Light-emitting device, preparation method thereof and display device

By using block copolymer etching technology, the light-emitting layer is located after the carrier functional layer, which solves the problems of high cost and short lifespan of photolithography process and realizes high brightness and long lifespan of light-emitting device.

CN118922041APending Publication Date: 2024-11-08TCL TECHNOLOGY GROUP CORPORATION
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310512905.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-08
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing back-contact light-emitting devices rely on photolithography, which is costly, time-consuming, and results in a short device lifespan.

Method used

Block copolymers are used to form regular patterns through phase separation, which are then used as masks to etch the functional layers. The light-emitting layer is located after the carrier functional layer to avoid corrosion from the upper solution and to shorten the distance between the positive and negative electrodes to improve the carrier transport efficiency.

Benefits of technology

This improves the stability and brightness of the light-emitting layer, extends the lifespan of the light-emitting device, and reduces manufacturing costs and time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118922041A_ABST
    Figure CN118922041A_ABST
Patent Text Reader

Abstract

The invention discloses a light-emitting device and a preparation method thereof, and a display device, the preparation method comprises the steps: providing a light-emitting device preform, arranging a block copolymer layer on the light-emitting device preform, the block copolymer layer comprises a first region and a plurality of second regions embedded in the first region at intervals, the first region comprises a first polymer, and the second region comprises a second polymer; the second region comprises a second polymer; removing the second region; removing the part, exposed through the segmented copolymer layer, of the prefabricated layer to obtain a patterned prefabricated layer; removing the first region, and performing oxidation treatment on the metal layer in the patterned prefabricated layer to obtain a second electrode combined with the insulating layer and a second carrier functional layer coated on the surface of the second electrode so as to form a patterned electrode-carrier composite layer; and arranging a light-emitting material in the patterning gap of the composite layer to form a light-emitting layer, thereby obtaining the light-emitting device. The method prevents the functional layer solution from corroding the light-emitting layer, shortens the distance between the positive electrode and the negative electrode, and improves the light-emitting efficiency of the device.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of display technology, and in particular to a method for preparing a light-emitting device, a light-emitting device prepared by the method for preparing the light-emitting device, and a display device including the light-emitting device. Background Art

[0002] Currently, the widely used light-emitting devices are organic light-emitting diodes (OLEDs) and quantum dot light-emitting diodes (QLEDs). OLED has become the mainstream technology in the field of display technology due to its excellent display performance, such as self-luminescence, simple structure, ultra-thinness, fast response speed, wide viewing angle, low power consumption, and flexible display. QLED has the advantages of saturated color and adjustable wavelength of emitted light, and high quantum yield of photoluminescence and electroluminescence, and has become a strong competitor of OLED in recent years.

[0003] The structure of traditional OLED and QLED devices generally includes an anode, a hole injection layer, a hole transport layer, a light-emitting layer, an electron transport layer, an electron injection layer and a cathode. Under the action of the electric field, the holes generated by the anode of the light-emitting diode and the electrons generated by the cathode move, are injected into the hole transport layer and the electron transport layer respectively, and finally migrate to the light-emitting layer. When the two meet in the light-emitting layer, energy excitons are generated, thereby exciting the light-emitting molecules to finally produce visible light. The orthogonal solution method is usually used to deposit functional layers such as the hole injection layer, the hole transport layer, the electron transport layer, and the electron injection layer. This method is difficult to avoid damage to the light-emitting layer during material deposition. At the same time, because the light-emitting layer is wrapped in the middle of the functional material, the functional layer will block the fluorescence of the light-emitting layer, affecting the performance of the light-emitting device.

[0004] As a new device structure, the back-contact light-emitting device is prepared in advance, and the light-emitting layer is placed on the top layer of the light-emitting device, thereby improving the performance of the device. However, the back-contact light-emitting device is currently mainly prepared by photolithography, which has extremely stringent requirements on equipment, and has disadvantages such as high cost and long time consumption. In addition, the light-emitting device prepared by the photolithography process still has the problem of short service life. Summary of the invention

[0005] In view of this, the present application provides a method for preparing a light-emitting device, aiming to improve the problem of short service life of existing light-emitting devices.

[0006] The embodiment of the present application is implemented as follows: a method for preparing a light-emitting device comprises the following steps:

[0007] Providing a light-emitting device preform, the light-emitting device preform comprising a first electrode, a first carrier functional layer and a prefabricated layer which are stacked, wherein the prefabricated layer comprises a stacked insulating layer and a metal layer;

[0008] Disposing a block copolymer layer on the prefabricated layer, the block copolymer layer comprising a first region and a plurality of second regions spaced and embedded in the first region, the first region comprising a first polymer, and the second region comprising a second polymer;

[0009] removing the plurality of second regions;

[0010] removing the portion of the prefabricated layer exposed through the block copolymer layer to obtain a patterned prefabricated layer;

[0011] removing the first region, and performing oxidation treatment on the metal layer in the patterned prefabricated layer to obtain a second electrode bonded to the insulating layer and a second carrier functional layer coated on the surface of the second electrode, thereby forming a patterned electrode-carrier composite layer;

[0012] A light-emitting material is arranged in the patterned gaps of the patterned electrode-carrier composite layer to form a light-emitting layer, thereby obtaining a light-emitting device.

[0013] Optionally, in some embodiments of the present application, the first polymer includes PS, PEO, PCL, PAA, PCL, the second polymer includes PMMA, PPO, PEG, PEO, and the first polymer and the second polymer are different; and / or

[0014] The material of the block copolymer layer includes block copolymers, and the block copolymers include PS-b-PMMA, PEO-b-PPO, PCL-b-PEG, PAA-b-PEG, PCL-b-PEO; and / or

[0015] The mass ratio of the first polymer to the second polymer is (50-90):(10-50); and / or

[0016] The area ratio of the first region to the plurality of the second regions is (1-9):1; and / or

[0017] The thickness of the block copolymer layer is 100 to 300 nm; and / or

[0018] The second region is a column extending in a direction away from the metal layer, and the diameter of the column is 300-500 nm.

[0019] Optionally, in some embodiments of the present application, setting a block copolymer layer on the prefabricated layer includes: providing a block copolymer solution, the block copolymer solution including block copolymers, setting the block copolymer solution on the prefabricated layer, and heat-treating the block copolymer solution to phase-separate the block copolymer into a first zone formed by the first polymer and multiple second zones formed by the second polymer, thereby forming a block copolymer layer.

[0020] Optionally, in some embodiments of the present application, in the block copolymer solution, the mass fraction of the block copolymer is 0.5% to 2%; and / or

[0021] The solvent of the block copolymer solution includes one or more of toluene, acetone, tetrahydrofuran, and cyclohexane; and / or

[0022] The temperature of heat treating the block copolymer solution is 110° C. to 160° C.; and / or

[0023] The heat treatment time of the block copolymer solution is 1 hour to 24 hours.

[0024] Optionally, in some embodiments of the present application, the method of removing the plurality of second regions comprises ultraviolet irradiation; and / or

[0025] The method of removing the portion of the prefabricated layer exposed through the block copolymer layer comprises etching; and / or

[0026] The method for removing the first zone comprises one or more of toluene ultrasonic treatment and acetone ultrasonic treatment; and / or

[0027] The method of oxidizing the metal layer in the patterned prefabricated layer includes heating the patterned prefabricated layer in an oxygen-containing atmosphere.

[0028] Optionally, in some embodiments of the present application, the method for removing the metal layer in the portion of the prefabricated layer exposed through the block copolymer layer comprises: immersing the portion of the metal layer exposed through the block copolymer layer in a first metal etching solution, wherein the first metal etching solution comprises one or more of a nickel etching solution, a copper etching solution, a molybdenum etching solution, a titanium etching solution, a zinc etching solution, and a tin etching solution; and / or

[0029] The method for removing the insulating layer in the portion of the prefabricated layer exposed through the block copolymer layer comprises: etching the portion of the insulating layer exposed through the block copolymer layer using an etching gas, wherein the etching gas comprises one or more of doped or undoped He, and the doped gas comprises one or more of C4F8, Ar, O2, CF4, CHF3, C2F6 and SF6; and / or

[0030] The temperature of heating the patterned prefabricated layer is 300° C. to 400° C.; and / or

[0031] The time for heating the patterned prefabricated layer is 30 min to 60 min.

[0032] Optionally, in some embodiments of the present application, the prefabricated layer further includes a barrier layer, and the barrier layer is disposed between the first carrier functional layer and the insulating layer.

[0033] Optionally, in some embodiments of the present application, the material of the barrier layer includes one or more of palladium, platinum, rhodium, iridium, and ruthenium; and / or

[0034] The thickness of the barrier layer is 8 to 15 nm; and / or

[0035] The method of removing the portion of the prefabricated layer exposed through the block copolymer layer also includes removing the portion of the barrier layer exposed through the block copolymer layer. The method of removing the portion of the barrier layer exposed through the block copolymer layer includes: immersing the portion of the barrier layer exposed through the block copolymer layer in a second metal etching solution, wherein the second metal etching solution includes one or more of a palladium etching solution, a platinum etching solution, a rhodium etching solution, an iridium etching solution, and a ruthenium etching solution.

