the development of future high-speed optical communication chips.
[0003] At present, the research on EML chips for high-speed optical communication mainly focuses on improving the modulation bandwidth, output power and single-mode characteristics of EML lasers. The modulation bandwidth of EML is mainly limited by the device capacitance of the electro-absorption modulator (EAM). At the same time, the parasitic parameters introduced by the package leads will also affect the high-frequency modulation characteristics of the device. In order to improve the modulation bandwidth of EML, it is necessary to reduce the PN junction capacitance and electrode pad capacitance of the EA modulator and eliminate the influence of the parasitic parameters introduced by the package. The following methods are used in the existing literature: (1) Neophotonics uses a thin absorption region structure, steep doping distribution and BCB electrode process to increase the modulation bandwidth of EML to more than 40GHz and reach 56GB; (2) Sumitomo Electric uses a dual-segment absorption region with different wavelengths to make the PN junction narrower and shorter, and the modulation bandwidth of EML can also reach 56GB. At present, the method to improve the power of EML integrated devices is mainly to reduce the light reflection between DFB and EAM. At the same time, the lateral buried confinement process is used to reduce the current leakage of DFB and increase the optical field coupling between DFB and EAM.
[0004] There are many ways to realize EML laser, the most commonly used are SAG and Butt-joint growth methods. SAG is the selective area epitaxial growth process, which uses a SiO2 mask to achieve the difference in MQW thickness between the DFB area and the EA area, so that their light-emitting wavelengths are different, and the modulation of the DFB light by the EA is realized. The advantages are simple process and no light reflection between the DFB and EA. Butt-joint is the heterogeneous coupling epitaxial growth process, which first grows the DFB area, then etches away the non-luminous area, and grows the EA area butt-jointly on the light-emitting surface of the DFB area to realize the modulation of the DFB light by the EA. The advantages are that the EA and DFB can be designed and grown in a distributed manner, and the EML characteristics are good. The disadvantages are that the process is complicated and there is an electrical isolation area between the EA and the DFB. The material of the electrical isolation area is low-refractive-index InP (its refractive index is 3.221, which is quite different from the refractive index of the DFB light-emitting area of 3.55). Therefore, when the light is transmitted from the DFB area to the EA area, obvious light reflection will occur, and the reflected light will coherently superimpose (interference destructive or interference subtraction) with the light in the DFB area, which will affect the lasing mode of the light in the DFB area.
[0005] The reflected light signal will interfere with the laser state of the distributed feedback (DFB) laser, resulting in unnecessary power fluctuations and large chirp of the output signal under modulation. At the same time, this light reflection will also cause large peaks and valleys in the frequency response, reducing the signal quality. In the prior art, M. Aoki et al. reduced the reflectivity of the output facet to less than ~2×10 -4 To reduce the chirp caused by facet reflection (i.e. DFB chirp) (M. Aoki, S. Takashima, Y. Fujiwara and S. Aoki, "New transmission simulation of EA-modulator integrated DFB-lasers considering the facetreflection-induced chirp", IEEE Photon. Technol. Lett., vol. 9, pp. 380-382, Mar. 1997.), however, the implementation of this technology requires high-precision coating equipment, and the operation is complex and difficult. Summary of the invention
[0006] The purpose of the present invention is to provide an electro-absorption modulated semiconductor laser and its preparation method and application. The electro-absorption modulated semiconductor laser obtained by the present invention has good optical performance, stable light emission mode, light-current-voltage curve without kink and mode hopping, and simple process and easy to realize.
[0007] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0008] The present invention provides an electro-absorption modulated semiconductor laser, which includes a DFB light emitting area and an EA electro-absorption modulation area arranged in sequence along the horizontal direction;
[0009] The DFB light emitting area includes a first functional layer, a quantum well layer, a second functional layer, a grating layer and a third functional layer arranged in sequence along the vertical direction; the grating layer includes an L1 area grating close to the EA electro-absorption modulation area and an L2 area grating far from the EA electro-absorption modulation area;
[0010] The length ratio of the L1 region grating to the L2 region grating is 60-80:200-500; the coupling coefficient of the L1 region grating is not less than 1.2 times the coupling coefficient of the L2 region grating.
[0011] Preferably, the first functional layer includes an InP substrate 1, a first InP buffer layer 2, a lower confinement layer 3 and a lower waveguide layer 4 arranged in sequence along the vertical direction, and the lower waveguide layer 4 is in contact with the quantum well layer;
[0012] The quantum well layer is an MQW quantum well active layer 5;
[0013] The second functional layer includes an upper waveguide layer 6, an upper confinement layer 7, a first InP cap 8 and a second InP buffer layer 10 arranged in sequence along the vertical direction, the upper waveguide layer 6 is in contact with the quantum well layer, and the second InP buffer layer 10 is in contact with the grating layer;
[0014] The grating layer is an InGaAsP grating layer 11;
[0015] The third functional layer includes a second InP cap layer 12, a third InP buffer layer 14, an MQW quantum well layer 15, a third InP cap layer 16, an InP confinement layer 17, an InGaAsP barrier transition layer 18 and an InGaAs ohmic contact layer arranged in sequence along the vertical direction, and the second InP cap layer 12 is in contact with the grating layer.
