Electroluminescent device and preparation method and application thereof
By adopting a transparent anode layer, electroluminescent unit and protective layer structure in QLED devices, the brightness and life problems caused by metal electrodes are solved, and electroluminescent devices with high transmittance and low voltage are achieved, satisfying electroluminescence Device usage requirements.
Patent Information
- Application Number
- CN202410908818.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-11-08
Smart Images

Figure BDA0004932948000000081 
Figure BDA0004932948000000082 
Figure HDA0004932948010000011
Abstract
Description
Technical Field
[0001] The invention belongs to the field of devices, and in particular relates to an electroluminescent device and a preparation method and application thereof. Background Art
[0002] The biggest feature of transparent display screens is that the display content can be seen in both directions of the screen, which can realize virtual reality superposition display and can be applied to sights, gun sights, amplifiers, advertising window displays, instruments and other products. Quantum dot light-emitting diodes (QLEDs) are considered to be excellent devices for the next generation of solid-state lighting and displays because they have tunable wavelengths and narrow full width at half maximum, good color gamut and high efficiency. In the structure of the device, the injection layer, the transmission layer, and the light-emitting layer are nanometer-thick films that are spin-coated layer by layer on a transparent ITO substrate by a solution process, and have high transparency. In order to achieve transparent display, the cathode generally uses an ultra-thin semi-transparent metal layer, such as 15-30nm Ag, Mg:Ag alloy film. The use of metal electrodes has the following problems: on the one hand, the metal electrode is semi-transparent (visible light transmittance is 20-50%), which will reduce the brightness of the QLED device, and most of the light can only be emitted from the anode such as the ITO electrode; on the other hand, the metal electrode absorbs light from the quantum dot light-emitting layer, resulting in excess heat inside the device, thereby reducing the life of the QLED device. Summary of the invention
[0003] In order to overcome the problems existing in the prior art, one of the objectives of the present invention is to provide an electroluminescent device.
[0004] A second object of the present invention is to provide a method for preparing an electroluminescent device.
[0005] A third object of the present invention is to provide an application of an electroluminescent device in a light-emitting device.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is:
[0007] The first aspect of the present invention provides an electroluminescent device, comprising a transparent anode layer, an electroluminescent unit, a protective layer and a transparent cathode layer stacked in sequence; the material of the protective layer is selected from ITO, AZO, ZnO, IZO, IGZO, TiN, Al2O3, TiO x At least one of the TiO x , 1.5≤x≤2. IGZO is indium gallium zinc oxide.
[0008] Preferably, the light transmittance of the transparent anode layer is ≥85%.
[0009] Preferably, the material of the transparent cathode layer is silver nanowires.
[0010] Preferably, the material of the transparent anode layer is selected from ITO, IZO, AZO or graphene. AZO refers to a mixture of Al and ZnO.
[0011] Preferably, the electroluminescent unit comprises a hole transport layer, a light emitting layer and an electron transport layer which are stacked.
[0012] Preferably, the material of the light-emitting layer is selected from at least one of CdSe and indium phosphide (InP)-based quantum dot materials. Further preferably, the material of the light-emitting layer is CdSe quantum dots.
[0013] Preferably, the material of the hole transport layer is poly(9,9-n-dioctyl-2,7-fluorene-alt-9-isooctyl-3,6-carbazole).
[0014] Preferably, the thickness of the transparent cathode layer is 20-200 nm.
[0015] Preferably, the material of the electron transport layer is selected from ZnO or ZnMgO.
[0016] When the material of the electron transport layer is ZnO or ZnMgO, if a transparent cathode layer is prepared directly on the electron transport layer, the solvent in the silver nanowire solution will corrode the electron transport layer, thereby causing damage to the electron transport layer, thereby making the voltage of the device higher. Therefore, the present invention preferably provides a protective layer on the electron transport layer to protect the electron transport layer by the protective layer to prevent the electron transport layer from being damaged by the silver nanowire solution.