[0036] Optionally, in some embodiments of the present application, the material of the insulating layer includes one or more of SiO2 and Al2O3; and / or

[0037] The material of the metal layer includes one or more of doped or undoped nickel, copper, molybdenum, titanium, zinc, and tin; and / or

[0038] The first electrode comprises one or more of a metal, a carbon material and a metal oxide; the metal comprises one or more of Al, Ag, Cu, Mo, Au, Ba, Ca, Yb and Mg; the carbon material comprises one or more of graphite, carbon nanotubes, graphene and carbon fiber; the metal oxide comprises a metal oxide electrode or a composite electrode in which a metal is sandwiched between doped or undoped transparent metal oxides, the material of the metal oxide electrode comprises one or more of ITO, FTO, ATO, AZO, GZO, IZO, MZO and AMO, and the composite electrode comprises one or more of AZO / Ag / AZO, AZO / Al / AZO, ITO / Ag / ITO, ITO / Al / ITO, ZnO / Ag / ZnO, ZnO / Al / ZnO, ZnS / Ag / ZnS, ZnS / Al / ZnS, TiO2 / Ag / TiO2 and TiO2 / Al / TiO2; and / or

[0039] The first carrier functional layer includes a hole functional layer or an electron functional layer; the hole functional layer includes 4,4'-N,N'-dicarbazolyl-biphenyl, N,N'-diphenyl-N,N'-bis(1-naphthyl)-1,1'-biphenyl-4,4"-diamine, N,N'-diphenyl-N,N'-bis(3-methylphenyl)-(1,1'-biphenyl)-4,4'-diamine (TPD), N,N'-bis(3-methylphenyl)-N,N'-bis(phenyl)-spiro, N,N'-bis(4-(N,N'-diphenyl-amino)phenyl)-N,N'-diphenylbenzidine, 4,4',4'-tri(N-carbazolyl)-triphenylamine, 4,4',4'-tri(carbazol-9-yl)-triphenylamine, Triphenylamine, trichloroisocyanuric acid, terbium-doped phosphate-based green luminescent materials, 2,3,6,7,10,11-hexacyano-1,4,5,8,9,12-hexaazatriphenylene, 4,4',4'-tri(N-3-methylphenyl-N-phenylamino)triphenylamine, poly[(9,9'-dioctylfluorene-2,7-diyl)-co-(4,4'-(N-(4-sec-butylphenyl)diphenylamine))], poly(4-butylphenyl-diphenylamine), poly[bis(4-phenyl)(4-butylphenyl)amine], polyaniline, polypyrrole, poly(p-phenylene vinylene), poly(phenylene vinylene), poly[2-methoxy-5-(2-ethylhexyloxy)-1,4-phenylene vinylene], Poly[2-methoxy-5-(3',7'-dimethyloctyloxy)-1,4-phenylene vinylene], copper phthalocyanine, aromatic tertiary amines, polynuclear aromatic tertiary amines, 4,4'-bis(p-carbazolyl)-1,1'-biphenyl compounds, N,N,N',N'-tetraaryl benzidine, PEDOT, PEDOT:PSS and its derivatives, PEDOT:PSS derivatives doped with s-MoO3, poly(N-vinyl carbazole) and its derivatives, polymethacrylate and its derivatives, poly(9,9-octylfluorene) and its derivatives, poly(spirofluorene) and its derivatives, N,N'-di(naphthalene-1-yl)-N,N'-diphenyl benzidine, spiro NPB, nano-polycrystalline diamond, microcrystalline cellulose and tetra One or more of cyanoquinodimethane, doped graphene, undoped graphene, transition metal oxides, transition metal sulfides, and transition metal tinides; the material of the electronic functional layer includes inorganic materials and / or organic materials, and the inorganic material includes one or more of doped or undoped zinc oxide, barium oxide, nickel oxide, titanium oxide, tin oxide, tantalum oxide, zirconium oxide, nickel oxide, lithium titanium oxide, zinc aluminum oxide, zinc manganese oxide, zinc tin oxide, lithium zinc oxide, indium tin oxide, cadmium sulfide, zinc sulfide, molybdenum sulfide, tungsten sulfide, copper sulfide, zinc tin, indium phosphide, gallium phosphide, copper indium sulfide, copper gallium sulfide, and barium titanate; the doped elements include one or more of aluminum, magnesium, lithium, manganese, yttrium, lanthanum, copper, nickel, zirconium, cerium, and gadolinium;The organic material includes one or more of quinoxaline compounds, imidazole compounds, triazine compounds, fluorene compounds, and hydroxyquinoline compounds; and / or;

[0040] The second carrier functional layer includes a hole functional layer or an electron functional layer. When the second carrier functional layer is a hole functional layer, the material of the second carrier functional layer includes NiO x , CuO x 、MoO x When the second carrier functional layer is an electronic functional layer, the material of the second carrier functional layer includes ZnO x 、TiO x SnO x One or more of; and / or

[0041] The forming of the light-emitting layer further comprises: arranging a light-emitting material on the surface of the patterned electrode-carrier recombination layer; and / or

[0042] The luminescent materials include 4,4'-bis(N-carbazole)-1,1'-biphenyl:tris[2-(p-tolyl)pyridine iridium(III)], 4,4',4"-tris(carbazole-9-yl)triphenylamine:tris[2-(p-tolyl)pyridine iridium], diarylanthracene derivatives, distilbene aromatic derivatives, pyrene derivatives, fluorene derivatives, TBPe fluorescent materials, TTPX fluorescent materials, TBRb fluorescent materials, DBP fluorescent materials, delayed fluorescent materials, TTA materials, TADF materials, polymers containing covalent bonding of BN, HLCT materials, Exciplex luminescent materials, CdS, CdSe, CdTe, ZnS, ZnSe, ZnTe, ZnO, HgS, HgSe, H gTe, CdSeS, CdSeTe, CdSTe, ZnSeS, ZnSeTe, ZnSTe, HgSeS, HgSeTe, HgSTe, CdZnS, CdZnSe, CdZnTe, CdHgS, CdHgSe, CdHgTe, HgZnS, HgZnSe, HgZnTe, CdZ nSeS, CdZnSeTe, CdZnSTe, CdHgSeS, CdHgSeTe, CdHgSTe, HgZnSeS, HgZnSeTe, HgZnSTe, SnS, SnSe, SnTe, PbS, PbSe, PbTe, SnSeS, SnSeTe, SnSTe, PbSeS , PbSeTe, PbSTe, SnPbS, SnPbSe, SnPbTe, SnPbSSe, SnPbSeTe, SnPbSTe, GaN, GaP, GaAs, GaSb, AlN, AlP, AlAs, AlSb, InN, InP, InAs, InSb, GaNP, GaNAs, GaNSb, GaPAs, GaPSb, AlNP, AlNAs, AlNSb, AlPAs, AlPSb, InNP, InNAs, InNSb, InPAs, InPSb, GaAlNP, GaAlNAs, GaAlNSb, GaAlPAs, GaAlPSb, GaInNP, Ga InNAs, GaInNSb, GaInPAs, GaInPSb, InAlNP, InAlNAs, InAlNSb, InAlPAs, InAlPSb, CuInS2, CuInSe2, AgInS2, CdSe / CdSeS / CdS, InP / ZnSeS / ZnS, CdZn One or more of Se / ZnSe / ZnS, CdSeS / ZnSeS / ZnS, CdSe / ZnS, CdSe / ZnSe / ZnS, ZnSe / ZnS, ZnSeTe / ZnS, CdSe / CdZnSeS / ZnS, InP / ZnSe / ZnS, AMX3 and BMX3, where A is Cs+ ion, M is a divalent metal cation selected from Pb 2+ Sn 2+ , Cu 2+ 、Ni 2+ 、Cd 2+ Cr 2+ , Mn 2+ 、Co 2+ , Fe 2+ ,Ge 2+ , Yb 2+ 、Eu 2+ One or more of, X is a halogen anion selected from Cl - Br - ,I - One or more of; B is an organic amine cation selected from CH3(CH2) n-2 NH3 + or [NH3(CH2) n NH3] 2+ , where n≥2.

[0043] Accordingly, an embodiment of the present application further provides a light emitting device, including:

[0044] A stacked first electrode and a first carrier functional layer;

[0045] A patterned functional layer, the patterned functional layer comprising a stacked insulating layer, a second electrode, and a second carrier functional layer, wherein the insulating layer and the second electrode are sequentially stacked on the first carrier functional layer, and the second carrier functional layer is arranged on a side surface of the second electrode and a surface of the second electrode away from the insulating layer;

[0046] The light-emitting layer is disposed in the patterned gap in the patterned functional layer, and the thickness of the light-emitting layer is greater than the thickness of the insulating layer.

[0047] Optionally, in some embodiments of the present application, the thickness of the light-emitting layer is less than or equal to the thickness of the patterned functional layer; or

[0048] The light-emitting layer includes a first light-emitting portion and a plurality of second light-emitting portions, the first light-emitting portion having a first surface, the plurality of second light-emitting portions being arranged at intervals on the first surface and extending in a direction away from the first surface, the plurality of second light-emitting portions being filled in patterned gaps of the patterned functional layer, and an area of ​​the first surface where no second light-emitting portion is arranged is arranged on a surface of the second carrier functional layer away from the first carrier functional layer.

[0049] Optionally, in some embodiments of the present application, the patterned functional layer further includes a barrier layer, and the barrier layer is disposed between the first carrier functional layer and the insulating layer.

[0050] Optionally, in some embodiments of the present application, the material of the barrier layer includes one or more of palladium, platinum, rhodium, iridium, and ruthenium; and / or

[0051] The thickness of the barrier layer is 8 to 15 nm; and / or

[0052] The thickness of the light emitting layer is greater than the sum of the thicknesses of the blocking layer and the insulating layer.

[0053] Optionally, in some embodiments of the present application, the thickness of the first electrode is 90-110 nm; and / or

[0054] The thickness of the first carrier functional layer is 20-40 nm; and / or

[0055] The thickness of the insulating layer is 25 to 35 nm; and / or

[0056] The thickness of the second carrier functional layer is 8-12 nm; and / or

[0057] The thickness of the second electrode is 50-60 nm.

