Preparation method of LTCC (Low Temperature Co-Fired Ceramic) substrate embedded solid metal wall shielding structure

By preparing a buried solid metal wall shielding structure on the LTCC substrate, the problem of high-frequency microwave signal isolation cannot be achieved in the prior art, the isolation effect of the radio frequency channel inside the substrate is improved, and compatible with conventional LTCC processes, suitable for complex circuits application.

CN118921890APending Publication Date: 2024-11-08SOUTHWEST CHINA RES INST OF ELECTRONICS EQUIP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410928735.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The prior art is difficult to achieve effective electromagnetic isolation of high-frequency microwave signals inside the LTCC substrate, and traditional methods cannot bury the solid metal wall shielding structure, and occupy wiring space, limiting the integrated density and isolation effect of the substrate.

Method used

Using raw ceramic micro-slit processing, overall coating protection, metal paste filling, film defiling and leveling, lamination and lamination, etc., the internal buried solid metal wall shielding structure is formed through the LTCC low-temperature co-fired ceramic process to achieve high-frequency microwave Good isolation of signals.

Benefits of technology

High isolation between adjacent radio frequency channels inside the LTCC substrate is achieved, especially in the high frequency band, and the process is compatible with conventional LTCC and is easy to apply in complex circuits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118921890A_ABST
    Figure CN118921890A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a solid metal wall shielding structure embedded in an LTCC substrate. The preparation method comprises the following steps: raw ceramic micro-gap processing: preparing a micro-gap required by the solid metal wall shielding structure on raw ceramic; performing overall film covering protection on the raw ceramic: performing overall film covering protection on the raw ceramic with the micro-gaps; micro-gap slurry filling: performing metal slurry filling on the micro-gaps in the raw ceramic; demolding the raw ceramic: demolding the multiple layers of raw ceramic, and flattening the redundant metal slurry; stacking and laminating raw ceramic: stacking multiple layers of raw ceramic through an LTCC conventional process, and laminating in a warm water isostatic pressing mode to form an LTCC circuit blank with an embedded solid metal wall shielding structure; and sintering the circuit blank: co-firing the LTCC circuit blank to finally form the LTCC circuit substrate with the embedded solid metal wall shielding structure. According to the invention, the isolation degree between the adjacent radio frequency channels in the substrate, especially at a high frequency band, can be greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of LTCC circuit substrate manufacturing, and in particular to a method for preparing a solid metal wall shielding structure embedded in an LTCC substrate. Background Art

[0002] LTCC (low temperature co-fired ceramic) has the characteristics of high density integration, good airtight packaging characteristics, and excellent high-frequency performance. It is widely used in the field of microwave / millimeter wave communications. However, with the increasing development of miniaturization, high frequency, broadband, and high performance in the field of communications, the physical distance between RF channels is getting smaller and smaller, the operating frequency is getting higher and higher, and the requirements for suppressing electromagnetic signal crosstalk between channels are also getting higher and higher. Therefore, as the LTCC circuit substrate for circuit interconnection and airtight carrier, while continuously improving the integration density, it is also urgent to improve the electromagnetic isolation capability between the RF channels inside the substrate.

[0003] In recent years, more and more attention has been paid to the electromagnetic isolation of high-density LTCC circuit substrates in engineering. The patent "A transmission structure of microwave signals on LTCC substrates and its manufacturing method" discloses a high-isolation microwave signal transmission structure on LTCC substrates. By arranging a cavity between the radio frequency channels and solid metallizing its side walls, the electromagnetic isolation between the microwave signal transmission channels inside the substrate is improved. However, the transmission structure disclosed in the patent requires special cavity processing and metallization after the LTCC substrate is formed. Therefore, the transmission structure can only be arranged in the circuit layer close to the surface of the substrate, and cannot be buried in the internal area of ​​the substrate, which restricts the application flexibility. At the same time, the production of isolation cavities requires a certain width, which occupies the wiring space and is not conducive to the improvement of the integration density of the circuit substrate. The patent "Circuit Board" also discloses a method for improving the isolation of signal routing on a multi-layer circuit substrate by using isolation grooves, but it is necessary to arrange a conductive medium inside the groove by electroplating metal to form a shielding wall. Therefore, this method still cannot be buried inside the substrate. At the same time, the production of isolation cavities also occupies the wiring space, which is not conducive to the improvement of the wiring density of the substrate.