[0017] Preferably, the light transmittance of the protective layer is not less than 85%.
[0018] Preferably, when the material of the protective layer is Al2O3 or TiO x When the protective layer is 0.5-2 nm thick.
[0019] Preferably, when the material of the protective layer is ITO, AZO, ZnO, IZO, IGZO, or TiN, the thickness of the protective layer is 3 to 10 nm.
[0020] Preferably, the electroluminescent unit is formed into a film by coating or printing.
[0021] Preferably, the protective layer is deposited by sputtering and / or atomic layer deposition.
[0022] Preferably, the transparent cathode layer is formed by coating or printing, and then heat-treated at a temperature not exceeding 120°C.
[0023] Preferably, the coating comprises knife coating, spray coating, spin coating or casting.
[0024] Preferably, the electroluminescent unit comprises a hole transport layer, a light emitting layer and an electron transport layer which are stacked, and the material of the light emitting layer is selected from at least one of CdSe and InP; the material of the electron transport layer is selected from ZnO or ZnMgO.
[0025] Preferably, a metal modification layer is provided on the electron transport layer; the metal modification layer is located between the electron transport layer and the protective layer; and the material of the metal modification layer is selected from Al, Mg, and Ga.
[0026] Preferably, the first protective layer and the second protective layer are sequentially arranged on the metal modification layer. In the present invention, the metal modification layer can be first arranged on the electron transport layer, and then one or two protective layers can be arranged, so that the electron transport layer can be better protected and the overall performance of the device can be improved.
[0027] Preferably, a first protective layer and a second protective layer are disposed on the electron transport layer.
[0028] In the present invention, the number of protective layers is not less than 1. When the number of protective layers is two, the protective layers include a first protective layer and a second protective layer. Preferably, the protective layer includes a first protective layer and a second protective layer stacked in sequence; the material of the first protective layer is selected from Al2O3, TiO x The material of the second protective layer is selected from ITO, AZO, ZnO, IZO, IGZO or TiN. The first protective layer is an insulating structure with a dense structure, which can protect the electron transport layer from being corroded by the transparent cathode layer; the second protective layer is a conductive structure, which has better compatibility and connection performance with the transparent cathode layer.
[0029] Preferably, the thickness of the first protective layer is 0.5-2 nm.
[0030] Preferably, the first protective layer is obtained by atomic layer deposition.
[0031] Preferably, the second protective layer is obtained by atomic layer deposition or sputtering.
[0032] Preferably, the second protective layer has a thickness of 3-10 nm.
[0033] The second aspect of the present invention provides a method for preparing the electroluminescent device provided in the first aspect of the present invention, comprising the following steps:
[0034] S1: forming an electroluminescent unit on the transparent anode layer;
[0035] S2: forming a protective layer on the electroluminescent unit by sputtering and / or atomic layer deposition;
[0036] S3: forming a transparent cathode layer on the protective layer.
[0037] Preferably, the step S1 is: sequentially forming a hole transport layer, a quantum dot layer and an electron transport layer on the transparent anode layer;
[0038] Preferably, the step S2 is: forming a protective layer on the electron transport layer by sputtering, and then performing a thermal annealing treatment at 60 to 120° C. for 10 to 60 minutes.
[0039] Preferably, the step S2 is: forming a protective layer on the electron transport layer by an atomic layer deposition method at a temperature of 80 to 120°C.
[0040] Preferably, step S3 comprises spraying the alcohol solution of silver nanowires on the protective layer at a spray rate of 0.02 to 0.3 mL / min at a temperature of 40 to 100° C. for 2 to 10 times. When the silver nanowire solution is sprayed at a spray rate of 0.02 to 0.3 mL / min for 2 to 10 times, the coverage of the silver nanowires is higher, the luminous efficiency is higher, and the transparent cathode layer can be prevented from being short-circuited due to being too thin.
[0041] Preferably, the spraying rate is 0.1-0.3 mL / min.