[0058] Optionally, in some embodiments of the present application, the material of the insulating layer includes one or more of SiO2 and Al2O3; and / or

[0059] The first electrode comprises one or more of a metal, a carbon material and a metal oxide; the metal comprises one or more of Al, Ag, Cu, Mo, Au, Ba, Ca, Yb and Mg; the carbon material comprises one or more of graphite, carbon nanotubes, graphene and carbon fiber; the metal oxide comprises a metal oxide electrode or a composite electrode in which a metal is sandwiched between doped or undoped transparent metal oxides, the material of the metal oxide electrode comprises one or more of ITO, FTO, ATO, AZO, GZO, IZO, MZO and AMO, and the composite electrode comprises one or more of AZO / Ag / AZO, AZO / Al / AZO, ITO / Ag / ITO, ITO / Al / ITO, ZnO / Ag / ZnO, ZnO / Al / ZnO, ZnS / Ag / ZnS, ZnS / Al / ZnS, TiO2 / Ag / TiO2 and TiO2 / Al / TiO2; and / or

[0060] The first carrier functional layer includes a hole functional layer or an electron functional layer; the hole functional layer includes 4,4'-N,N'-dicarbazolyl-biphenyl, N,N'-diphenyl-N,N'-bis(1-naphthyl)-1,1'-biphenyl-4,4"-diamine, N,N'-diphenyl-N,N'-bis(3-methylphenyl)-(1,1'-biphenyl)-4,4'-diamine (TPD), N,N'-bis(3-methylphenyl)-N,N'-bis(phenyl)-spiro, N,N'-bis(4-(N,N'-diphenyl-amino)phenyl)-N,N'-diphenylbenzidine, 4,4',4'-tri(N-carbazolyl)-triphenylamine, 4,4',4'-tri(carbazol-9-yl)-triphenylamine, Triphenylamine, trichloroisocyanuric acid, terbium-doped phosphate-based green luminescent materials, 2,3,6,7,10,11-hexacyano-1,4,5,8,9,12-hexaazatriphenylene, 4,4',4'-tri(N-3-methylphenyl-N-phenylamino)triphenylamine, poly[(9,9'-dioctylfluorene-2,7-diyl)-co-(4,4'-(N-(4-sec-butylphenyl)diphenylamine))], poly(4-butylphenyl-diphenylamine), poly[bis(4-phenyl)(4-butylphenyl)amine], polyaniline, polypyrrole, poly(p-phenylene vinylene), poly(phenylene vinylene), poly[2-methoxy-5-(2-ethylhexyloxy)-1,4-phenylene vinylene], Poly[2-methoxy-5-(3',7'-dimethyloctyloxy)-1,4-phenylene vinylene], copper phthalocyanine, aromatic tertiary amines, polynuclear aromatic tertiary amines, 4,4'-bis(p-carbazolyl)-1,1'-biphenyl compounds, N,N,N',N'-tetraaryl benzidine, PEDOT, PEDOT:PSS and its derivatives, PEDOT:PSS derivatives doped with s-MoO3, poly(N-vinyl carbazole) and its derivatives, polymethacrylate and its derivatives, poly(9,9-octylfluorene) and its derivatives, poly(spirofluorene) and its derivatives, N,N'-di(naphthalene-1-yl)-N,N'-diphenyl benzidine, spiro NPB, nano-polycrystalline diamond, microcrystalline cellulose and tetra One or more of cyanoquinodimethane, doped graphene, undoped graphene, transition metal oxides, transition metal sulfides, and transition metal tinides; the material of the electronic functional layer includes inorganic materials and / or organic materials, and the inorganic material includes one or more of doped or undoped zinc oxide, barium oxide, nickel oxide, titanium oxide, tin oxide, tantalum oxide, zirconium oxide, nickel oxide, lithium titanium oxide, zinc aluminum oxide, zinc manganese oxide, zinc tin oxide, lithium zinc oxide, indium tin oxide, cadmium sulfide, zinc sulfide, molybdenum sulfide, tungsten sulfide, copper sulfide, zinc tin, indium phosphide, gallium phosphide, copper indium sulfide, copper gallium sulfide, and barium titanate; the doped elements include one or more of aluminum, magnesium, lithium, manganese, yttrium, lanthanum, copper, nickel, zirconium, cerium, and gadolinium;The organic material includes one or more of quinoxaline compounds, imidazole compounds, triazine compounds, fluorene compounds, and hydroxyquinoline compounds; and / or;

[0061] The second carrier functional layer includes a hole functional layer or an electron functional layer. When the second carrier functional layer is a hole functional layer, the material of the second carrier functional layer includes NiO x , CuO x 、MoO x When the second carrier functional layer is an electronic functional layer, the material of the second carrier functional layer includes ZnO x 、TiO x SnO x One or more of; and / or

[0062] The material of the second electrode includes one or more of Ni, Cu, Mo, Zn, Ti, and Sn; and / or

[0063] The luminescent materials include 4,4'-bis(N-carbazole)-1,1'-biphenyl:tris[2-(p-tolyl)pyridine iridium(III)], 4,4',4"-tris(carbazole-9-yl)triphenylamine:tris[2-(p-tolyl)pyridine iridium], diarylanthracene derivatives, distilbene aromatic derivatives, pyrene derivatives, fluorene derivatives, TBPe fluorescent materials, TTPX fluorescent materials, TBRb fluorescent materials, DBP fluorescent materials, delayed fluorescent materials, TTA materials, TADF materials, polymers containing covalent bonding of BN, HLCT materials, Exciplex luminescent materials, CdS, CdSe, CdTe, ZnS, ZnSe, ZnTe, ZnO, HgS, HgSe, H gTe, CdSeS, CdSeTe, CdSTe, ZnSeS, ZnSeTe, ZnSTe, HgSeS, HgSeTe, HgSTe, CdZnS, CdZnSe, CdZnTe, CdHgS, CdHgSe, CdHgTe, HgZnS, HgZnSe, HgZnTe, CdZ nSeS, CdZnSeTe, CdZnSTe, CdHgSeS, CdHgSeTe, CdHgSTe, HgZnSeS, HgZnSeTe, HgZnSTe, SnS, SnSe, SnTe, PbS, PbSe, PbTe, SnSeS, SnSeTe, SnSTe, PbSeS , PbSeTe, PbSTe, SnPbS, SnPbSe, SnPbTe, SnPbSSe, SnPbSeTe, SnPbSTe, GaN, GaP, GaAs, GaSb, AlN, AlP, AlAs, AlSb, InN, InP, InAs, InSb, GaNP, GaNAs, GaNSb, GaPAs, GaPSb, AlNP, AlNAs, AlNSb, AlPAs, AlPSb, InNP, InNAs, InNSb, InPAs, InPSb, GaAlNP, GaAlNAs, GaAlNSb, GaAlPAs, GaAlPSb, GaInNP, Ga InNAs, GaInNSb, GaInPAs, GaInPSb, InAlNP, InAlNAs, InAlNSb, InAlPAs, InAlPSb, CuInS2, CuInSe2, AgInS2, CdSe / CdSeS / CdS, InP / ZnSeS / ZnS, CdZn One or more of Se / ZnSe / ZnS, CdSeS / ZnSeS / ZnS, CdSe / ZnS, CdSe / ZnSe / ZnS, ZnSe / ZnS, ZnSeTe / ZnS, CdSe / CdZnSeS / ZnS, InP / ZnSe / ZnS, AMX3 and BMX3, where A is Cs+ ion, M is a divalent metal cation selected from Pb 2+ Sn 2+ , Cu 2+ 、Ni 2+ 、Cd 2+ Cr 2+ , Mn 2+ 、Co 2+ , Fe 2+ ,Ge 2+ , Yb 2+ 、Eu 2+ One or more of, X is a halogen anion selected from Cl - Br - ,I - One or more of; B is an organic amine cation selected from CH3(CH2) n-2 NH3 + or [NH3(CH2) n NH3] 2+ , where n≥2.

[0064] Correspondingly, the present application also provides a display device, comprising the above-mentioned light-emitting device.

[0065] The preparation method of the light-emitting device described in the present application utilizes the characteristic of block copolymers to form regular patterns by phase separation, and uses this as a mask to etch the functional layer. On the one hand, the light-emitting layer is prepared after the carrier functional layer, which avoids the corrosion of the light-emitting layer by the upper solution in the previous stacked structure and improves the stability of the light-emitting layer; on the other hand, the preparation method described in the present application greatly reduces the size of the pattern, that is, shortens the distance between the positive and negative electrodes, which can effectively improve the transmission of carriers, enhance the luminous brightness of the light-emitting device, and extend the service life of the light-emitting device. BRIEF DESCRIPTION OF THE DRAWINGS

[0066] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without paying any creative work.

[0067] Figure 1 is a flow chart of a method for preparing a light-emitting device provided in an embodiment of the present application;

[0068] Figure 2 is a schematic structural diagram of a light-emitting device preform provided in an embodiment of the present application;

[0069] Figure 3 It is a schematic structural diagram of a light-emitting device preform provided in an embodiment of the present application after a block copolymer layer is provided;

[0070] Figure 4 This is a schematic diagram of the structure of the light-emitting device preform provided in an embodiment of the present application after PMMA is removed;

[0071] Figure 5 It is a schematic diagram of the structure of the light-emitting device preform provided in an embodiment of the present application after etching the metal layer, the insulating layer and the barrier layer;

[0072] Figure 6 It is a schematic diagram of the structure of the light-emitting device preform provided in an embodiment of the present application after removing PS and forming a second carrier functional layer;

[0073] Figure 7 is a schematic structural diagram of a light-emitting device provided in an embodiment of the present application;

[0074] Figure 8 is a schematic structural diagram of the first electrode and the first carrier functional layer provided in Comparative Example 2 of the present application;

[0075] Fig. 9 It is a schematic diagram of the structure after the photoresist is provided in Comparative Example 2 of the present application;

[0076] Fig.10 It is a schematic diagram of the structure of the photoresist after development provided in Comparative Example 2 of the present application;

[0077] Fig.11 This is a schematic diagram of the structure after the insulating layer and the metal layer are provided in Comparative Example 2 of the present application;

[0078] Fig.12 It is a schematic diagram of the structure after removing the photoresist and forming the second carrier functional layer provided in Comparative Example 2 of the present application;

[0079] Fig.13 It is a schematic diagram of the structure of a quantum dot light-emitting diode provided in Comparative Example 2 of the present application;

[0080] Reference numerals:

[0081] Light-emitting device 100; light-emitting device preform 101; first electrode 10; first carrier functional layer 20; barrier layer 30; insulating layer 40; metal layer 50; second carrier functional layer 501; second electrode 502; block copolymer layer 60; first region 601; second region 602; patterned gap 70; light-emitting layer 80; patterned functional layer 345;

[0082] Cathode 11; electronic functional layer 21; SiO2 layer 41; Ni layer 51; hole functional layer 511; anode 512; photoresist layer 61; first region 611; second region 612; region to be filled 71; quantum dot light-emitting layer 81. DETAILED DESCRIPTION

[0083] The technical solutions in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without making creative work belong to the scope of protection of the present application. In addition, it should be understood that the specific implementation methods described herein are only used to illustrate and explain the present application, and are not used to limit the present application.