[0004] The patent "Method for manufacturing a hybrid multilayer circuit substrate" forms an electromagnetic shielding layer by printing a conductive coating on the extreme difference part of the flexible circuit substrate, but this method is applied to the interconnection between circuit substrates and cannot be used to make the shielding layer inside the circuit substrate. The patent "A miniaturized wide stopband filter in the N79 frequency band based on LTCC process", the patent "A LTCC radio frequency device and electronic device", and the patent "Bandpass filter and filtering method based on LTCC technology" all form a shielding layer by including a metal layer on the outer layer of the device, but this method cannot be used to make a shielding structure buried in the LTCC substrate.

[0005] The patent "Integrated Circuit Packaging and Method for Manufacturing Integrated Circuits", the patent "LTCC Filter", the patent "X-band Dual-Polarization High-Isolation Microwave TR Component for Spaceborne Active Phased Array Radar", the patent "An LTCC Bandpass Filter Loaded with Square Ridges and Shielding Layers", and the patent "An Improved Layered One-to-Two Power Splitter Based on LTCC" all improve the isolation between the upper and lower signal layers by arranging horizontal planar metal layers. However, this method of horizontally arranging metal layers can only be used for electromagnetic isolation between the upper and lower transmission lines, and cannot be used for isolation of electromagnetic signals in the horizontal direction.

[0006] The paper "Research on Isolation Problems between LTCC Filter Paths", the patent "A Coupled Resonance Structure of Ultra-Wideband YIG Electrically Tunable Filter Based on LTCC", and the patent "A LTCC Millimeter-Wave Filter" all improve the electromagnetic isolation effect between devices or signal channels and the outside world in the horizontal direction by arranging discrete metallized through-holes. However, these discrete metallized through-holes are made based on the conventional LTCC through-hole processing technology. Due to the minimum spacing requirements between through-holes, the proportion of metallized through-holes in the isolation area is low. The shielding effect on electromagnetic signals is highly related to the through-hole arrangement density, the number of through-hole arrangements, the frequency of electromagnetic signals, etc. It not only takes up wiring space, but the shielding effect will also decrease significantly with the increase of the frequency of the electromagnetic signal, especially in the millimeter wave and above frequency bands, the shielding effect deteriorates significantly.

[0007] The patent "A radio frequency signal shielding hole for LTCC packaging glass and its production method" discloses a method for producing ultra-high density metallized through holes, which can effectively increase the proportion of metallized through holes in the isolation area, thereby achieving signal protection and isolated transmission. However, this method requires special photolithographic sealing glass and is implemented in conjunction with semiconductor processes such as polishing, exposure, and reactive ion etching. It is incompatible with conventional LTCC materials and LTCC processes and cannot be used for the processing of embedded shielding structures in LTCC substrates.

[0008] In view of the urgent need for high isolation between embedded RF channels in high-density LTCC substrates, it is urgent to develop a solid metal wall shielding structure that can be embedded inside the LTCC substrate to achieve good shielding of high-frequency microwave signals at a relatively small space cost. Summary of the invention

[0009] In order to solve the above problems, the present invention proposes a method for preparing a solid metal wall shielding structure embedded in an LTCC substrate. The solid metal wall structure can be flexibly embedded and integrated inside the LTCC substrate to achieve good isolation of high-frequency microwave signals without affecting the conventional circuit wiring of the substrate.

[0010] The technical solution adopted by the present invention is as follows:

[0011] A method for preparing a solid metal wall shielding structure embedded in a LTCC substrate, comprising:

[0012] Raw porcelain micro-gap processing: Prepare the micro-gap required for the solid metal wall shielding structure on raw porcelain;

[0013] Overall coating protection for raw porcelain: overall coating protection for raw porcelain with micro cracks;

[0014] Micro-gap slurry filling: Fill the micro-gap on the raw porcelain with metal slurry;

[0015] Raw porcelain demolding: demolding of multiple layers of raw porcelain and smoothing of excess metal slurry;

[0016] Green porcelain stacking and lamination: Multi-layer green porcelain is stacked through the LTCC (low temperature co-fired ceramic) process and laminated by warm water isostatic pressing to form an LTCC circuit embryo with an embedded solid metal wall shielding structure;

[0017] Circuit embryo sintering: The LTCC circuit embryo is co-fired to eventually form an LTCC circuit substrate with an embedded solid metal wall shielding structure.