[0042] Preferably, the spraying times are 4 to 10 times.
[0043] Preferably, the spraying temperature is 40-100°C.
[0044] Preferably, the alcohol is selected from at least one of ethanol and isopropanol; more preferably, the alcohol is selected from ethanol.
[0045] Preferably, the mass percentage of the silver nanowires in the silver nanowire solution is 0.3-0.5%.
[0046] Preferably, the coating step in step S3 is selected from one of blade coating, spin coating or spray coating.
[0047] The third aspect of the present invention provides use of the electroluminescent device provided by the first aspect of the present invention in a light-emitting device.
[0048] The beneficial effects of the present invention are as follows: the cathode side and the anode side of the electroluminescent device of the present invention both have high light transmittance, and the light transmittance in the visible light wavelength range of 450nm to 700nm exceeds 80%, and the cathode side and the anode side of the device both have low voltage and high current efficiency, the voltage is as low as 1.8V, and the current efficiency is 2 to 3cd / A, which meets the use requirements of the electroluminescent device, and the performance of the cathode side and the anode side of the device are basically close, and balanced light emission on both sides can be achieved. BRIEF DESCRIPTION OF THE DRAWINGS
[0049] Figure 1 This is an AFM image of a silver nanowire layer formed by spraying the ethanol solution of Ag NWs twice according to the present invention.
[0050] Figure 2 This is an AFM image of a silver nanowire layer formed by spraying the ethanol solution of Ag NWs of the present invention six times.
[0051] Figure 3 This is an AFM image of a silver nanowire layer formed by spraying the ethanol solution of Ag NWs of the present invention 10 times.
[0052] Figure 4 This is an AFM image of a silver nanowire layer formed by the ethanol solution of Ag NWs in the present invention at a spraying rate of 0.1 mL / min.
[0053] Figure 5 This is an AFM image of a silver nanowire layer formed by the ethanol solution of Ag NWs in the present invention at a spraying rate of 0.15 mL / min.
[0054] Figure 6 This is an AFM image of a silver nanowire layer formed by the ethanol solution of Ag NWs in the present invention at a spraying rate of 0.3 mL / min.
[0055] Figure 7 This is a transmittance test diagram of the electroluminescent device in Example 1.
[0056] Figure 8 This is a transmittance test diagram of the electroluminescent device in Example 2.
[0057] Fig. 9 This is a transmittance test diagram of the electroluminescent device in Example 3.
[0058] Fig.10 This is a transmittance test diagram of the electroluminescent device in Example 4.
[0059] Fig.11 This is a transmittance test diagram of the electroluminescent device in Comparative Example 1.
[0060] Fig.12 This is a transmittance test diagram of the electroluminescent device in Comparative Example 2. DETAILED DESCRIPTION
[0061] The specific implementation of the present invention is further described in detail below in conjunction with the accompanying drawings and examples, but the implementation and protection of the present invention are not limited thereto. It should be noted that if there are processes that are not particularly described in detail below, they can be implemented or understood by those skilled in the art with reference to the prior art. The reagents or instruments used that do not indicate the manufacturer are all conventional products that can be purchased commercially.