[0016] Preferably, the lower confinement layer 3 is an InGaAsP lower confinement layer; the lower waveguide layer 4 is an InGaAsP lower waveguide layer; the MQW quantum well active layer 5 is an MQW InGaAsP quantum well structure layer; the upper waveguide layer 6 is an InGaAsP upper waveguide layer; and the upper confinement layer 7 is an InGaAsP upper confinement layer.
[0017] Preferably, the thickness of the first InP buffer layer 2 is 500nm, the thickness of the lower confinement layer 3 is 30nm, the thickness of the lower waveguide layer 4 is 30nm, the thickness of the upper waveguide layer 6 is 30nm, the thickness of the upper confinement layer 7 is 30nm, and the thickness of the first InP cap layer 8 is 15nm.
[0018] Preferably, the MQW quantum well active layer 5 is composed of 10 pairs of quantum wells, and the thickness of the barrier layer of each pair of quantum wells is 10 nm, and the thickness of the well layer is 5 nm.
[0019] Preferably, the thickness of the second InP buffer layer 10 is 100 nm, the thickness of the InGaAsP grating layer 11 is 20 nm, and the thickness of the second InP cap layer 12 is 15 nm;
[0020] The thickness of the third InP buffer layer 14 is 10 nm, and the thickness of the third InP cap layer 16 is 100 nm;
[0021] The MQW quantum well layer 15 is composed of 10 pairs of MQWs, the barrier layer thickness of each pair of MQWs is 5nm, and the well layer thickness is 10nm; the height difference between the quantum well of the MQW quantum well layer 15 and the quantum well of the MQW quantum well active layer 5 in the vertical direction is less than 30nm;
[0022] The thickness of the InP limiting layer 17 is 1500 nm, the thickness of the InGaAsP barrier transition layer 18 is 50 nm, and the thickness of the InGaAs ohmic contact layer 19 is 200 nm.
[0023] The present invention provides a method for preparing the electro-absorption modulated semiconductor laser described in the above technical solution, comprising the following steps:
[0024] The first functional layer, the quantum well layer, the second functional layer, the grating layer and the third functional layer are sequentially grown in a stacked manner along the vertical direction to obtain the electro-absorption modulated semiconductor laser.
[0025] Preferably, the preparation method comprises the following steps:
[0026] A first InP buffer layer 2, a lower confinement layer 3, a lower waveguide layer 4, an MQW quantum well active layer 5, an upper waveguide layer 6, an upper confinement layer 7 and a first InP cap layer 8 are sequentially grown on the upper surface of the InP substrate 1 to form a first device on the InP substrate 1;
[0027] Depositing a first SiO2 film 9 on the upper surface of the first device, and sequentially performing a first photolithography and a first etching to remove a portion of the first SiO2 film 9 and retaining a portion of the first SiO2 film 9 in the region where the grating of the L1 region is located, so as to form a second device on the InP substrate 1;
[0028] A second InP buffer layer 10, an InGaAsP grating layer 11 and a second InP cap layer 12 are sequentially grown on the upper surface of the second device to form a third device on the InP substrate 1;
[0029] The remaining first SiO2 film 9 on the third device is removed, and a second SiO2 film 13 is deposited on the upper surface of the area where the DFB light emitting area is located, and then a second photolithography and a second etching are performed in sequence to expose the InP substrate 1 in the area where the EA electro-absorption modulation area is located, so as to form a table for growing the EA area on the InP substrate 1;
[0030] A third InP buffer layer 14, an MQW quantum well layer 15 and a third InP cap layer 16 are sequentially grown on the terrace of the growth EA region to form a fourth device on the InP substrate 1;
[0031] The second SiO2 film 13 is removed, and an InP confinement layer 17, an InGaAsP barrier transition layer 18 and an InGaAs ohmic contact layer 19 are sequentially grown on the upper surfaces of the third device and the fourth device to obtain the electro-absorption modulated semiconductor laser.
[0032] Preferably, the growth of the first InP buffer layer 2, the lower confinement layer 3, the lower waveguide layer 4, the MQW quantum well active layer 5, the upper waveguide layer 6, the upper confinement layer 7, the first InP cap layer 8, the second InP buffer layer 10, the InGaAsP grating layer 11, the second InP cap layer 12, the third InP buffer layer 14, the MQW quantum well layer 15, the third InP cap layer 16, the InP confinement layer 17, the InGaAsP barrier transition layer 18 and the InGaAs ohmic contact layer is carried out in an MOCVD system, the reaction chamber pressure is 60 mbar, the growth temperature is 700°C, and the carrier gas is H2.