[0018] Furthermore, the preparation of micro gaps required for the solid metal wall shielding structure on the raw porcelain includes: processing the micro gaps on the raw porcelain based on laser cutting technology, and adsorbing the raw porcelain flatly on the processing table by vacuum adsorption during the processing.

[0019] Furthermore, the overall coating protection of the green porcelain with micro gaps includes: after the micro gap processing of the green porcelain is completed and the processing slag is cleaned, a low-viscosity PET film is adhered to the front of the green porcelain as an overall coating, and during the coating process, the green porcelain is flatly adsorbed on the processing table by vacuum adsorption.

[0020] Furthermore, the filling of the micro gaps on the raw porcelain with metal slurry comprises: using a screen printing process to fill the metal slurry into the micro gaps, the metal slurry is filled in from one side of the PET film of the raw porcelain, during the filling process the raw porcelain adheres to the protective film and is fixed by the vacuum and flat adsorption workbench of the printing press, the PET film of the raw porcelain faces upwards and contacts with the printing screen, and repeated printing allows sufficient and adequate slurry to be filled into the micro gaps of the raw porcelain.

[0021] Furthermore, the metal slurry includes a pore-filling slurry that can be co-fired with green porcelain.

[0022] Furthermore, the material of the printing screen includes stainless steel wire mesh.

[0023] Furthermore, the demolding of the multi-layer green porcelain and smoothing of the excess metal slurry include:

[0024] Remove the PET film of the green porcelain: adsorb the whole coated side of the green porcelain on the vacuum workbench, tear off the PET film of the green porcelain from the back of the green porcelain, and use the scraping method to remove the excess protruding slurry filled in the micro gaps, so that the height of the slurry filled in the micro gap area is flush with the green porcelain;

[0025] Remove the overall coating: adsorb the back of the raw porcelain with the PET film removed on a vacuum workbench, and tear off the overall coating from the front of the raw porcelain.

[0026] Furthermore, the method of laminating multiple layers of raw porcelain by conventional LTCC (low temperature co-fired ceramic) process includes: utilizing the porous stone adsorption robot table of the LTCC lamination equipment to adsorb and grab the raw porcelain after demolding, stacking each layer of raw porcelain together in order through visual alignment of the equipment, and fixing them by gluing or spot welding.

[0027] Furthermore, the lamination by conventional warm water isostatic pressing includes: vacuum packaging the laminated green porcelain, and then placing it in a warm water isostatic press, and combining the layers of green porcelain tightly together by heating and pressurizing to form a LTCC circuit substrate embryo.

[0028] Furthermore, the co-firing of the LTCC circuit embryo body includes: sintering the LTCC circuit embryo body using sintering conditions matching the green porcelain, so as to transform the LTCC circuit embryo body into a circuit substrate.

[0029] The beneficial effects of the present invention are:

[0030] This patent replaces the traditional discrete metalized through-hole shielding structure by making a buried solid metal wall shielding structure in the LTCC substrate, and realizes continuous metal conductor shielding between microwave RF channels buried in the LTCC substrate, which can greatly improve the isolation between adjacent RF channels inside the substrate, especially in the high-frequency band. The preparation process used in this method is compatible with conventional LTCC substrate process technology and is easy to apply in complex circuit substrates. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 It is a top view of the combination 1 of LTCC raw ceramic and self-contained PET film that has completed conventional punching, filling and printing processes.

[0032] Figure 2 It is a cross-sectional view of the assembly 1 along 1-A to 1-A'.

[0033] Figure 3 It is a top view after processing micro gaps on the assembly 1.

[0034] Figure 4 It is a cross-sectional view along 1-A to 1-A' after processing micro gaps on the assembly 1.

[0035] Figure 5 This is a top view of the raw porcelain 1-g after overall coating protection.

[0036] Figure 6 It is a cross-sectional view along 1-A to 1-A' after the green porcelain is entirely coated.

[0037] Figure 7 This is a cross-sectional view of the micro-gaps on the green porcelain 1-g after being filled with metal slurry.

[0038] Figure 8 It is a cross-sectional view after the PET film 1-p attached to the back of the raw porcelain 1-g is removed.

[0039] Fig. 9 This is a cross-sectional view of the green porcelain 1-g after the excess slurry on the back has been trimmed.