[0062] In the embodiment of the present invention, the spraying times and spraying rate of the ethanol solution of Ag NWs have a great influence on the morphology of the transparent cathode layer. Specifically, when the spraying rate is 0.15 mL / min, the ethanol solution of Ag NWs is sprayed 2 times, 6 times and 10 times respectively, and sprayed in the XY direction. When the substrate is completely covered, it is counted as one spraying. After the spraying is completed, annealing is performed at 60°C for 30 minutes to form three different transparent cathode layers. Then, the surface morphology of the three transparent cathode layers is tested by atomic force microscopy. The specific test results are shown as follows: Figure 1 to Figure 3 As shown, Figure 1 , Figure 2 and Figure 3 AFM images of the silver nanowire layers formed by spraying 2 times, 6 times, and 10 times, respectively. Figure 1 to Figure 3 It can be seen that under the same discharge speed, as the number of spraying times increases, the coverage of the silver nanowire layer will become better. However, when the number of spraying times is too many, it will cause the stacking of silver nanowires. The ethanol solution of Ag NWs was sprayed 10 times at a spraying rate of 0.1mL / min, 0.15mL / min, and 0.3mL / min, respectively. After the spraying was completed, it was annealed at 60°C for 30min to form three different transparent cathode layers. Then, the surface morphology of the three transparent cathode layers was tested by atomic force microscopy. The specific test results are shown in the figure. Figures 4 to 6 As shown, Figure 4 , Figure 5 and Figure 6 The AFM images of the silver nanowire layer formed at a spraying rate of 0.1 mL / min, 0.15 mL / min, and 0.3 mL / min are shown in Figure 1. Figures 4 to 6 It can be seen that, under the same spraying times, as the discharge speed increases, the coverage of the silver nanowire layer will become better. However, when the discharge speed is too fast, the silver nanowires will agglomerate and affect the morphology. Therefore, in the embodiments of the present invention, the spraying speed is 0.1 mL / min and the spraying is 10 times. At this spraying rate and spraying times, a better morphology can be obtained.
[0063] Example 1
[0064] This example provides an electroluminescent device, comprising a substrate layer, a transparent anode layer, a hole transport layer, a quantum dot layer, an electron transport layer, an ITO protective layer and a transparent cathode layer stacked in sequence, wherein the material of the substrate layer is transparent glass, the material of the transparent anode layer is ITO with a thickness of 170 nm, the thickness of the hole transport layer is 50 nm, the material of the hole transport layer is poly (9,9-n-dioctyl-2,7-fluorene-alt-9-isooctyl-3,6-carbazole) (abbreviated as PF8-Cz), the thickness of the quantum dot layer is 20 nm, the quantum dots are CdSe quantum dots, the material of the electron transport layer is ZnMgO material (abbreviated as ZMO layer), the thickness of the electron transport layer is 45 nm, the thickness of the ITO protective layer is 5 nm, and its material is ITO; the material of the transparent cathode layer is silver nanowires with a thickness of 100 nm, which is prepared by spraying Ag NWs (ethanol) 10 times. The electroluminescent device in this example is: Glass / ITO / HIL (50nm) / red QD (20nm) / ZMO (45nm) / ITO (5nm) / silver nanowire layer.
[0065] The electroluminescent device in this example is prepared by the following preparation method, and the specific steps are:
[0066] The ITO substrate was ultrasonically cleaned with deionized water, ethanol and isopropanol for 15 minutes, and then treated with ozone generated by ultraviolet light in the air for 15 minutes. The substrate was then transferred to a glove box filled with nitrogen and spin-coated with a 1% PF8-Cz solution at 1500 rpm, followed by annealing in a glove box at 200°C for 30 minutes to obtain a 50nm thick PF8-Cz film, i.e., the hole transport layer. After cooling, a 20nm QD film (i.e., quantum dot layer) and a 45nm ZnMgO layer (i.e., electron transport layer) were spin-coated. The QD solution concentration was 100 mg / mL, and it was spin-coated at a speed of 2500 rpm for 30 seconds, and then annealed at 60°C for 10 minutes. The ZnMgO solution concentration was 30 mg / mL, and it was spin-coated at a speed of 2500 rpm, and then annealed at 90°C for 30 minutes to form a ZMO layer. An ITO protective layer was sputtered on the ZnMgO layer. The specific steps were as follows: the DC power during the sputtering of the ITO protective layer was fixed at 100 W (1.23 W / cm 2 ), the substrate temperature was set to 363K. The substrate holder rotated at 40rpm to achieve uniform deposition and form an ITO protective layer. Finally, the ethanol solution of Ag NWs was sprayed on the top of the ITO protective layer 10 times, specifically: a silver nanowire solution containing an ethanol solvent with a mass percentage of ω=0.5% was used, the spraying speed was 0.1mL / min, and the spraying was 10 times. After the spraying was completed, annealing was performed at 60°C for 30min to obtain the electroluminescent device in this example.