[0084] In this application, unless otherwise stated, directional words such as "upper" and "lower" generally refer to the upper and lower parts of the device in actual use or working state, specifically the drawing direction in the accompanying drawings; while "inner" and "outer" refer to the outline of the device. In addition, in the description of this application, the term "including" means "including but not limited to". The terms first, second, third, etc. are used only as labels and do not impose numerical requirements or establish an order.

[0085] In this application, "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural.

[0086] In the present application, "at least one" means one or more, and "plurality" means two or more. "At least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.

[0087] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values ​​within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.

[0088] The technical solution of this application is as follows:

[0089] See also Figure 1 The present invention provides a method for preparing a light emitting device 100, comprising the following steps:

[0090] S11: Please refer to Figure 2 , providing a light emitting device preform 101, wherein the light emitting device preform 101 comprises a first electrode 10, a first carrier functional layer 20 and a prefabricated layer which are stacked, wherein the prefabricated layer comprises a stacked insulating layer 40 and a metal layer 50;

[0091] S12: Please refer to Figure 3 and Figure 4 , a block copolymer layer 60 is disposed on the prefabricated layer, wherein the block copolymer layer 60 includes a first region 601 and a plurality of second regions 602 spaced and embedded in the first region 601, wherein the first region 601 includes a first polymer, and the second region 602 includes a second polymer;

[0092] S13: removing the plurality of second regions 602;

[0093] S14: Please refer to Figure 5 , removing the portion of the prefabricated layer exposed through the block copolymer layer 60 to obtain a patterned prefabricated layer;

[0094] S15: Please refer to Figure 6 , removing the first region 601, and performing oxidation treatment on the metal layer 50 in the patterned prefabricated layer to obtain a second electrode 502 combined with the insulating layer 40 and a second carrier functional layer 501 coated on the surface of the second electrode 502, thereby forming a patterned electrode-carrier composite layer;

[0095] S16: Please refer to Figure 7 A light-emitting material is arranged in the patterned gap 70 of the patterned electrode-carrier recombination layer to form a light-emitting layer 80 , thereby obtaining a light-emitting device 100 .

[0096] The preparation method of the light-emitting device 100 described in the present application utilizes the characteristic of block copolymers to form regular patterns by phase separation, and uses this as a mask to etch the functional layer. On the one hand, the light-emitting layer 80 is prepared after the carrier functional layer, thereby avoiding the corrosion of the light-emitting layer 80 by the upper solution in the previous laminated structure, thereby improving the stability of the light-emitting layer 80; on the other hand, the preparation method described in the present application greatly reduces the size of the pattern, that is, shortens the distance between the positive and negative electrodes, which can effectively improve the transmission of carriers, enhance the luminous brightness of the light-emitting device 100, and extend the service life of the light-emitting device 100; in addition, the preparation method of the light-emitting device 100 omits the cumbersome steps of conventional photolithography and reduces the expensive equipment costs of photolithography.

[0097] In the step S11:

[0098] In some embodiments, the first electrode 10 comprises an electrode known in the art for use in light-emitting devices, for example, independently including but not limited to one or more of metals, carbon materials, and metal oxides. The metal includes one or more of Al, Ag, Cu, Mo, Au, Ba, Ca, Yb and Mg; the carbon material includes one or more of graphite, carbon nanotubes, graphene and carbon fiber; the metal oxide includes a metal oxide electrode or a composite electrode with a metal sandwiched between doped or undoped transparent metal oxides, the material of the metal oxide electrode includes one or more of ITO, FTO, ATO, AZO, GZO, IZO, MZO and AMO, and the composite electrode includes one or more of AZO / Ag / AZO, AZO / Al / AZO, ITO / Ag / ITO, ITO / Al / ITO, ZnO / Ag / ZnO, ZnO / Al / ZnO, ZnS / Ag / ZnS, ZnS / Al / ZnS, TiO2 / Ag / TiO2 and TiO2 / Al / TiO2. Here, “ / ” represents a stacked structure. For example, AZO / Ag / AZO represents a composite electrode including an AZO layer, an Ag layer and an AZO layer stacked in sequence.

[0099] In some embodiments, the first carrier functional layer 20 may include a hole functional layer or an electron functional layer. It is understood that when the first carrier functional layer 20 includes a hole functional layer, in step S16, the second carrier functional layer 501 includes an electron functional layer; when the first carrier functional layer 20 includes an electron functional layer, in step S16, the second carrier functional layer 501 includes a hole functional layer.

[0100] The hole functional layer includes one or more of a hole injection layer and a hole transport layer; the electron functional layer includes one or more of an electron injection layer and an electron transport layer.

[0101] The hole functional layers are independently but not limited to 4,4'-N,N'-dicarbazolyl-biphenyl (CBP), N,N'-diphenyl-N,N'-bis(1-naphthyl)-1,1'-biphenyl-4,4"-diamine (α-NPD), N,N'-diphenyl-N,N'-bis(3-methylphenyl)-(1,1'-biphenyl)-4,4'-diamine (TPD), N,N'-bis(3-methylphenyl)-N,N'-bis(phenyl)-spiro(spiro-TPD), N,N'-bis(4-(N,N'-diphenyl-amino)phenyl)-N,N'-diphenylbenzidine (DNTPD), 4,4',4'-tri(N-carbazolyl)- )-triphenylamine (TCTA), 4,4',4'-tri(carbazole-9-yl)triphenylamine (TCATA), trichloroisocyanuric acid (TCCA), terbium-doped phosphate-based green luminescent material (TAPC), 2,3,6,7,10,11-hexacyano-1,4,5,8,9,12-hexaazatriphenylene (HAT-CN), 4,4',4'-tri(N-3-methylphenyl-N-phenylamino)triphenylamine (m-MTDATA), poly[(9,9'-dioctylfluorene-2,7-diyl)-co-(4,4'-(N-(4-sec-butylphenyl)diphenylamine))] (TFB), poly(4-butylphenyl-diphenylamine) (poly -TPD), poly[bis(4-phenyl)(4-butylphenyl)amine] (Poly-TPD), polyaniline, polypyrrole, poly(p-phenylene vinylene), poly(phenylene vinylene) (PPV), poly[2-methoxy-5-(2-ethylhexyloxy)-1,4-phenylene vinylene] (MEH-PPV), poly[2-methoxy-5-(3',7'-dimethyloctyloxy)-1,4-phenylene vinylene] (MOMO-PPV), copper phthalocyanine, aromatic tertiary amine, polynuclear aromatic tertiary amine, 4,4'-bis(p-carbazolyl)-1,1'-biphenyl compound, N,N,N',N'-tetraarylbenzidine, PEDOT, PED One or more of OT:PSS and its derivatives, PEDOT:PSS derivatives doped with s-MoO3 (PEDOT:PSS:s-MoO3), poly(N-vinylcarbazole) (PVK) and its derivatives, polymethacrylate and its derivatives, poly(9,9-octylfluorene) and its derivatives, poly(spirofluorene) and its derivatives, N,N'-di(naphthalene-1-yl)-N,N'-diphenylbenzidine (NPB), spiro NPB, nano-polycrystalline diamond, microcrystalline cellulose (MCC) and tetracyanoquinodimethane (F4-TCQN), doped graphene, undoped graphene, transition metal oxides, transition metal sulfides, and transition metal tin compounds.

[0102] The materials of the electronic functional layer independently include inorganic materials and / or organic materials. The inorganic materials include one or more of doped or undoped zinc oxide, barium oxide, nickel oxide, titanium oxide, tin oxide, tantalum oxide, zirconium oxide, nickel oxide, lithium titanium oxide, aluminum zinc oxide, manganese zinc oxide, zinc tin oxide, lithium zinc oxide, indium tin oxide, cadmium sulfide, zinc sulfide, molybdenum sulfide, tungsten sulfide, copper sulfide, zinc tin, indium phosphide, gallium phosphide, copper indium sulfide, copper gallium sulfide, and barium titanate, and the doped elements include one or more of aluminum, magnesium, lithium, manganese, yttrium, lanthanum, copper, nickel, zirconium, cerium, and gadolinium; the organic materials include one or more of quinoxaline compounds, imidazole compounds, triazine compounds, fluorene compounds, and hydroxyquinoline compounds.

[0103] In some embodiments, the material of the insulating layer 40 includes one or more of SiO 2 and Al 2 O 3 .

[0104] In some embodiments, the material of the metal layer 50 includes one or more of doped or undoped nickel, copper, molybdenum, titanium, zinc, and tin.

[0105] In some embodiments, the thickness of the first electrode 10 is 90-110 nm.

[0106] In some embodiments, the thickness of the first carrier functional layer 20 is 20-40 nm.

[0107] In some embodiments, the thickness of the metal layer 50 is 55-70 nm.

[0108] In some embodiments, the thickness of the insulating layer 40 is 25-35 nm.

[0109] In some embodiments, the thickness of the second carrier functional layer 501 is 8-12 nm.

[0110] In some embodiments, the thickness of the second electrode 502 is 50-60 nm.

[0111] In some embodiments, the prefabricated layer further includes a barrier layer 30, and the barrier layer 30 is disposed between the first carrier functional layer 20 and the insulating layer 40. It can be understood that when the insulating layer 40 is removed by an ion gas etching method, the ion gas is prone to etching the first carrier functional layer 20, thereby affecting the transmission of carriers by the first carrier functional layer 20, and the barrier layer 30 can protect the first carrier functional layer 20 from being etched by the ion gas.

[0112] In some embodiments, the material of the barrier layer 30 includes one or more of palladium, platinum, rhodium, iridium, and ruthenium.

[0113] In some embodiments, the barrier layer 30 has a thickness of 8-15 nm.

[0114] In step S12:

[0115] In some embodiments, the area ratio of the first region 601 to the plurality of second regions 602 is (1-9):1, for example, (2-8):1, (3-7):1, (4-6):1, 5:1, etc.