[0033] The present invention provides the application of the electro-absorption modulated semiconductor laser described in the above technical solution or the electro-absorption modulated semiconductor laser obtained by the above preparation method in a high-speed optical communication chip.
[0034] The present invention provides an electro-absorption modulated semiconductor laser, which includes a DFB light-emitting area and an EA electro-absorption modulation area arranged in sequence in the horizontal direction; the DFB light-emitting area includes a first functional layer, a quantum well layer, a second functional layer, a grating layer and a third functional layer arranged in sequence in the vertical direction; the grating layer includes an L1 area grating close to the EA electro-absorption modulation area and an L2 area grating far away from the EA electro-absorption modulation area; the length ratio of the L1 area grating to the L2 area grating is 60-80:200-500; the coupling coefficient of the L1 area grating is not less than 1.2 times the coupling coefficient of the L2 area grating. The present invention adopts a two-segment grating design, the L1 area grating is short, the L2 area grating is long, and the optical coupling coefficient kappa of the L1 area grating is greater than 1.2 times that of the L2 area grating. After such a design, the light reflected back by the L2 area grating will be reflected back by the L1 area grating, and will not affect the mode of the laser. The light emission mode of the electro-absorption modulated semiconductor laser of the present invention is stable, and the light-current-voltage (Light-Current-Voltage) curve has no kink and no mode hopping.
[0035] The present invention also provides a method for preparing the electro-absorption modulated semiconductor laser. The present invention adopts the SAG method to grow the grating layer of the laser, so that the grating thickness of the L1 region is 22-78% thicker than the grating thickness of the L2 region. After being made into a grating, the optical coupling coefficient kappa of the L1 region is greater than 1.2 times that of the L2 region. The preparation method provided by the present invention has the advantages of simple process and easy implementation, and the electro-absorption modulated semiconductor laser obtained thereby has good optical performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0037] Figure 1 It is a schematic diagram of the structure of the EML laser;
[0038] Figure 2 Schematic diagram of the DFB light emitting area of the EML laser;
[0039] Figure 3 Schematic diagram of the shape of SiO2 film before growth in L1 region;
[0040] Figure 4 It is a cross-sectional schematic diagram of a device obtained by a single epitaxial growth;
[0041] Figure 5 It is a cross-sectional schematic diagram of a device obtained by three-step epitaxial growth;
[0042] Figure 6 is a schematic cross-sectional view of the device obtained after forming a terrace in the EA region;
[0043] Figure 7 It is a schematic cross-sectional view of a device obtained by four times of epitaxial growth;
[0044] Figure 8 is a schematic cross-sectional view of a device obtained by five epitaxial growths;
[0045] Fig. 9 is the LIV curve of EML laser;
[0046] Fig.10 It is the EA curve diagram of EML laser;
[0047] Among them, 1-InP substrate; 2-first InP buffer layer; 3-InGaAsP lower confinement layer; 4-InGaAsP lower waveguide layer; 5-InGaAsP MQW quantum well active layer; 6-InGaAsP upper waveguide layer; 7-InGaAsP upper confinement layer; 8-first InP cap layer; 9-first SiO2 film; 10-second InP buffer layer; 11-InGaAsP grating layer; 12-second InP cap layer; 13-second SiO2 film; 14-third InP buffer layer; 15-InGaAsP MQW quantum well layer; 16-third InP cap layer; 17-InP confinement layer; 18-InGaAsP barrier transition layer; 19-InGaAs ohmic contact layer. DETAILED DESCRIPTION
[0048] The present invention provides an electro-absorption modulated semiconductor laser, which includes a DFB light emitting area and an EA electro-absorption modulation area arranged in sequence along the horizontal direction;
[0049] The DFB light emitting area includes a first functional layer, a quantum well layer, a second functional layer, a grating layer and a third functional layer arranged in sequence along the vertical direction; the grating layer includes an L1 area grating close to the EA electro-absorption modulation area and an L2 area grating far from the EA electro-absorption modulation area;
[0050] The length ratio of the L1 region grating to the L2 region grating is 60-80:200-500; the coupling coefficient of the L1 region grating is not less than 1.2 times the coupling coefficient of the L2 region grating. In an embodiment of the present invention, the coupling coefficient of the L1 region grating is 1.22 times the coupling coefficient of the L2 region grating.
[0051] In the present invention, the first functional layer preferably includes an InP substrate 1, a first InP buffer layer 2, a lower confinement layer 3 and a lower waveguide layer 4 arranged in sequence along the vertical direction;
[0052] The quantum well layer is preferably an MQW quantum well active layer 5;
[0053] The second functional layer preferably includes an upper waveguide layer 6, an upper confinement layer 7, a first InP cap layer 8 and a second InP buffer layer 10 arranged in sequence along the vertical direction;
[0054] The grating layer is preferably an InGaAsP grating layer 11;
[0055] The third functional layer preferably includes a second InP cap layer 12, a third InP buffer layer 14, an MQW quantum well layer 15, a third InP cap layer 16, an InP confinement layer 17, an InGaAsP barrier transition layer 18 and an InGaAs ohmic contact layer 19 arranged in sequence along the vertical direction.