[0067] Example 2
[0068] The structure of the electroluminescent device in this example is different from that in Example 1 only in that an Al2O3 protective layer (thickness of 1 nm) is used in this example to replace the ITO protective layer in Example 1. The electroluminescent device in this example is Glass / ITO / HIL (50 nm) / red QD (20 nm) / ZMO (45 nm) / Al2O3 (ALD, 1 nm) / silver nanowire layer.
[0069] The preparation method of the electroluminescent device in this example is different from that in Example 1 in that the preparation steps of the Al2O3 protective layer in this example are: depositing the Al2O3 protective layer on the ZnMgO layer by atomic layer deposition (ALD), and the specific steps are: introducing trimethylaluminum (TMA) and H2O as precursor and reactant respectively for 2s, reacting for five seconds, blowing for 15s, introducing water for 2s, reacting for five seconds, and blowing for 15s. The theoretical deposition thickness of each cycle is 1.2A. After 8 cycles, an Al2O3 protective layer with a thickness of about 1nm is formed.
[0070] Example 3
[0071] The structure of the electroluminescent device in this example is different from that in Example 2 only in that an Al metal modification layer (1 nm thick) is provided between the electron transport layer and the Al2O3 protective layer in this example. The electroluminescent device in this example is Glass / ITO / HIL (50 nm) / red QD (20 nm) / ZMO (45 nm) / Al (ALD, 1 nm) / Al2O3 (ALD, 1 nm) / silver nanowire layer.
[0072] The preparation method of the electroluminescent device in this example is different from that in Example 2 in that: this example also includes the step of depositing an Al metal modification layer on the ZnMgO layer by atomic layer deposition (ALD), specifically: the Al metal is generated by reacting the precursor trimethylaluminum (TMA) and H2 plasma, with a thickness of 1 nm and a deposition temperature of 100°C.
[0073] Example 4
[0074] The structure of the electroluminescent device in this example is different from that in Example 3 only in that an IZO second protective layer is provided behind the protective layer Al2O3 in this example. The electroluminescent device in this example is Glass / ITO / HIL (50nm) / red QD (20nm) / ZMO (45nm) / Al (ALD, 1nm) / Al2O3 (ALD, 1nm) / IZO (10nm) / silver nanowire layer. The IZO second protective layer is obtained by sputtering with a sputtering power of 500W.
[0075] Example 5
[0076] The structure of the electroluminescent device in this example is different from that in Example 2 only in that the thickness of the protective layer Al2O3 in this example is 0.5 nm.
[0077] Example 6
[0078] The structure of the electroluminescent device in this example is different from that in Example 3 only in that the thickness of the protective layer Al2O3 in this example is 2 nm.
[0079] Example 7
[0080] The structure of the electroluminescent device in this example is different from that in Example 1 only in that the thickness of the ITO protective layer in this example is 3 nm.
[0081] Example 8
[0082] The structure of the electroluminescent device in this example is different from that in Example 1 only in that the thickness of the ITO protective layer in this example is 10 nm.
[0083] Comparative Example 1
[0084] The structure of the electroluminescent device in this example is different from that in Example 1 only in that: this example does not include an ITO protective layer and the material of the transparent cathode layer in this example is a Mg-Ag alloy, wherein the mass ratio of Mg:Ag is 1:9, and the thickness of the transparent cathode layer is 20nm. The electroluminescent device in this example is Glass / ITO / PF8-Cz (50nm) / red QD (CdSe 20nm) / ZnMgO (45nm) / Mg:Ag (20nm 1:9).
[0085] The preparation method of the electroluminescent device in this example is different from that in Example 1 in that: on the top of the electron transport layer (ie, the ZnMgO layer), Mg and Ag are co-evaporated in a mass ratio of 1:9 by vacuum thermal evaporation to obtain a 20 nm Mg-Ag alloy film.