[0040] Fig.10 This is a cross-sectional view of the raw porcelain 1-g after removing the front protective film 1-f.

[0041] Fig.11 This is a top view of the raw porcelain 1-g after removing the front protective film 1-f.

[0042] Fig.12 This is a cross-sectional view of each layer of raw porcelain after the circuit elements are processed.

[0043] Fig.13 It is a cross-sectional view of the LTCC substrate stacking structure.

[0044] Figure markings: 1-g is raw porcelain, 1-p is the PET film of raw porcelain; 1-f is the low-viscosity PET film covering the front of raw porcelain; 1-1 is a through hole processed on the assembly 1 for interlayer interconnection; 1-2 is the wiring printed on the surface of the raw porcelain 1-g, 1-2 can be either a signal line for signal transmission or a ground metal for microwave grounding; 1-3 is a micro gap processed on the assembly 1; 1-4 is the metal slurry filled in the micro gaps of the raw porcelain 1-g and the PET film 1-p of the raw porcelain; 1-S is a microwave signal transmission line made using the same process as 1-2; n is the processing state of the raw porcelain; Ground and Ground-1 are ground metals made on the surface and inside the substrate using the same process as the signal line 1-2. DETAILED DESCRIPTION

[0045] In order to have a clearer understanding of the technical features, purposes and effects of the present invention, the specific implementation methods of the present invention are now described. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention, that is, the embodiments described are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without making creative work are within the scope of protection of the present invention.

[0046] Example 1

[0047] This embodiment provides a method for preparing a solid metal wall shielding structure embedded in a LTCC substrate, comprising:

[0048] Raw porcelain micro-gap processing: Prepare the micro-gap required for the solid metal wall shielding structure on raw porcelain;

[0049] Overall coating protection for raw porcelain: overall coating protection for raw porcelain with micro cracks;

[0050] Micro-gap slurry filling: Fill the micro-gap on the raw porcelain with metal slurry;

[0051] Raw porcelain demolding: demolding of multiple layers of raw porcelain and smoothing of excess metal slurry;

[0052] Green porcelain stacking and lamination: Multi-layer green porcelain is stacked by conventional LTCC (low temperature co-fired ceramic) process, and laminated by warm water isostatic pressing to form an LTCC circuit embryo with an embedded solid metal wall shielding structure;

[0053] Circuit embryo sintering: The LTCC circuit embryo is co-fired to eventually form an LTCC circuit substrate with an embedded solid metal wall shielding structure.

[0054] The raw porcelain material is conventional LTCC raw porcelain, and the thickness range is usually 0.05mm to 0.15mm. The bottom of the raw porcelain is equipped with a PET film, which is combined with the back of the raw porcelain during the raw porcelain casting process, and is called a self-contained PET film. The thickness range is usually 0.03mm to 0.1mm.

[0055] Before the micro-gap processing, the raw porcelain has been processed through the punching, filling and printing processes in the conventional LTCC process to produce the inter-layer signal interconnection through holes and intra-layer interconnection wiring required for the LTCC multi-layer circuit. The punching method is usually mechanical punching or laser punching, and the optional range of through-hole diameter is usually 0.05mm to 0.3mm. The filling method is usually printing filling or injection filling, and the filling slurry is a matching slurry that can be co-fired with the raw porcelain. The intra-layer interconnection wiring is processed by screen printing, and the wiring bandwidth is usually ≥0.08mm. The wiring slurry is a matching slurry that can be co-fired with the raw porcelain.

[0056] The micro-gap required for the solid metal wall structure is usually 0.05mm to 0.15mm wide and 1.0mm to 30mm long, penetrating the raw porcelain and its own PET film in the depth direction. Preferably, the micro-gap processing method is laser cutting, and the raw porcelain is flatly adsorbed on the processing table by vacuum adsorption during the processing to avoid processing deviation due to local displacement of the raw porcelain.

[0057] Preferably, the green porcelain with micro gaps is protected by an overall coating, including: after the micro gaps of the green porcelain are processed, a low-viscosity PET film is pasted on the front of the green porcelain to provide complete support and protection for the green porcelain. The protective film is usually a PET film, and the selected PET film can be selected with a thickness of 0.05mm to 0.2mm. Its surface has low viscosity to the green porcelain, that is, it can adhere to the surface of the green porcelain and can be smoothly detached from the surface of the green porcelain when needed.