[0056] In the present invention, the InP substrate 1 is preferably an N-type InP substrate. In an embodiment of the present invention, the InP substrate 1 has a carrier concentration of 3×10 18 cm -3 N-type InP substrate.
[0057] In the present invention, the thickness of the first InP buffer layer 2 is preferably 500 nm. The growth of the first InP buffer layer 2 of the present invention is preferably carried out in an MOCVD system; the reaction chamber pressure is preferably 60 mbar; the growth temperature is preferably 700°C; the carrier gas is preferably H2; and the reaction source gas is preferably trimethylindium and phosphine.
[0058] In the present invention, the lower confinement layer 3 is preferably an InGaAsP lower confinement layer, and the thickness of the lower confinement layer 3 is preferably 30 nm. The growth of the lower confinement layer 3 of the present invention is preferably carried out in an MOCVD system; the reaction chamber pressure is preferably 60 mbar; and the reaction source gas is preferably trimethyl indium, diethyl gallium, arsine and phosphine.
[0059] In the present invention, the lower waveguide layer 4 is preferably an InGaAsP lower waveguide layer, and the thickness of the lower waveguide layer 4 is preferably 30 nm. The growth of the lower waveguide layer 4 in the present invention is preferably carried out in an MOCVD system; the reaction chamber pressure is preferably 60 mbar; and the reaction source gas is preferably trimethyl indium, diethyl gallium, arsine and phosphine.
[0060] In the present invention, the MQW quantum well active layer 5 is preferably an InGaAsP MQW quantum well structure layer. The MQW quantum well active layer 5 of the present invention is preferably composed of 10 pairs of quantum wells; the thickness of the barrier layer of each pair of quantum wells is preferably 10nm; the thickness of the well layer is preferably 5nm. The growth of the MQW quantum well active layer 5 of the present invention is preferably carried out in an MOCVD system; the reaction chamber pressure is preferably 60mbar; the reaction source gas is preferably trimethylindium, diethylgallium, arsine and phosphine.
[0061] In the present invention, the upper waveguide layer 6 is preferably an InGaAsP upper waveguide layer, and the thickness of the upper waveguide layer 6 is preferably 30 nm. The growth of the upper waveguide layer 6 in the present invention is preferably carried out in an MOCVD system; the reaction chamber pressure is preferably 60 mbar; and the reaction source gas is preferably trimethyl indium, diethyl gallium, arsine and phosphine.
[0062] In the present invention, the upper confinement layer 7 is preferably an InGaAsP upper confinement layer, and the thickness of the upper confinement layer 7 is preferably 30 nm. The growth of the upper confinement layer 7 of the present invention is preferably carried out in an MOCVD system; the reaction chamber pressure is preferably 60 mbar; and the reaction source gas is preferably trimethyl indium, diethyl gallium, arsine and phosphine.
[0063] In the present invention, the thickness of the first InP cap layer 8 is preferably 15 nm. The growth of the first InP cap layer 8 of the present invention is preferably carried out in an MOCVD system; the reaction chamber pressure is preferably 60 mbar; the growth temperature is preferably 700°C; the carrier gas is preferably H2; and the reaction source gas is preferably trimethylindium and phosphine.
[0064] In the present invention, the thickness of the second InP buffer layer 10 is preferably 100 nm. The growth of the second InP buffer layer 10 of the present invention is preferably carried out in an MOCVD system; the reaction chamber pressure is preferably 60 mbar; the growth temperature is preferably 700°C; the carrier gas is preferably H2; and the reaction source gas is preferably trimethylindium and phosphine.
[0065] In the present invention, the thickness of the InGaAsP grating layer 11 is preferably 20 nm. The InGaAsP grating layer 11 of the present invention is preferably grown in a MOCVD system; the reaction chamber pressure is preferably 60 mbar; and the reaction source gas is preferably trimethylindium, diethylgallium, arsine and phosphine.
[0066] In the present invention, the thickness of the second InP cap layer 12 is preferably 15 nm. The growth of the second InP cap layer 12 of the present invention is preferably carried out in a MOCVD system; the reaction chamber pressure is preferably 60 mbar; the growth temperature is preferably 700°C; the carrier gas is preferably H2; and the reaction source gas is preferably trimethylindium and phosphine.
[0067] In the present invention, the thickness of the third InP buffer layer 14 is preferably 10 nm. The growth of the third InP buffer layer 14 of the present invention is preferably carried out in a MOCVD system; the reaction chamber pressure is preferably 60 mbar; the growth temperature is preferably 700°C; the carrier gas is preferably H2; and the reaction source gas is preferably trimethylindium and phosphine.