[0086] Comparative Example 2
[0087] This example provides an electroluminescent device, comprising a substrate layer, a transparent anode layer, a hole transport layer, a quantum dot layer, an electron transport layer and a transparent cathode layer stacked in sequence, wherein the material of the substrate layer is transparent glass, the material of the transparent anode layer is ITO (thickness is 170nm), the thickness of the hole transport layer is 50nm, the material of the hole transport layer is poly (9,9-n-dioctyl-2,7-fluorene-alt-9-isooctyl-3,6-carbazole) (abbreviated as PF8-Cz), the thickness of the quantum dot layer is 20nm, the quantum dots are CdSe quantum dots, the material of the electron transport layer is ZnMgO material (abbreviated as ZMO layer), the thickness of the electron transport layer is 45nm, and the material of the transparent cathode layer is silver nanowires with a thickness of 100nm, which is prepared by spraying Ag NWs (ethanol) 10 times. The electroluminescent device in this example is: Glass / ITO / HIL (50nm) / red QD (20nm) / ZMO (45nm) / silver nanowire layer.
[0088] The electroluminescent device in this example is prepared by the following preparation method, and the specific steps are:
[0089] The ITO substrate was ultrasonically cleaned with deionized water, ethanol and isopropanol for 15 minutes, and then treated with ozone generated by ultraviolet light in the air for 15 minutes. The substrate was then transferred to a glove box filled with nitrogen and spin-coated with a 1% PF8-Cz solution at 1500 rpm, followed by annealing in a glove box at 200°C for 30 minutes to obtain a 50nm thick PF8-Cz film, i.e., the hole transport layer. After cooling, a 20nm QD film (i.e., quantum dot layer) and a 45nm ZnMgO layer (i.e., electron transport layer) were spin-coated. The QD solution concentration was 100mg / mL, and it was spin-coated at 2500 rpm for 30s, then annealed at 60°C for 10min. The ZnMgO solution concentration was 30mg / mL, and it was spin-coated at 2500 rpm, and then annealed at 90°C for 30min. Finally, the ethanol solution of Ag NWs was sprayed on the top of the ZMO layer 10 times, specifically: a silver nanowire solution containing an ethanol solvent with a mass percentage of ω=0.5% was used, the spraying speed was 0.1 mL / min, and the spraying was 10 times. After the spraying was completed, annealing was performed at 60° C. for 30 minutes to obtain the electroluminescent device in this example.
[0090] Performance Testing:
[0091] The light transmittance of the electroluminescent devices in Examples 1 to 4 and Comparative Examples 1 to 2 in the wavelength range of 450 nm to 700 nm was tested respectively. The specific test results are as follows: Figure 7 to Figure 12 As shown, according to Figure 7 to Figure 12 The transmittance data in Table 1 can be obtained, and then the light-on voltage V of the device can be obtained by testing. on, current efficiency (LE) and other data are shown in Table 2, where @1000cd / m 2 Indicates brightness is 1000cd / m 2 Device performance, V represents the corresponding device voltage, LE represents the corresponding current efficiency of the device; @100cd / m 2 Indicates brightness at 100cd / m 2 Device performance, V represents the corresponding device voltage, LE is the corresponding current efficiency of the device; 1cd / m 2 Refers to the brightness of 1cd / m 2 Device performance when LE 阴 / LE 阳 Indicates at 100cd / m 2 The ratio of the cathode light output efficiency to the anode light output efficiency at a certain brightness.