[0058] More preferably, the green porcelain with micro-gaps is subjected to overall coating protection after the micro-gaps are processed and the processing slag is cleaned. During the coating process, the green porcelain is flatly adsorbed on a vacuum fixed table to ensure that the green porcelain does not experience local displacement and deformation due to the existence of long-distance micro-gaps, thereby ensuring the inter-layer alignment accuracy of the LTCC multi-layer circuit substrate.

[0059] Preferably, the micro gaps on the raw porcelain are filled with metal slurry, including: using a screen printing process to fill the metal slurry into the micro gaps. The metal slurry is filled from one side of the PET film of the raw porcelain. During the filling process, the raw porcelain adheres to the protective film and is fixed by the vacuum and flat adsorption workbench of the printer. The PET film of the raw porcelain faces upward and contacts the printing screen. By repeated printing (for example, 3-5 times), the slurry is sufficiently and fully filled into the micro gaps of the raw porcelain.

[0060] More preferably, the drying conditions after the slurry filling are the conventional process conditions of the LTCC process, the drying temperature is usually 50° C. to 80° C., and the drying time is usually 5 min to 10 min.

[0061] More preferably, the metal slurry is a pore-filling slurry that can be co-fired with green porcelain.

[0062] More preferably, the printing screen used is made of stainless steel screen, and the width and length of the printing slit area should be increased by 0.05mm to 0.2mm on one side compared with the width and length of the micro-gap on the raw porcelain to ensure that the filling slurry can fully cover the micro-gap surface during the slit printing process.

[0063] Preferably, the demolding of the multi-layer green porcelain is carried out in two steps. The first step is to remove the PET film of the green porcelain, and the second step is to remove the overall coating:

[0064] Remove the PET film of the green porcelain: adsorb the whole coated side of the green porcelain flatly on the vacuum workbench, tear off the PET film of the green porcelain from the back of the green porcelain, and use the scraping method to remove the excess protruding slurry filled in the micro-gap, so that the height of the slurry filled in the micro-gap area is flush with the green porcelain;

[0065] Removing the overall coating: The back of the green porcelain with the PET film removed is flatly adsorbed on the vacuum workbench, and the overall coating is torn off from the front of the green porcelain. More preferably, the film removal vacuum workbench is the loading workbench of the lamination equipment, and the lamination process is carried out immediately after the protective film is removed.

[0066] Preferably, multiple layers of raw porcelain are laminated by conventional LTCC (low temperature co-fired ceramic) processes, including: using the porous stone of the LTCC lamination equipment to adsorb the robot table, adsorb and grab the raw porcelain after demolding, and stack each layer of raw porcelain together in order through visual alignment of the equipment, and fix them by gluing or spot welding. This process is a conventional LTCC lamination process.

[0067] Preferably, lamination is performed by conventional warm water isostatic pressing, including: vacuum packaging the laminated green porcelain, and then placing it in a warm water isostatic press, and heating and pressurizing the green porcelain layers to form a LTCC circuit substrate embryo. This process is a conventional LTCC lamination process, the lamination water temperature is usually 70-75°C, the pressure condition is usually 2500PSI-3500PSI, and the holding time is 8-20min.

[0068] Preferably, the LTCC circuit embryo is co-fired, including: sintering the LTCC circuit embryo using sintering conditions matching the green porcelain, so that the LTCC circuit embryo is transformed into a circuit substrate, and the functions of each part of the circuit are realized. This process is a conventional LTCC sintering process.

[0069] Example 2

[0070] This embodiment is based on embodiment 1:

[0071] This embodiment provides a method for preparing a solid metal wall shielding structure embedded in a LTCC substrate. Figure 1 , Figure 2As shown, the JC29 raw porcelain produced by China Building Materials Academy is selected. The raw porcelain 1-g has a thickness of 0.127mm, the dielectric thickness after sintering is 0.112mm, and the PET film 1-p on the back of the raw porcelain has a thickness of 0.05mm. The LTCC substrate is designed as 8 layers of raw porcelain. Through holes 1-1 and wiring patterns 1-2 are made on the raw porcelain using conventional LTCC processes such as punching, filling, and printing. The through hole diameter is 0.2mm, the filling paste is the matching Ag01 filling silver paste, and the printed wiring paste is the matching Ag02 wiring silver paste (inner layer) or Ag12 wiring silver paste (surface layer). The minimum wiring width is 0.15mm, and the wiring pattern 1-2 includes the control signal line, microwave signal transmission line, and microwave ground large-area metal layer required for circuit design.