[0116] In some embodiments, the mass ratio of the first polymer to the second polymer is (50-90): (10-50), for example, (50-90): (10-50), (55-88): (12-40), (58-80): (20-42), (60-75): (25-40), (65-70): (30-35), etc. In this way, the block copolymer can be microphased, and the second polymer forms a columnar structure, which is dispersed in the interconnect mask pattern formed by the first polymer.

[0117] In some embodiments, the first polymer includes PS (polystyrene), PEO (polyethylene oxide), PCL (polycaprolactone), PAA (polyacrylic acid), PCL (polycaprolactone), and the second polymer includes PMMA (polymethyl methacrylate), PPO (polypropylene ether), PEG (polyethylene glycol), PEO (polyethylene oxide), and the first polymer and the second polymer are different.

[0118] In some embodiments, the material of the block copolymer layer 60 includes block copolymers, and the block copolymers include PS-b-PMMA (polystyrene-b-polymethyl methacrylate), PEO-b-PPO (polyethylene oxide-b-polypropylene ether), PCL-b-PEG (polycaprolactone-b-polyethylene glycol), PAA-b-PEG (polyacrylic acid-b-polyethylene glycol), and PCL-b-PEO (polycaprolactone-b-polyethylene oxide).

[0119] In some embodiments, the thickness of the block copolymer layer 60 is 100-300 nm, for example, 110-290 nm, 120-280 nm, 130-270 nm, 140-250 nm, 180-200 nm, etc. Within the thickness range, the metal layer 50, the insulating layer 40 and the barrier layer 30 of the prefabricated layer below the first region 601 can be effectively protected from being etched.

[0120] In some embodiments, the second region 602 is a column extending in a direction away from the metal layer 50, and the diameter of the column is 300-500 nm, for example, 320-480 nm, 340-460 nm, 360-440 nm, 380-420 nm, 390-400 nm, etc. Within the diameter range, it is beneficial to fill the light-emitting material and transport and recombine the carriers, thereby improving the performance of the light-emitting device.

[0121] Each second region 602 is a columnar structure and is embedded in the first region 601 at intervals.

[0122] In some embodiments, setting the block copolymer layer 60 on the prefabricated layer includes: providing a block copolymer solution, the block copolymer solution including block copolymers, setting the block copolymer solution on the prefabricated layer, and heat-treating the block copolymer solution to separate the block copolymers into a first zone 601 formed by the first polymer and multiple second zones 602 formed by the second polymer, thereby forming a block copolymer layer 60.

[0123] In some embodiments, the solvent of the block copolymer solution includes one or more of toluene, acetone, tetrahydrofuran, and cyclohexane.

[0124] In some embodiments, in the block copolymer solution, the mass fraction of the block copolymer is 0.5% to 2%, for example, 0.6% to 1.8%, 0.8% to 1.5%, 0.9% to 1.4%, 1% to 1.3%, 1.1% to 1.2%, etc. If the mass fraction is too high, the block copolymer is easy to form a multilayer structure, if the mass fraction is too low, the PS is not easy to form a complete mask pattern, within the mass fraction range, a complete single-layer film can be formed.

[0125] In some embodiments, the temperature for heat treating the block copolymer solution is 110°C to 160°C, for example, 112°C to 158°C, 115°C to 152°C, 118°C to 150°C, 120°C to 140°C, 130°C to 135°C, etc. Within the temperature range, the block copolymer is conducive to softening and microphase separation.

[0126] In some embodiments, the heat treatment time of the block copolymer solution is 1 h to 24 h, for example, 2 h to 22 h, 5 h to 20 h, 6 h to 18 h, 8 h to 15 h, 10 h to 12 h, etc. Within the heat treatment time range, the first polymer and the second polymer can be fully microphased.

[0127] In step S13:

[0128] In some embodiments, the method of removing the plurality of second regions 602 comprises ultraviolet irradiation. After removing the plurality of second regions 602, the first region 601 can act as a mask during etching.

[0129] In step S14:

[0130] In some embodiments, the method of removing the portion of the prefabricated layer exposed through the block copolymer layer 60 comprises etching.

[0131] In some embodiments, the etching method of the metal layer 50 includes dry etching or wet etching, the dry etching includes one or more of plasma etching, reactive ion etching, sputtering etching, ion beam etching, reactive ion beam etching, and laser etching, and the wet etching includes chemical corrosion.

[0132] In at least one embodiment, the method for removing the metal layer 50 in the portion of the prefabricated layer exposed by the block copolymer layer 60 is chemical etching. Specifically, the metal layer 50 is immersed in a first metal etching solution and taken out after the metal layer 50 exposed by the block copolymer layer 60 is completely removed.

[0133] The first metal etching liquid includes, but is not limited to, one or more of a nickel etching liquid, a copper etching liquid, a molybdenum etching liquid, a titanium etching liquid, a zinc etching liquid, and a tin etching liquid.

[0134] In some embodiments, the etching method of the insulating layer 40 includes dry etching, and the dry etching includes one or more of plasma etching, reactive ion etching, sputtering etching, ion beam etching, reactive ion beam etching, and laser etching.

[0135] In at least one embodiment, the method for removing the insulating layer 40 in the portion of the prefabricated layer exposed through the block copolymer layer 60 is reactive ion etching, specifically, an etching gas is used to etch the portion of the insulating layer 40 exposed through the block copolymer layer 60. The etching gas includes one or more of doped or undoped He, and the doped gas includes one or more of C4F8, Ar, O2, CF4, CHF3, C2F6 and SF6.

[0136] In some embodiments, when the prefabricated layer includes a barrier layer 30, the etching method of the barrier layer 30 includes dry etching or wet etching, the dry etching includes laser etching, and the wet etching includes chemical etching. It can be understood that the laser etching and the chemical etching can avoid corrosion of the first carrier function layer 20.

[0137] In at least one embodiment, the barrier layer 30 is etched by chemical etching. Specifically, the barrier layer 30 is immersed in a second metal etching solution and taken out after the barrier layer 30 exposed by the block copolymer layer 60 is completely removed.

[0138] The second metal etching solution includes, but is not limited to, one or more of a palladium etching solution, a platinum etching solution, a rhodium etching solution, an iridium etching solution, and a ruthenium etching solution.

[0139] In some embodiments, when the prefabricated layer also includes a barrier layer 30, the removing of the portion of the prefabricated layer exposed through the block copolymer layer 60 also includes removing the portion of the barrier layer 30 exposed through the block copolymer layer 60, and the method for removing the portion of the barrier layer 30 exposed through the block copolymer layer 60 includes: immersing the portion of the barrier layer 30 exposed through the block copolymer layer 60 in a second metal corrosion liquid, wherein the second metal corrosion liquid includes one or more of a palladium corrosion liquid, a platinum corrosion liquid, a rhodium corrosion liquid, an iridium corrosion liquid, and a ruthenium corrosion liquid.

[0140] In step S15:

[0141] In some embodiments, the method for removing the first zone 601 includes one or more of toluene ultrasonic treatment and acetone ultrasonic treatment.

[0142] In some embodiments, the method of oxidizing the metal layer 50 in the patterned prefabricated layer includes heating the patterned prefabricated layer in an oxygen-containing atmosphere.

[0143] In some embodiments, the temperature of heating the patterned prefabricated layer is 300° C. to 400° C., for example, 305° C. to 395° C., 310° C. to 390° C., 320° C. to 380° C., 330° C. to 370° C., 340° C. to 360° C., etc.; the time of heating the patterned prefabricated layer is 30 min to 60 min, for example, 32 min to 58 min, 35 min to 56 min, 38 min to 55 min, 40 min to 52 min, 45 min to 50 min, etc. Under the heating conditions, effective oxidation of the metal layer 50 can be ensured.

[0144] In some embodiments, the second carrier functional layer 501 may be a hole functional layer or an electron functional layer. When the second carrier functional layer 501 is a hole functional layer, the material of the metal layer 50 includes nickel, copper, and molybdenum. The material of the second carrier functional layer 501 includes NiO x , CuO x 、MoO xWhen the second carrier functional layer 501 is an electronic functional layer, the material of the metal layer 50 includes zinc, titanium, and tin, and the material of the second carrier functional layer 501 includes ZnO x 、TiO x SnO x .

[0145] The hole functional layer includes one or more of a hole injection layer and a hole transport layer; the electron functional layer includes one or more of an electron injection layer and an electron transport layer.

[0146] In step S16:

[0147] In some embodiments, the forming of the light-emitting layer 80 also includes: disposing a light-emitting material on the surface of the patterned electrode-carrier recombination layer, so that the light-emitting layer 80 includes a portion filling in the patterned gap 70 of the patterned electrode-carrier recombination layer and a portion bonded to the surface of the patterned electrode-carrier recombination layer.

[0148] In some embodiments, the light-emitting material includes one or more of an organic light-emitting material and a quantum dot light-emitting material.

[0149] The organic light-emitting material can be selected from but not limited to CBP:Ir(mppy)3(4,4'-bis(N-carbazole)-1,1'-biphenyl:tris[2-(p-tolyl)pyridine iridium(III)]), TCTX:Ir(mmpy)(4,4',4"-tris(carbazole-9-yl)triphenylamine:tris[2-(p-tolyl)pyridine iridium]), diaromatic anthracene derivatives, distilbene aromatic derivatives, pyrene derivatives, fluorene derivatives, TBPe fluorescent materials, TTPX fluorescent materials, TBRb fluorescent materials, DBP fluorescent materials, delayed fluorescent materials, TTA materials, TADF (thermally activated delay) materials, polymers containing covalent bonds of BN, HLCT (hybridized localized charge transfer excited state) materials, and Exciplex (exciplex) light-emitting materials.

[0150] The quantum dot light-emitting material may be selected from, but not limited to, one or more of single structure quantum dots, core-shell structure quantum dots and perovskite semiconductor materials.