[0068] In the present invention, the MQW quantum well layer 15 is preferably an InGaAsP MQW quantum well layer. The MQW quantum well layer 15 of the present invention is preferably composed of 10 pairs of MQWs; the barrier layer and the well layer of the MQW in the MQW quantum well layer 15 grow alternately; the thickness of the barrier layer of each pair of the MQW is preferably 5nm; the thickness of the well layer is preferably 10nm. The height difference between the quantum well of the MQW quantum well layer 15 of the present invention and the quantum well of the MQW quantum well active layer 5 in the vertical direction is preferably less than 30nm. The growth of the MQW quantum well layer 15 of the present invention is preferably carried out in an MOCVD system; the reaction chamber pressure is preferably 60mbar; the reaction source gas is preferably trimethylindium, diethylgallium, arsine and phosphine.
[0069] In the present invention, the thickness of the third InP cap layer 16 is preferably 100 nm. The growth of the third InP cap layer 16 of the present invention is preferably carried out in a MOCVD system; the reaction chamber pressure is preferably 60 mbar; the growth temperature is preferably 700°C; the carrier gas is preferably H2; and the reaction source gas is preferably trimethylindium and phosphine.
[0070] In the present invention, the thickness of the InP confinement layer 17 is preferably 1500 nm. The growth of the InP confinement layer 17 of the present invention is preferably carried out in a MOCVD system; the reaction chamber pressure is preferably 60 mbar; the growth temperature is preferably 700°C; the carrier gas is preferably H2; and the reaction source gas is preferably trimethylindium and phosphine.
[0071] In the present invention, the thickness of the InGaAsP barrier transition layer 18 is preferably 50 nm. The growth of the InGaAsP barrier transition layer 18 is preferably carried out in a MOCVD system; the reaction chamber pressure is preferably 60 mbar; and the reaction source gas is preferably trimethylindium, diethylgallium, arsine and phosphine.
[0072] In the present invention, the thickness of the InGaAs ohmic contact layer 19 is preferably 200 nm. The growth of the InGaAs ohmic contact layer 19 is preferably carried out in a MOCVD system; the reaction chamber pressure is preferably 60 mbar; and the reaction source gas is preferably trimethylindium, diethylgallium, arsine and phosphine.
[0073] In the electro-absorption modulated semiconductor laser of the present invention, the length ratio of the L1 region grating to the L2 region grating is 60-80:200-500, preferably 70:250-350, and more preferably 70:280.
[0074] The present invention also provides a method for preparing the electro-absorption modulated semiconductor laser described in the above technical solution, comprising the following steps: growing a first functional layer, a quantum well layer, a second functional layer, a grating layer and a third functional layer in sequence in a vertical direction to obtain the electro-absorption modulated semiconductor laser.
[0075] The method for preparing an absorption modulated semiconductor laser of the present invention preferably comprises the following steps:
[0076] A first InP buffer layer 2, a lower confinement layer 3, a lower waveguide layer 4, an MQW quantum well active layer 5, an upper waveguide layer 6, an upper confinement layer 7 and a first InP cap layer 8 are sequentially grown on the upper surface of the InP substrate 1 to form a first device on the InP substrate 1;
[0077] Depositing a first SiO2 film 9 on the upper surface of the first device, and sequentially performing a first photolithography and a first etching to remove a portion of the first SiO2 film 9 and retaining a portion of the first SiO2 film 9 in the region where the grating of the L1 region is located, so as to form a second device on the InP substrate 1;
[0078] A second InP buffer layer 10, an InGaAsP grating layer 11 and a second InP cap layer 12 are sequentially grown on the upper surface of the second device to form a third device on the InP substrate 1;
[0079] The remaining first SiO2 film 9 is removed, and a second SiO2 film 13 is deposited on the upper surface of the area where the DFB light emitting area is located, and then a second photolithography and a second etching are performed in sequence to expose the InP substrate 1 in the area where the EA electro-absorption modulation area is located, so as to form a table of the EA area on the InP substrate 1;
[0080] A third InP buffer layer 14, an MQW quantum well layer 15 and a third InP cap layer 16 are sequentially grown on the terrace of the growth EA region to form a fourth device on the InP substrate 1;
[0081] The second SiO2 film 13 is removed, and an InP confinement layer 17, an InGaAsP barrier transition layer 18 and an InGaAs ohmic contact layer 19 are sequentially grown on the upper surfaces of the third device and the fourth device to obtain the electro-absorption modulated semiconductor laser.
[0082] In the present invention, unless otherwise specified, the raw materials used are commercially available products well known to those skilled in the art or are prepared by methods well known to those skilled in the art.
[0083] In the present invention, the thickness of the first SiO2 film 9 is preferably 100 nm. The first photolithography and the first etching of the present invention adopt conventional techniques in the art.
[0084] In the present invention, the thickness of the second SiO2 film 13 is preferably 100 nm. The second photolithography and the second etching of the present invention adopt conventional techniques in the art.