[0092] Table 1 Transmittance data of electroluminescent devices in Examples 1 to 4 and Comparative Examples 1 to 2
[0093]
[0094] Table 2 Performance comparison of the electroluminescent devices in Examples 1 to 4 and Comparative Examples 1 to 2
[0095]
[0096] Depend on Figure 7 As shown in Tables 1 and 2, the transmittance of the electroluminescent device in Example 1 is ≥ 80% in the wavelength range of 450nm to 700nm, and the transmittance is ≥ 80% in the wavelength range of 100cd / m 2 Under the highest brightness, the sum of the light output efficiency on the anode side and the light output efficiency on the cathode side of the device is 4.82cd / A. The obtained device has high brightness and high luminous efficiency, and the ratio of the light output efficiency on the anode side to the light output efficiency on the cathode side is 0.992, which is close to 1. The device maintains high transmittance while showing a good balance of light emission on both sides, and achieves better protection of the electron transport layer so that it will not be damaged by the spraying of silver nanowires.
[0097] Depend on Figure 8As shown in Tables 1 and 2, the electroluminescent device in Example 2 is deposited with an Al2O3 protective layer. The device maintains a high transmittance (at wavelengths of 460nm, 530nm, and 620nm, the transmittance is 86.8%, 87.6%, and 85.6%, respectively) while maintaining a high brightness and luminous efficiency of the device. Moreover, due to the dense characteristics of ALD, a complete protective film can be formed with only 1nm. Therefore, the electron transport layer (i.e., the ZnMgO layer) can be ensured at a relatively thin thickness (1nm) so that it will not be damaged by the spraying of silver nanowires. At the same time, the thinner barrier layer will not affect the working electrical characteristics of the device, so that a higher device performance and a relatively complete and uniform light-emitting surface can be obtained, and the transmittance, brightness, and efficiency can be improved.
[0098] Depend on Fig. 9 As shown in Tables 1 and 2, the electroluminescent device in Example 3 is deposited with an Al protective layer. Since the protective layer is only 1 nm, it does not affect its light transmission characteristics. The device maintains a high transmittance while maintaining a high brightness and luminous efficiency. 2 At a brightness of , the sum of the light output efficiency on the anode side and the light output efficiency on the cathode side reaches 4.83 cd / A, which is higher than the sum of the light output efficiency on the anode side and the light output efficiency on the cathode side of the device without an Al protective layer in Example 2, which is 4.6 cd / A. The main reason is that the diffusion and recombination of Al in ZnMgO further hinders the transmission of electron carriers, promotes the balance of carriers on both sides, and further improves the performance of the device.
[0099] Depend on Fig.10 As shown in Tables 1 and 2, the electroluminescent device in Example 4 has an Al modified layer deposited, and an IZO second protective layer is provided after the first protective layer Al2O3. The transmittance of each layer of this double protective layer is good, so the overall transmittance of the device is also good. When the wavelengths are 460nm, 530nm, and 620nm, the transmittances are 80.1%, 84.3%, and 80.6%, respectively. In particular, the device has a higher luminous efficiency, at 100cd / m 2 At a brightness of , the sum of the light output efficiency on the anode side and the light output efficiency on the cathode side reaches 4.93cd / A, which is higher than that of other embodiments and comparative examples. At the same time, the ratio of the light output efficiency on the cathode side to the light output efficiency on the anode side is 0.964, which is close to 1. The device exhibits good uniformity of light emission on both sides.
[0100] Depend on Fig.11 As can be seen from Tables 1 to 2, the device in Comparative Example 1 is a transparent QLED device with a general transmittance of about 50% in the visible light wavelength range of 450nm to 700nm. The transmittance is poor, and the brightness efficiency of the device's double-sided emission is quite different, and the device performance cannot meet the use requirements.
[0101] Depend on Fig.12 As can be seen from Tables 1 and 2, the light transmittance of the device of Comparative Example 2 in the wavelength range of 450nm to 700nm is ≥85%, achieving high transmittance and double-sided light emission, with almost no difference in double-sided emission brightness, but the overall brightness and current efficiency (LE) are low, and the device voltage is high. The main reason is that after the ZnMgO electron transport layer is spin-coated, an ethanol solution of Ag NWs is directly spin-coated thereon, causing a certain degree of damage to the underlying cathode layer ZnMgO layer.