[0151] The material of the single structure quantum dot, the core material of the core-shell structure quantum dot and the shell material of the core-shell structure quantum dot can be respectively selected from, but not limited to, the single structure quantum dot is selected from one or more of II-VI group compounds, IV-VI group compounds, III-V group compounds and I-III-VI group compounds; the II-VI group compound can be selected from, but not limited to, CdS, CdSe, CdTe, ZnS, ZnSe, ZnTe, HgS, HgSe, HgTe, CdSeS, CdSeTe, CdSTe, ZnSeS, ZnSeTe, ZnSTe, HgSeS, HgSeTe, HgSTe, CdZnS, CdZnSe, CdZnTe, CdHgS, One or more of CdHgSe, CdHgTe, HgZnS, HgZnSe, HgZnTe, CdZnSeS, CdZnSeTe, CdZnSTe, CdHgSeS, CdHgSeTe, CdHgSTe, HgZnSeS, HgZnSeTe and HgZnSTe; the IV-VI group compound can be selected from but not limited to one or more of SnS, SnSe, SnTe, PbS, PbSe, PbTe, SnSeS, SnSeTe, SnSTe, PbSeS, PbSeTe, PbSTe, SnPbS, SnPbSe, SnPbTe, SnPbSSe, SnPbSeTe and SnPbSTe. The III-V group compound may be selected from but not limited to one or more of GaN, GaP, GaAs, GaSb, AlN, AlP, AlAs, AlSb, InN, InP, InAs, InSb, GaNP, GaNAs, GaNSb, GaPAs, GaPSb, AlNP, AlNAs, AlNSb, AlPAs, AlPSb, InNP, InNAs, InNSb, InPAs, InPSb, GaAlNP, GaAlNAs, GaAlNSb, GaAlPAs, GaAlPSb, GaInNP, GaInNAs, GaInNSb, GaInPAs, GaInPSb, InAlNP, InAlNAs, InAlNSb, InAlPAs and InAlPSb; the I-III-VI group compound may be selected from but not limited to one or more of CuInS2, CuInSe2 and AgInS2.

[0152] As an example, the core-shell structured quantum dots may be selected from but not limited to one or more of CdSe / CdSeS / CdS, InP / ZnSeS / ZnS, CdZnSe / ZnSe / ZnS, CdSeS / ZnSeS / ZnS, CdSe / ZnS, CdSe / ZnSe / ZnS, ZnSe / ZnS, ZnSeTe / ZnS, CdSe / CdZnSeS / ZnS and InP / ZnSe / ZnS.

[0153] The perovskite semiconductor material may be selected from, but not limited to, doped or undoped inorganic perovskite semiconductors, or organic-inorganic hybrid perovskite semiconductors. The inorganic perovskite semiconductor has a general structural formula of AMX3, wherein A is Cs + ion, M is a divalent metal cation selected from Pb 2+ Sn 2+ , Cu 2+ 、Ni 2+ 、Cd 2+ Cr 2+ , Mn 2+ 、Co 2+ , Fe 2+ ,Ge 2+ , Yb 2+ 、Eu 2+ One or more of, X is a halogen anion selected from Cl - Br - ,I - One or more of the following; the general structural formula of the organic-inorganic hybrid perovskite semiconductor is BMX3, wherein B is an organic amine cation selected from CH3(CH2) n-2 NH3 + or [NH3(CH2) n NH3] 2+ , where n≥2, M is a divalent metal cation selected from Pb 2+ Sn 2+ , Cu 2+ 、Ni 2+ 、Cd 2+ Cr 2+ , Mn 2+ 、Co 2+ , Fe 2+ ,Ge 2+ , Yb 2+ 、Eu 2+ One or more of, X is a halogen anion selected from Cl - Br - ,I - One or more of the .

[0154] The light emitting device 100 is a back contact light emitting device.

[0155] The method for forming the insulating layer 40, the metal layer 50, the block copolymer layer 60 and the light-emitting layer 80 can be implemented by conventional techniques in the art, such as chemical methods or physical methods. Among them, the chemical method includes chemical vapor deposition, continuous ion layer adsorption and reaction, anodization, electrolytic deposition, and coprecipitation. The physical method includes physical plating and solution method, among which the physical plating method includes: thermal evaporation coating, electron beam evaporation coating, magnetron sputtering, multi-arc ion plating, physical vapor deposition, atomic layer deposition, pulsed laser deposition, etc.; the solution method can be spin coating, printing, inkjet printing, blade coating, printing, dip-pull method, immersion method, spraying, roll coating, casting, slit coating and strip coating, etc.

[0156] See also Figure 7 , the embodiment of the present application further provides a light emitting device 100, the light emitting device 100 comprising a stacked first electrode 10 and a first carrier functional layer 20;

[0157] A patterned functional layer 345, wherein the patterned functional layer 345 includes a stacked insulating layer 40, a second electrode 502, and a second carrier functional layer 501, wherein the insulating layer 40 and the second electrode 502 are sequentially stacked on the first carrier functional layer 20, and the second carrier functional layer 501 is arranged on the side of the second electrode 502 and the surface of the second electrode 502 away from the insulating layer 40;

[0158] The light emitting layer 80 is disposed in the patterned gap 70 in the patterned functional layer, and the thickness of the light emitting layer 80 is greater than the thickness of the insulating layer 40 .

[0159] In some embodiments, the thickness of the light emitting layer 80 is less than or equal to the thickness of the patterned functional layer 345 .

[0160] In some embodiments, the light-emitting layer 80 includes a first light-emitting portion and a plurality of second light-emitting portions, the first light-emitting portion having a first surface, the plurality of second light-emitting portions being arranged at intervals on the first surface and extending in a direction away from the first surface, the plurality of second light-emitting portions being filled in patterned gaps of the patterned functional layer, and an area of ​​the first surface where no second light-emitting portion is arranged is arranged on a surface of the second carrier functional layer 501 away from the first carrier functional layer 20.

[0161] In some embodiments, the thickness of the first electrode 10 is 90-100 nm.

[0162] In some embodiments, the thickness of the first carrier functional layer 20 is 20-40 nm.

[0163] In some embodiments, the thickness of the insulating layer 40 is 25-35 nm.

[0164] In some embodiments, the thickness of the second carrier functional layer 501 is 8-12 nm.

[0165] In some embodiments, the thickness of the second electrode 502 is 50-60 nm.

[0166] In some embodiments, the second light emitting portion is columnar, and a diameter of the column is 300-500 nm.

[0167] In some embodiments, the patterned functional layer further includes a barrier layer 30 , and the barrier layer 30 is disposed between the first carrier functional layer 20 and the insulating layer 40 .

[0168] In some embodiments, the barrier layer 30 has a thickness of 8-15 nm.

[0169] In some embodiments, when the patterned functional layer includes a barrier layer 30 , the thickness of the light emitting layer 80 is greater than the sum of the thicknesses of the barrier layer 30 and the insulating layer 40 .

[0170] The light emitting device 100 is a back contact light emitting device.

[0171] The materials of the first electrode 10 , the first carrier functional layer 20 , the barrier layer 30 , the insulating layer 40 , the second carrier functional layer 501 , the second electrode 502 and the light emitting layer 80 are as described above and will not be described again here.

[0172] The light-emitting device 100 described in the present application is manufactured by setting up block copolymer etching, which has low manufacturing cost and short production time. The light-emitting layer 80 is located at the top layer, which avoids corrosion of the light-emitting layer 80 by other functional layers, and can improve the stability of the light-emitting layer 80. At the same time, the distance between the positive and negative electrodes of this light-emitting device 100 is small, which can effectively improve the transmission efficiency of carriers, thereby improving the luminous brightness of the light-emitting device 100 and extending the service life of the light-emitting device 100.

[0173] The embodiment of the present application further provides a display device, which includes the light-emitting device 100 described above.

[0174] The display device can be any electronic product with a display function, including but not limited to smart phones, tablet computers, laptops, digital cameras, digital video cameras, smart wearable devices, smart weighing electronic scales, car displays, televisions or e-book readers, among which smart wearable devices can be, for example, smart bracelets, smart watches, virtual reality (VR) helmets, etc.

[0175] The present application is described in detail below through specific embodiments. The following embodiments are only partial embodiments of the present application and are not limitations of the present application.

[0176] Example 1

[0177] This embodiment provides a quantum dot light emitting diode, and the preparation method thereof is as follows:

[0178] The ITO glass sheet was placed in a glass dish filled with ethanol solution, and ultrasonicated with acetone, deionized water, and ethanol for 20 minutes in sequence, and then dried with a nitrogen gun; then, the cleaned ITO glass sheet was placed in oxygen plasma for further cleaning for 10 minutes; the surface of the ITO substrate was treated with ultraviolet-ozone irradiation for 15 minutes to obtain a cathode;

[0179] A ZnO dispersion with a concentration of 30 mg / mL was spin-coated on the above ITO substrate at a rotation speed of 3000 r / min for 30 s, and annealed at 80° C. for 30 min to form an electron transport layer with a thickness of 30 nm;

[0180] At a vacuum degree of 1x10 -6 Under the condition of 100 mbar, Pd for 100 s, SiO2 for 300 s and Ni for 600 s were sequentially evaporated on the electronic functional layer at a rate of 1 angstrom / s to form a 10 nm barrier layer, a 30 nm insulating layer and a 60 nm metal layer;

[0181] Providing a PS-b-PMMA solution dissolved in toluene, wherein the mass fraction of PS-b-PMMA is 1%, and the mass ratio of PS to PMMA is 70:30, and spin-coating the PS-b-PMMA solution on the metal layer at a rotation speed of 3000 r / min for 30 seconds to form a block copolymer layer with a thickness of 300 nm;

[0182] The samples were placed in a vacuum of 100 mTorr, heated at 160 °C for 2 h, and then exposed to a laser at 254 nm and an irradiation intensity of 10 mW / cm 2 The film was exposed to ultraviolet light for 3 min, then ultrasonicated in acetic acid for 3 min, rinsed with deionized water and dried under nitrogen to form a honeycomb mask pattern formed by PS;

[0183] The sample was placed in a nickel etching solution (Nickel Etch TFP, Transene Company, Inc), soaked for 30 seconds, taken out, rinsed with deionized water and dried to etch Ni; then placed in a reactive ion beam etching device, with a gas flow rate of 70sccm He and 22sccm C4F8, 150W RF and 2000W ICP parameters, treated for 2 minutes to etch SiO2; then placed in a palladium etching solution (Palladium Etch TFP, Transene Company, Inc), soaked for 10 seconds, taken out, rinsed with deionized water and dried to etch Pd to obtain the part to be filled; finally, the sample was placed in toluene and ultrasonicated for 10 minutes to remove PS;

[0184] The above samples were placed on a 300°C hot plate and heated for 30 min to oxidize the Ni surface to form NiO. x The hole transport layer, the unoxidized part of Ni forms the anode;

[0185] Spin coating a 20 mg / mL CdSe n-octane solution on the to-be-filled portion of the sample and the surface of the hole transport layer away from the electron transport layer at a rotation speed of 2000 r / min for 30 s to form a light-emitting layer with a thickness of 100 nm;

[0186] Encapsulation is performed to obtain a quantum dot light emitting diode.