[0085] In the present invention, the thickness of the third SiO2 film 20 is preferably 100 nm. The third photolithography and the third etching of the present invention adopt conventional techniques in the art.
[0086] The present invention also provides the application of the electro-absorption modulated semiconductor laser described in the above technical solution or the electro-absorption modulated semiconductor laser obtained by the above preparation method in a high-speed optical communication chip.
[0087] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0088] The InP substrate 1 used in the embodiment has a carrier concentration of 3×10 18 cm -3 N-type InP substrate;
[0089] The instrument used in the embodiment is an MOCVD device from Aixtron, the reaction chamber pressure is 60 mbar, the growth temperature is 700°C, H2 is used as the carrier gas, and trimethylindium (TMIn), diethylgallium (TEGa), trimethylaluminum (TMAl), silane (SiH4), trimethylarsenic (TMAs), arsine (AsH3) and phosphine (PH3) are used as reaction source gases.
[0090] Figure 1 Schematic diagram of the EML laser structure. Figure 2 Schematic diagram of the DFB light-emitting area of the EML laser. Figure 3 Schematic diagram of the shape of the SiO2 film before growth in the L1 region.
[0091] Example 1
[0092] This embodiment provides an EML laser, which includes a DFB light-emitting area and an EA electro-absorption modulation area arranged in sequence along the horizontal direction; the DFB light-emitting area includes a first functional layer, a quantum well layer, a second functional layer, a grating layer and a third functional layer arranged in sequence along the vertical direction; the grating layer includes an L1 area grating close to the EA electro-absorption modulation area and an L2 area grating far from the EA electro-absorption modulation area, the length of the L1 area grating is 70 μm; the length of the L2 area grating is 280 μm; the coupling coefficient of the L1 area grating is not less than 1.22 times the coupling coefficient of the L2 area grating;
[0093] The first functional layer includes an InP substrate 1, a first InP buffer layer 2, an InGaAsP lower confinement layer 3 and an InGaAsP lower waveguide layer 4 arranged in sequence along the vertical direction, and the lower waveguide layer 4 is in contact with the quantum well layer;
[0094] The quantum well layer is an InGaAsP MQW quantum well active layer 5;
[0095] The second functional layer includes an InGaAsP upper waveguide layer 6, an InGaAsP upper confinement layer 7, a first InP cap layer 8 and a second InP buffer layer 10 arranged in sequence along the vertical direction, the upper waveguide layer 6 is in contact with the quantum well layer, and the second InP buffer layer 10 is in contact with the grating layer;
[0096] The grating layer is an InGaAsP grating layer 11;
[0097] The third functional layer includes a second InP cap layer 12, a third InP buffer layer 14, an InGaAsP MQW quantum well layer 15, a third InP cap layer 16, an InP confinement layer 17, an InGaAsP barrier transition layer 18 and an InGaAs ohmic contact layer 19 arranged in sequence along the vertical direction, and the second InP cap layer 12 is in contact with the grating layer.
[0098] The preparation method of the EML laser is as follows:
[0099] Step 1: If Figure 4 As shown, an InP substrate is placed in an MOCVD device, and a first InP buffer layer 2, an InGaAsP lower confinement layer 3, an InGaAsP lower waveguide layer 4, an InGaAsPMMQW quantum well active layer 5, an InGaAsP upper waveguide layer 6, an InGaAsP upper confinement layer 7 and a first InP cap layer 8 are sequentially stacked and grown on the upper surface of the InP substrate 1 in a vertical direction to obtain a first device on the InP substrate 1 and realize a single epitaxial growth; wherein the thickness of the first InP buffer layer 2 is 500nm, the thickness of the InGaAsP lower confinement layer 3 is 30nm, the thickness of the InGaAsP lower waveguide layer 4 is 30nm, the thickness of the InGaAsP upper waveguide layer 6 is 30nm, the thickness of the InGaAsP upper confinement layer 7 is 30nm, and the thickness of the first InP cap layer 8 is 15nm; the InGaAsP MQW quantum well active layer 5 consists of 10 pairs of quantum wells, the thickness of the barrier layer of each pair of the quantum wells is 10nm, and the thickness of the well layer is 5nm.
[0100] Step 2: Use alignment marks to define the DFB region and the EA region, and divide the DFB region into the L1 region and the L2 region in the horizontal direction, wherein the L1 region is far away from the EA region and has a length of 70 μm; the L2 region is close to the EA region and has a length of 280 μm. A first SiO2 film 9 with a thickness of 100 nm is deposited on the upper surface of the first device, and then a photolithography and etching process are performed in sequence to remove part of the first SiO2 film 9 and retain part of the first SiO2 film 9 on the surface of the region where the L1 region is located. The remaining first SiO2 film 9 after etching is used as a SiO2 mask layer. The SiO2 mask layer is formed by two trapezoidal regions, each of which has a short side of 30 μm, a long side of 100 μm, a trapezoidal height of 50 μm, and a distance of 35 μm between the two trapezoidal regions, i.e., a second device is obtained on the InP substrate 1.