[0072] like Figure 3 , Figure 4 As shown, micro gaps 1-3 are made on the green porcelain by laser cutting, with a width of 0.1 mm and a length of 20 mm. The micro gaps 1-3 penetrate the green porcelain 1-g and the PET film 1-p of the green porcelain.

[0073] like Figure 5 , Figure 6 As shown, the front side of the raw porcelain is covered with an overall protective coating. During the coating process, the raw porcelain is flatly sucked onto a vacuum table, and the protective film 1-f is adhered to the front side of the raw porcelain. The protective film 1-f protects the raw porcelain from defects such as local breakage and displacement during subsequent processing.

[0074] like Figure 7 As shown, the pore-filling slurry Ag01 is filled into the micro-gap from one side of the PET film 1-p of the raw porcelain by means of printing and filling. During the printing and filling process, the raw porcelain 1-g is adhered to the protective film 1-f, and the protective film 1-f is firmly adsorbed on the printing work surface. During the printing process, 5 consecutive repeated printings are used to ensure that a sufficient amount of the pore-filling slurry Ag01 is filled into the micro-gap 1-3. After filling, it is as shown in 1-4.

[0075] like Figure 8 As shown, the PET film 1-p on the back of the raw porcelain 1-g is removed. During the film removal process, the raw porcelain 1-g is adhered to the protective film 1-f and is firmly adsorbed on the work surface.

[0076] like Fig. 9 As shown, the raised slurry on the back of each layer of raw porcelain 1-g is removed cleanly by scraping with a knife.

[0077] like Fig.10 , Fig.11As shown, the protective films 1-f on each layer of green porcelain 1-g are removed from the green porcelain. During the film removal process, the green porcelain 1-g is firmly adsorbed on the loading work surface of the laminating machine. After the film removal, the laminating operation is immediately carried out. During the laminating process, the green porcelain is transferred and aligned for lamination by the vacuum plane adsorption manipulator of the laminating machine. The order of green porcelain lamination is as follows: Fig.12 As shown, K=8, the stacking order from top to bottom is N(1)-N(8), the microwave signal transmission line 1-S on the upper surface of the fifth layer of raw porcelain N5 is processed using the same wiring process as the wiring pattern 1-2, and the embedded solid metal wall is arranged on the third layer of raw porcelain N(3), the fourth layer of raw porcelain N(4), the fifth layer of raw porcelain N(5), and the sixth layer of raw porcelain N(6), as shown in the corresponding layers 1-4.

[0078] like Fig.13 The figure shows that the conventional LTCC lamination, isostatic pressing and co-firing process is used to laminate, press and sinter the layers of raw porcelain, and finally form an LTCC substrate with an embedded solid metal wall flat shielding structure. The slurry 1-4 filled in the micro-gaps 1-3 forms a solid metal wall structure embedded in the substrate after sintering, and is interconnected with the microwave ground metal Ground-1 inside the substrate to form a solid metal shielding wall structure. Specifically, this embodiment uses the conventional LTCC process to isostatically press the laminated 8 layers of raw porcelain N(1)-N(8), the water temperature is 71°C, the pressure is 3000PSI, and the holding time is 10 minutes, so that it becomes an LTCC substrate embryo. Then the conventional LTCC co-firing process is used for sintering, the sintering temperature is 850°C, and the sintering holding time is 15 minutes. Finally, an LTCC substrate with embedded solid metal wall structures 1-4 is formed on the 3rd to 6th layers, and the metal walls 1-4 are connected to the inner microwave ground Ground-1 of the substrate to form an embedded solid metal wall shielding structure to shield the signals of the microwave signal lines 1-S on the 5th layer, ultimately achieving high isolation between adjacent RF channels embedded in the LTCC.

[0079] It should be noted that, for the aforementioned method embodiments, for the sake of simplicity of description, they are expressed as a series of action combinations, but those skilled in the art should be aware that the present application is not limited by the order of the actions described, because according to the present application, certain steps can be performed in other orders or simultaneously. Secondly, those skilled in the art should also be aware that the embodiments described in the specification are all preferred embodiments, and the actions and modules involved are not necessarily required by the present application.