[0187] Example 2

[0188] This embodiment is substantially the same as Embodiment 1, except that, in this embodiment, the mass ratio of PS to PMMA is 90:10.

[0189] Example 3

[0190] This embodiment is substantially the same as Embodiment 1, except that, in this embodiment, the mass ratio of PS to PMMA is 50:50.

[0191] Example 4

[0192] This embodiment is substantially the same as Embodiment 1, except that in this embodiment, the material Pd of the barrier layer is replaced by Pt.

[0193] Example 5

[0194] This embodiment is basically the same as Embodiment 1, except that in this embodiment, the material SiO2 of the insulating layer is replaced by Al2O3.

[0195] Example 6

[0196] This embodiment is basically the same as the embodiment 1, except that in this embodiment, NiO is first formed on the ITO substrate. x The hole transport layer and the metal layer are made of Zn, which is finally oxidized to ZnO x Electron transport layer.

[0197] Example 7

[0198] This embodiment is substantially the same as Embodiment 1, except that in this embodiment, PS-b-PMMA is replaced by PEO-b-PPO.

[0199] Comparative Example 1

[0200] This comparative example is substantially the same as Example 1, except that a stacked cathode, an electron transport layer, a light-emitting layer, a hole transport layer and an anode are prepared in sequence.

[0201] Comparative Example 2

[0202] The quantum dot light-emitting diode in this comparative example is prepared by photolithography, and the specific method is as follows:

[0203] See also Figure 8 , placing an ITO glass sheet in a glass dish filled with an ethanol solution, and then ultrasonically treating with acetone, deionized water, and ethanol for 20 minutes in sequence, and then drying with a nitrogen gun; then, placing the cleaned ITO glass sheet in an oxygen plasma and continuing to clean for 10 minutes; treating the surface of the ITO substrate with ultraviolet-ozone irradiation for 15 minutes to obtain a cathode 11; spin coating a ZnO dispersion with a concentration of 30 mg / mL on the ITO substrate, the rotation speed is 3000 r / min, the spin coating time is 30 seconds, and annealing is performed at 80°C for 30 minutes to form an electronic functional layer 21 with a thickness of 30 nm;

[0204] See also Fig. 9 and Fig.10 , in a class 100 yellow light clean room, spin-coating AZ1512 photoresist on the above ITO substrate at a rotation speed of 3000 r / min, a spin coating time of 30 seconds, and heating treatment at 110° C. for 2 minutes to form a photoresist layer 61 with a thickness of 1200 nm; using a honeycomb photolithography mask to expose under UV light for 5 seconds, and then developing the exposed sample in AZ726 developer for 25 seconds to obtain a plurality of first regions 611 formed by the photoresist, and a plurality of exposed second regions 612;

[0205] See also Fig.11 , at a vacuum degree of 3x10 -4 Under the condition of mbar, SiO2 for 300s and Ni for 600s are sequentially evaporated on the exposed second area 612 at a rate of 1 angstrom / s to form a 30nm SiO2 layer 41 and a 60nm Ni layer 51;

[0206] See also Fig.12 The sample was placed in acetone and the photoresist was removed by ultrasonic wave to obtain the area to be filled 71; then the sample was placed on a hot plate at 300°C and heated for 30 minutes to oxidize the Ni surface to form NiO x Hole functional layer 511, unoxidized Ni forms anode 512;

[0207] See also Fig.13 , spin-coat a 20 mg / mL CdSe n-octane solution on the to-be-filled area 71 of the sample and the surface of the hole functional layer 511 away from the electron functional layer 21, at a rotation speed of 2000 r / min and a spin coating time of 30 s to form a quantum dot light-emitting layer 81 with a thickness of 100 nm;

[0208] Encapsulation is performed to obtain a quantum dot light emitting diode.

[0209] The 128-channel lifetime test system customized by Guangzhou New Vision Company was used to test the lifetime T95 and lifetime T95@1knit (lifetime at brightness of 1000nit) of the quantum dot light-emitting diodes prepared in Examples 1 to 6 and Comparative Examples 1 to 2. The system architecture is that a 2mA constant current source drives the quantum dot light-emitting diode to test the change in voltage or current. The photodiode detector and the test system test the brightness (photocurrent) change of the light-emitting device. The brightness meter tests and calibrates the brightness (photocurrent) of the electroluminescent device to obtain the lifetime T95 and the time taken for the initial brightness of the light-emitting device to decay to 95%. The time taken for the initial brightness of the light-emitting device to decay to 95% is converted to the aging time at 1000nit to obtain the lifetime T95@1000nit.

[0210] The maximum brightness of the quantum dot light-emitting diodes prepared in Examples 1 to 6 and Comparative Examples 1 to 2 was tested using a brightness meter PR650.

[0211] The test results of lifespan T95, lifespan T95@1knit and maximum brightness are shown in Table 1.

[0212] Table 1

[0213]

[0214] From Table 1, we can see that:

[0215] Compared with the quantum dot light-emitting diode of the traditional structure of comparative example 1, the back-contact quantum dot light-emitting diode prepared by the photolithography method of comparative example 2 and the block copolymer method of examples 1 to 7 has higher maximum brightness and longer service life; compared with the quantum dot light-emitting device prepared by the photolithography method of comparative example 2, the maximum brightness of the quantum dot light-emitting diode prepared by the block copolymer method of examples 1 to 7 is increased by 843 to 1932 nit, the lifespan T95 is not much different, and the lifespan T95@1000 nit is extended by 4.6 to 22.4 h; it can be seen from example 1, example 7 and comparative examples 1 to 2 that whether the light-emitting device is prepared by PS-b-PMMA block copolymer or PEO-b-PPO block copolymer, the maximum brightness of the light-emitting device can be effectively improved and the service life of the light-emitting device can be extended. Compared with the light-emitting device of example 7 prepared by PEO-b-PPO block copolymer, the light-emitting device of example 1 prepared by PS-b-PMMA block copolymer has higher maximum brightness and longer service life.

[0216] Compared with Comparative Example 1, in which a stacked cathode, electron transport layer, light-emitting layer, hole transport layer and anode are prepared in sequence, the block copolymer method provided in Examples 1 to 7 prepares the light-emitting device, and finally arranges the light-emitting layer so that the light-emitting layer is located at the top, thereby avoiding corrosion of the light-emitting layer by other functional layers, thereby improving the stability of the light-emitting layer, and the spacing between the positive and negative electrodes of the light-emitting devices in Examples 1 to 7 is small, which can effectively improve the carrier transmission efficiency, thereby improving the luminous brightness of the light-emitting device and extending the service life of the light-emitting device; compared with Comparative Example 2, in which the light-emitting device is prepared by photolithography, the block copolymers used in Examples 1 to 7 have a lower cost and can improve the preparation and production efficiency of the light-emitting device, while also improving the maximum brightness and service life of the light-emitting device, and are suitable for large-scale promotion and application.

[0217] In summary, the use of block copolymer method to prepare quantum dot light-emitting diodes can effectively improve the luminous efficiency of light-emitting devices and extend the service life of light-emitting devices.

[0218] The light-emitting device and its preparation method, and the display device provided in the embodiments of the present application are introduced in detail above. Specific examples are used in this article to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the method of the present application and its core idea; at the same time, for technical personnel in this field, according to the idea of ​​the present application, there will be changes in the specific implementation method and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.

Claims

1. A method for preparing a light-emitting device, characterized in that: The steps include: Providing a light-emitting device preform, the light-emitting device preform comprising a first electrode, a first carrier functional layer and a prefabricated layer which are stacked, wherein the prefabricated layer comprises a stacked insulating layer and a metal layer; Disposing a block copolymer layer on the prefabricated layer, the block copolymer layer comprising a first region and a plurality of second regions spaced and embedded in the first region, the first region comprising a first polymer, and the second region comprising a second polymer; removing the plurality of second regions; removing the portion of the prefabricated layer exposed through the block copolymer layer to obtain a patterned prefabricated layer; removing the first region, and performing oxidation treatment on the metal layer in the patterned prefabricated layer to obtain a second electrode bonded to the insulating layer and a second carrier functional layer coated on the surface of the second electrode, thereby forming a patterned electrode-carrier composite layer; A light-emitting material is arranged in the patterned gaps of the patterned electrode-carrier composite layer to form a light-emitting layer, thereby obtaining a light-emitting device.

2. The preparation method according to claim 1, characterized in that The first polymer includes PS, PEO, PCL, PAA, PCL, the second polymer includes PMMA, PPO, PEG, PEO, and the first polymer and the second polymer are different; and / or The material of the block copolymer layer includes block copolymers, and the block copolymers include PS-b-PMMA, PEO-b-PPO, PCL-b-PEG, PAA-b-PEG, PCL-b-PEO; and / or The mass ratio of the first polymer to the second polymer is (50-90):(10-50); and / or The area ratio of the first region to the plurality of the second regions is (1-9):1; and / or The thickness of the block copolymer layer is 100 to 300 nm; and / or The second region is a column extending in a direction away from the metal layer, and the diameter of the column is 300-500 nm.

3. The preparation method according to claim 1, characterized in that: The method of arranging the block copolymer layer on the prefabricated layer comprises: providing a block copolymer solution, wherein the block copolymer solution comprises a block copolymer, arranging the block copolymer solution on the prefabricated layer, and heat-treating the block copolymer solution to separate the block copolymer into a first zone formed by the first polymer and a plurality of second zones formed by the second polymer, thereby forming a block copolymer layer.