[0101] Step 3: If Figure 5 As shown, a second InP buffer layer 10 and an InGaAsP grating layer 11 are sequentially grown on the upper surface of the second device to achieve secondary epitaxial growth; an InP cap layer 12 is then grown on the upper surface of the obtained device to achieve tertiary epitaxial growth, so as to obtain a third device on the InP substrate 1, wherein the thickness of the second InP buffer layer 10 is 100nm, the thickness of the InGaAsP grating layer 11 is 20nm, and the thickness of the second InP cap layer 12 is 15nm; and the thickness of the film layer between two adjacent trapezoidal regions is 23% thicker than that in other regions.
[0102] Step 4: Figure 6 As shown, the remaining first SiO2 film 9 on the third device is removed by etching, and then a second SiO2 film 13 with a thickness of 100 nm is deposited on the upper surface of the area where the DFB light-emitting area is located, and then photolithography and etching are performed in sequence to expose the InP substrate 1 in the area where the EA electro-absorption modulation area is located, so as to form a table for growing the EA area on the InP substrate 1.
[0103] Step 5: Figure 7 As shown, a third InP buffer layer 14, an InGaAsPMMQW quantum well layer 15 and a third InP cap layer 16 are sequentially stacked and grown on the terrace of the growth EA region to obtain a fourth device on the InP substrate 1, thereby realizing four epitaxial growths, wherein the thickness of the third InP buffer layer 14 is 10 nm, and the thickness of the third InP cap layer 16 is 100 nm; the InGaAsP MQW quantum well layer 15 is composed of 10 pairs of MQWs, and the thickness of the barrier layer of each pair of MQWs is 5 nm, and the thickness of the well layer is 10 nm, and the height difference between the quantum well of the InGaAsP MQW quantum well layer 15 and the quantum well of the MQW quantum well active layer 5 in the vertical direction is less than 30 nm.
[0104] Step 6: Figure 8As shown, the second SiO2 film 13 is removed by etching, and an InP confinement layer 17, an InGaAsP barrier transition layer 18 and an InGaAs ohmic contact layer 19 are sequentially stacked and grown on the upper surfaces of the third device and the fourth device to obtain a fifth device on the InP substrate 1, realizing five epitaxial growths, wherein the thickness of the InP confinement layer 17 is 1500nm, the thickness of the InGaAsP barrier transition layer 18 is 50nm, and the thickness of the InGaAs ohmic contact layer 19 is 200nm, thereby obtaining the electro-absorption modulated semiconductor laser (EML laser).
[0105] The EML laser was tested at 45°C and 100 mA. Fig. 9 and Fig.10 As shown, it can be seen that the LIV of the EML laser has no kink and mode hopping phenomenon.
[0106] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. An electro-absorption modulated semiconductor laser, characterized in that: The horizontal direction includes a DFB light emitting area and an EA electro-absorption modulation area arranged in sequence; The DFB light emitting area includes a first functional layer, a quantum well layer, a second functional layer, a grating layer and a third functional layer arranged in sequence along the vertical direction; the grating layer includes an L1 area grating close to the EA electro-absorption modulation area and an L2 area grating far from the EA electro-absorption modulation area; The length ratio of the L1 region grating to the L2 region grating is 60-80:200-500; the coupling coefficient of the L1 region grating is not less than 1.2 times the coupling coefficient of the L2 region grating.
2. The electro-absorption modulated semiconductor laser according to claim 1, characterized in that: The first functional layer comprises an InP substrate (1), a first InP buffer layer (2), a lower confinement layer (3) and a lower waveguide layer (4) arranged in sequence along the vertical direction, and the lower waveguide layer (4) is in contact with the quantum well layer; The quantum well layer is an MQW quantum well active layer (5); The second functional layer comprises an upper waveguide layer (6), an upper confinement layer (7), a first InP cap layer (8) and a second InP buffer layer (10) arranged in sequence along the vertical direction, the upper waveguide layer (6) is in contact with the quantum well layer, and the second InP buffer layer (10) is in contact with the grating layer; The grating layer is an InGaAsP grating layer (11); The third functional layer comprises, in a vertical direction, a second InP cap layer (12), a third InP buffer layer (14), an MQW quantum well layer (15), a third InP cap layer (16), an InP confinement layer (17), an InGaAsP barrier transition layer (18) and an InGaAs ohmic contact layer (19), which are arranged in sequence; the second InP cap layer (12) is in contact with the grating layer.
3. The electro-absorption modulated semiconductor laser according to claim 2, characterized in that: The lower limiting layer (3) is an InGaAsP lower limiting layer; the lower waveguide layer (4) is an InGaAsP lower waveguide layer; the MQW quantum well active layer (5) is an InGaAsP MQW quantum well structure layer; the upper waveguide layer (6) is an InGaAsP upper waveguide layer; and the upper limiting layer (7) is an InGaAsP upper limiting layer.