Claims

1. A method for preparing a solid metal wall shielding structure embedded in a LTCC substrate, characterized in that: include: Raw porcelain micro-gap processing: Prepare the micro-gap required for the solid metal wall shielding structure on raw porcelain; Overall coating protection for raw porcelain: overall coating protection for raw porcelain with micro cracks; Micro-gap slurry filling: Fill the micro-gap on the raw porcelain with metal slurry; Raw porcelain demolding: demolding of multiple layers of raw porcelain and smoothing of excess metal slurry; Green porcelain stacking and lamination: Multi-layer green porcelain is stacked by conventional LTCC (low temperature co-fired ceramic) process, and laminated by warm water isostatic pressing to form an LTCC circuit embryo with an embedded solid metal wall shielding structure; Circuit embryo sintering: The LTCC circuit embryo is co-fired to eventually form an LTCC circuit substrate with an embedded solid metal wall shielding structure.

2. The method for preparing a solid metal wall shielding structure embedded in a LTCC substrate according to claim 1, characterized in that: The method of preparing the micro gaps required for the solid metal wall shielding structure on the raw porcelain comprises: processing the micro gaps on the raw porcelain based on laser cutting technology, and adsorbing the raw porcelain flatly on the processing table by vacuum adsorption during the processing.

3. The method for preparing a solid metal wall shielding structure embedded in a LTCC substrate according to claim 1, characterized in that: The overall coating protection of the green porcelain with micro gaps includes: after the micro gap processing of the green porcelain is completed and the processing slag is cleaned, a low-viscosity PET film is adhered to the front of the green porcelain as an overall coating, and during the coating process, the green porcelain is flatly adsorbed on the processing table by vacuum adsorption.

4. The method for preparing a solid metal wall shielding structure embedded in a LTCC substrate according to claim 1, characterized in that: The method of filling the micro gaps on the raw porcelain with metal slurry comprises: using a screen printing process to fill the metal slurry into the micro gaps, wherein the metal slurry is filled in from one side of a PET film on the raw porcelain, during the filling process the raw porcelain adheres to the protective film and is fixed by a vacuum and flat adsorption workbench of a printing press, wherein the PET film on the raw porcelain faces upward and contacts with a printing screen, and repeated printing allows sufficient and adequate slurry to be filled into the micro gaps of the raw porcelain.

5. The method for preparing a solid metal wall shielding structure embedded in a LTCC substrate according to claim 4, characterized in that: The metal slurry includes a pore-filling slurry that can be co-fired with green porcelain.

6. The method for preparing a solid metal wall shielding structure embedded in a LTCC substrate according to claim 4, characterized in that: The material of the printing screen includes stainless steel wire mesh.

7. The method for preparing a solid metal wall shielding structure embedded in a LTCC substrate according to claim 1, characterized in that: The method of stripping the multi-layer green porcelain and smoothing the excess metal slurry includes: Remove the PET film of the green porcelain: adsorb the whole coated side of the green porcelain on the vacuum workbench, tear off the PET film of the green porcelain from the back of the green porcelain, and use the scraping method to remove the excess protruding slurry filled in the micro gaps, so that the height of the slurry filled in the micro gap area is flush with the green porcelain; Remove the overall coating: adsorb the back of the raw porcelain with the PET film removed on a vacuum workbench, and tear off the overall coating from the front of the raw porcelain.

8. The method for preparing a solid metal wall shielding structure embedded in a LTCC substrate according to claim 1, characterized in that: The method of laminating multiple layers of raw porcelain by conventional LTCC (low temperature co-fired ceramic) process includes: utilizing a porous stone adsorption robot table of LTCC lamination equipment to adsorb and grab the raw porcelain after demolding, stacking each layer of raw porcelain together in order through visual alignment of the equipment, and fixing them by gluing or spot welding.

9. The method for preparing a solid metal wall shielding structure embedded in a LTCC substrate according to claim 1, characterized in that: The lamination by conventional warm water isostatic pressing includes: vacuum packaging the laminated green porcelain, and then placing it in a warm water isostatic press, and combining each layer of green porcelain tightly together by heating and pressurizing to form a LTCC circuit substrate embryo.

10. The method for preparing a solid metal wall shielding structure embedded in a LTCC substrate according to claim 1, characterized in that: The co-firing of the LTCC circuit embryo body comprises: sintering the LTCC circuit embryo body using sintering conditions matching the green ceramic, so as to transform the LTCC circuit embryo body into a circuit substrate.