[0102] In summary, the cathode side and the anode side of the electroluminescent device of the present invention have high light transmittance, and the light transmittance in the visible light wavelength range of 450nm to 700nm exceeds 80%, and the cathode side and the anode side of the device have low voltage and high current efficiency, the turn-on voltage is as low as 1.8V, and the current efficiency is 100cd / m 2 At low brightness, the photocurrent efficiency on both sides exceeds 2cd / A, which meets the use requirements of electroluminescent devices. In addition, the performance of the cathode side and the anode side of the device are basically close, and balanced light emission can be achieved on both sides.
[0103] The above is a detailed description of the embodiments of the present invention, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge of ordinary technicians in the relevant technical field without departing from the purpose of the present invention. In addition, the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.
Claims
1. An electroluminescent device, characterized in that: The invention comprises a transparent anode layer, an electroluminescent unit, a protective layer and a transparent cathode layer which are stacked in sequence; the material of the protective layer is selected from ITO, AZO, ZnO, IZO, IGZO, TiN, Al2O3, TiO x At least one of the TiO x , 1.5≤x≤2.
2. The electroluminescent device according to claim 1, characterized in that: The light transmittance of the transparent anode layer is ≥85%; And / or, the material of the transparent anode layer is selected from ITO, IZO, AZO or graphene; And / or, the electroluminescent unit comprises a hole transport layer, a light emitting layer, and an electron transport layer which are stacked; And / or, the material of the transparent cathode layer is silver nanowires; And / or, the thickness of the transparent cathode layer is 20-200 nm.
3. The electroluminescent device according to claim 1, characterized in that: The electroluminescent unit is formed into a film by coating or printing; And / or, the protective layer is deposited by sputtering and / or atomic layer deposition; And / or, the transparent cathode layer is formed by coating or printing, and then heat-treated at a temperature not exceeding 120°C.
4. The electroluminescent device according to claim 1, characterized in that: When the material of the protective layer is Al2O3 or TiO x When the protective layer has a thickness of 0.5 to 2 nm; Alternatively, when the material of the protective layer is ITO, AZO, ZnO, IZO, IGZO, or TiN, the thickness of the protective layer is 3 to 10 nm.
5. The electroluminescent device according to claim 1, characterized in that: The protective layer comprises a first protective layer and a second protective layer stacked in sequence; the first protective layer is obtained by atomic layer deposition, and the material of the first protective layer is selected from Al2O3, TiO x The thickness of the first protective layer is 0.5 to 2 nm; the second protective layer is obtained by atomic layer deposition or sputtering, the material of the second protective layer is selected from ITO, AZO, ZnO, IZO, IGZO, TiN, and the thickness of the second protective layer is 3 to 10 nm.
6. The electroluminescent device according to any one of claims 1 to 5, characterized in that: The electroluminescent unit comprises a stacked hole transport layer, a light-emitting layer and an electron transport layer, wherein the material of the light-emitting layer is selected from at least one of CdSe and InP-based quantum dot materials; and the material of the electron transport layer is selected from ZnO or ZnMgO.
7. The electroluminescent device according to claim 6, characterized in that: A metal modification layer is provided on the electron transport layer; the metal modification layer is located between the electron transport layer and the protective layer; and the material of the metal modification layer is selected from Al, Mg, and Ga.
8. The method for preparing an electroluminescent device according to any one of claims 1 to 7, characterized in that: The following steps are involved: S1: forming an electroluminescent unit on the transparent anode layer; S2: forming a protective layer on the electroluminescent unit by sputtering and / or atomic layer deposition; S3: forming a transparent cathode layer on the protective layer.
9. The method for preparing an electroluminescent device according to claim 8, characterized in that: The step S3 is: spraying the alcohol solution of silver nanowires on the protective layer at a spraying rate of 0.02 to 0.3 mL / min at a temperature of 40 to 100° C. for 2 to 10 times.
10. Use of the electroluminescent device according to any one of claims 1 to 7 in a light-emitting device or an organic photoelectric device.