4. The electro-absorption modulated semiconductor laser according to claim 2 or 3, characterized in that: The thickness of the first InP buffer layer (2) is 500 nm, the thickness of the lower limiting layer (3) is 30 nm, the thickness of the lower waveguide layer (4) is 30 nm, the thickness of the upper waveguide layer (6) is 30 nm, the thickness of the upper limiting layer (7) is 30 nm, and the thickness of the second InP cap layer (8) is 15 nm.
5. The electro-absorption modulated semiconductor laser according to claim 2, characterized in that: The MQW quantum well active layer (5) consists of 10 pairs of quantum wells, the barrier layer of each pair of quantum wells has a thickness of 10 nm, and the well layer has a thickness of 5 nm.
6. The electro-absorption modulated semiconductor laser according to claim 2, characterized in that: The thickness of the second InP buffer layer (10) is 100 nm, the thickness of the InGaAsP grating layer (11) is 20 nm, and the thickness of the second InP cap layer (12) is 15 nm; The thickness of the third InP buffer layer (14) is 10 nm, and the thickness of the third InP cap layer (16) is 100 nm; The MQW quantum well layer (15) is composed of 10 pairs of MQWs, the barrier layer of each pair of MQWs has a thickness of 5 nm, and the well layer has a thickness of 10 nm; the height difference between the quantum well of the MQW quantum well layer (15) and the quantum well of the MQW quantum well active layer (5) in the vertical direction is less than 30 nm; The thickness of the InP limiting layer (17) is 1500 nm, the thickness of the InGaAsP barrier transition layer (18) is 50 nm, and the thickness of the InGaAs ohmic contact layer (19) is 200 nm.
7. The method for preparing the electro-absorption modulated semiconductor laser according to any one of claims 1 to 6, comprising the following steps: The first functional layer, the quantum well layer, the second functional layer, the grating layer and the third functional layer are sequentially stacked and grown in a vertical direction to obtain the electro-absorption modulated semiconductor laser.
8. The preparation method according to claim 7, characterized in that: The following steps are involved: A first InP buffer layer (2), a lower confinement layer (3), a lower waveguide layer (4), an MQW quantum well active layer (5), an upper waveguide layer (6), an upper confinement layer (7) and a first InP cap layer (8) are sequentially grown on the upper surface of an InP substrate (1) to form a first device on the InP substrate (1); Depositing a first SiO2 film (9) on the upper surface of the first device, and sequentially performing first photolithography and first etching to remove a portion of the first SiO2 film (9) and retain a portion of the first SiO2 film (9) in the region where the L1 region grating is located, so as to form a second device on the InP substrate (1); A second InP buffer layer (10), a grating layer (11) and a second InP cap layer (12) are sequentially grown on the upper surface of the second device to form a third device on the InP substrate (1); Removing the remaining first SiO2 film (9) on the third device, depositing a second SiO2 film (13) on the upper surface of the region where the DFB light emitting region is located, and then sequentially performing a second photolithography and a second etching to expose the InP substrate (1) in the region where the EA electro-absorption modulation region is located, so as to form a table on the InP substrate (1) for growing the EA region; A third InP buffer layer (14), an MQW quantum well layer (15) and a third InP cap layer (16) are sequentially grown on the terrace of the growth EA region to form a fourth device on the InP substrate (1); The second SiO2 film (13) is removed, and an InP limiting layer (17), an InGaAsP barrier transition layer (18) and an InGaAs ohmic contact layer (19) are sequentially grown on the upper surfaces of the third device and the fourth device to obtain the electro-absorption modulated semiconductor laser.
9. The preparation method according to claim 8, characterized in that: The growth of the first InP buffer layer (2), the lower confinement layer (3), the lower waveguide layer (4), the MQW quantum well active layer (5), the upper waveguide layer (6), the upper confinement layer (7), the first InP cap layer (8), the second InP buffer layer (10), the InGaAsP grating layer (11), the second InP cap layer (12), the third InP buffer layer (14), the MQW quantum well layer (15), the third InP cap layer (16), the InP confinement layer (17), the InGaAsP barrier transition layer (18) and the InGaAs ohmic contact layer (19) is carried out in an MOCVD system, the reaction chamber pressure is 60 mbar, the growth temperature is 700°C, and the carrier gas is H2.
10. Use of the electro-absorption modulated semiconductor laser according to any one of claims 1 to 6 or the electro-absorption modulated semiconductor laser prepared by the preparation method according to any one of claims 7 to 9 in high-speed optical communication chips.
Citation Information
Patent Citations
Electro-absorption modulated laser chip and preparation method thereof
CN116995530A
Electro-absorption modulated laser and preparation method thereof
CN117154541A
Compound semiconductor device and its manufacturing method
JP2003174224A
Distributed feedback type semiconductor laser device
JP2004023035A
Optical semiconductor device
US20130208751A1