4. The preparation method according to claim 3, characterized in that: In the block copolymer solution, the mass fraction of the block copolymer is 0.5% to 2%; and / or The solvent of the block copolymer solution includes one or more of toluene, acetone, tetrahydrofuran, and cyclohexane; and / or The temperature of heat treating the block copolymer solution is 110° C. to 160° C.; and / or The heat treatment time of the block copolymer solution is 1 hour to 24 hours.

5. The preparation method according to claim 1, characterized in that: The method of removing the plurality of second regions comprises ultraviolet irradiation; and / or The method of removing the portion of the prefabricated layer exposed through the block copolymer layer comprises etching; and / or The method for removing the first zone comprises one or more of toluene ultrasonic treatment and acetone ultrasonic treatment; and / or The method of oxidizing the metal layer in the patterned prefabricated layer includes heating the patterned prefabricated layer in an oxygen-containing atmosphere.

6. The preparation method according to claim 5, characterized in that: The method for removing the metal layer in the portion of the prefabricated layer exposed through the block copolymer layer comprises: immersing the portion of the metal layer exposed through the block copolymer layer in a first metal etching solution, wherein the first metal etching solution comprises one or more of a nickel etching solution, a copper etching solution, a molybdenum etching solution, a titanium etching solution, a zinc etching solution, and a tin etching solution; and / or The method for removing the insulating layer in the portion of the prefabricated layer exposed through the block copolymer layer comprises: etching the portion of the insulating layer exposed through the block copolymer layer using an etching gas, wherein the etching gas comprises one or more of doped or undoped He, and the doped gas comprises one or more of C4F8, Ar, O2, CF4, CHF3, C2F6 and SF6; and / or The temperature of heating the patterned prefabricated layer is 300° C. to 400° C.; and / or The time for heating the patterned prefabricated layer is 30 min to 60 min.

7. The preparation method according to claim 1, characterized in that: The prefabricated layer further includes a barrier layer, and the barrier layer is arranged between the first carrier functional layer and the insulating layer.

8. The preparation method according to claim 7, characterized in that: The material of the barrier layer includes one or more of palladium, platinum, rhodium, iridium and ruthenium; and / or The thickness of the barrier layer is 8 to 15 nm; and / or The method of removing the portion of the prefabricated layer exposed through the block copolymer layer also includes removing the portion of the barrier layer exposed through the block copolymer layer. The method of removing the portion of the barrier layer exposed through the block copolymer layer includes: immersing the portion of the barrier layer exposed through the block copolymer layer in a second metal etching solution, wherein the second metal etching solution includes one or more of a palladium etching solution, a platinum etching solution, a rhodium etching solution, an iridium etching solution, and a ruthenium etching solution.

9. The preparation method according to claim 1, characterized in that: The material of the insulating layer includes one or more of SiO2 and Al2O3; and / or The material of the metal layer includes one or more of doped or undoped nickel, copper, molybdenum, titanium, zinc, and tin; and / or The first electrode comprises one or more of a metal, a carbon material and a metal oxide; the metal comprises one or more of Al, Ag, Cu, Mo, Au, Ba, Ca, Yb and Mg; the carbon material comprises one or more of graphite, carbon nanotubes, graphene and carbon fiber; the metal oxide comprises a metal oxide electrode or a composite electrode in which a metal is sandwiched between doped or undoped transparent metal oxides, the material of the metal oxide electrode comprises one or more of ITO, FTO, ATO, AZO, GZO, IZO, MZO and AMO, and the composite electrode comprises one or more of AZO / Ag / AZO, AZO / Al / AZO, ITO / Ag / ITO, ITO / Al / ITO, ZnO / Ag / ZnO, ZnO / Al / ZnO, ZnS / Ag / ZnS, ZnS / Al / ZnS, TiO2 / Ag / TiO2 and TiO2 / Al / TiO2; and / or The first carrier functional layer includes a hole functional layer or an electron functional layer; the hole functional layer includes 4,4'-N,N'-dicarbazolyl-biphenyl, N,N'-diphenyl-N,N'-bis(1-naphthyl)-1,1'-biphenyl-4,4"-diamine, N,N'-diphenyl-N,N'-bis(3-methylphenyl)-(1,1'-biphenyl)-4,4'-diamine (TPD), N,N'-bis(3-methylphenyl)-N,N'-bis(phenyl)-spiro, N,N'-bis(4-(N,N'-diphenyl-amino)phenyl)-N,N'-diphenylbenzidine, 4,4',4'-tri(N-carbazolyl)-triphenylamine, 4,4',4'-tri(carbazol-9-yl)-triphenylamine, Triphenylamine, trichloroisocyanuric acid, terbium-doped phosphate-based green luminescent materials, 2,3,6,7,10,11-hexacyano-1,4,5,8,9,12-hexaazatriphenylene, 4,4',4'-tri(N-3-methylphenyl-N-phenylamino)triphenylamine, poly[(9,9'-dioctylfluorene-2,7-diyl)-co-(4,4'-(N-(4-sec-butylphenyl)diphenylamine))], poly(4-butylphenyl-diphenylamine), poly[bis(4-phenyl)(4-butylphenyl)amine], polyaniline, polypyrrole, poly(p-phenylene vinylene), poly(phenylene vinylene), poly[2-methoxy-5-(2-ethylhexyloxy)-1,4-phenylene vinylene], Poly[2-methoxy-5-(3',7'-dimethyloctyloxy)-1,4-phenylene vinylene], copper phthalocyanine, aromatic tertiary amines, polynuclear aromatic tertiary amines, 4,4'-bis(p-carbazolyl)-1,1'-biphenyl compounds, N,N,N',N'-tetraaryl benzidine, PEDOT, PEDOT:PSS and its derivatives, PEDOT:PSS derivatives doped with s-MoO3, poly(N-vinyl carbazole) and its derivatives, polymethacrylate and its derivatives, poly(9,9-octylfluorene) and its derivatives, poly(spirofluorene) and its derivatives, N,N'-di(naphthalene-1-yl)-N,N'-diphenyl benzidine, spiro NPB, nano-polycrystalline diamond, microcrystalline cellulose and tetra One or more of cyanoquinodimethane, doped graphene, undoped graphene, transition metal oxides, transition metal sulfides, and transition metal tinides; the material of the electronic functional layer includes inorganic materials and / or organic materials, and the inorganic material includes one or more of doped or undoped zinc oxide, barium oxide, nickel oxide, titanium oxide, tin oxide, tantalum oxide, zirconium oxide, nickel oxide, lithium titanium oxide, zinc aluminum oxide, zinc manganese oxide, zinc tin oxide, lithium zinc oxide, indium tin oxide, cadmium sulfide, zinc sulfide, molybdenum sulfide, tungsten sulfide, copper sulfide, zinc tin, indium phosphide, gallium phosphide, copper indium sulfide, copper gallium sulfide, and barium titanate; the doped elements include one or more of aluminum, magnesium, lithium, manganese, yttrium, lanthanum, copper, nickel, zirconium, cerium, and gadolinium;The organic material includes one or more of quinoxaline compounds, imidazole compounds, triazine compounds, fluorene compounds, and hydroxyquinoline compounds; and / or; The second carrier functional layer includes a hole functional layer or an electron functional layer. When the second carrier functional layer is a hole functional layer, the material of the second carrier functional layer includes NiO x , CuO x 、MoO x When the second carrier functional layer is an electronic functional layer, the material of the second carrier functional layer includes ZnO x 、TiO x SnO x One or more of the following; and / or The forming of the light-emitting layer further comprises: disposing a light-emitting material on the surface of the patterned electrode-carrier recombination layer; and / or The luminescent materials include 4,4'-bis(N-carbazole)-1,1'-biphenyl:tris[2-(p-tolyl)pyridine iridium(III)], 4,4',4"-tris(carbazole-9-yl)triphenylamine:tris[2-(p-tolyl)pyridine iridium], diarylanthracene derivatives, distilbene aromatic derivatives, pyrene derivatives, fluorene derivatives, TBPe fluorescent materials, TTPX fluorescent materials, TBRb fluorescent materials, DBP fluorescent materials, delayed fluorescent materials, TTA materials, TADF materials, polymers containing covalent bonding of BN, HLCT materials, Exciplex luminescent materials, CdS, CdSe, CdTe, ZnS, ZnSe, ZnTe, ZnO, HgS, HgSe, H gTe, CdSeS, CdSeTe, CdSTe, ZnSeS, ZnSeTe, ZnSTe, HgSeS, HgSeTe, HgSTe, CdZnS, CdZnSe, CdZnTe, CdHgS, CdHgSe, CdHgTe, HgZnS, HgZnSe, HgZnTe, CdZ nSeS, CdZnSeTe, CdZnSTe, CdHgSeS, CdHgSeTe, CdHgSTe, HgZnSeS, HgZnSeTe, HgZnSTe, SnS, SnSe, SnTe, PbS, PbSe, PbTe, SnSeS, SnSeTe, SnSTe, PbSeS , PbSeTe, PbSTe, SnPbS, SnPbSe, SnPbTe, SnPbSSe, SnPbSeTe, SnPbSTe, GaN, GaP, GaAs, GaSb, AlN, AlP, AlAs, AlSb, InN, InP, InAs, InSb, GaNP, GaNAs, GaNSb, GaPAs, GaPSb, AlNP, AlNAs, AlNSb, AlPAs, AlPSb, InNP, InNAs, InNSb, InPAs, InPSb, GaAlNP, GaAlNAs, GaAlNSb, GaAlPAs, GaAlPSb, GaInNP, Ga InNAs, GaInNSb, GaInPAs, GaInPSb, InAlNP, InAlNAs, InAlNSb, InAlPAs, InAlPSb, CuInS2, CuInSe2, AgInS2, CdSe / CdSeS / CdS, InP / ZnSeS / ZnS, CdZn One or more of Se / ZnSe / ZnS, CdSeS / ZnSeS / ZnS, CdSe / ZnS, CdSe / ZnSe / ZnS, ZnSe / ZnS, ZnSeTe / ZnS, CdSe / CdZnSeS / ZnS, InP / ZnSe / ZnS, AMX3 and BMX3, where A is Cs + ion, M is a divalent metal cation selected from Pb 2+ Sn 2+ , Cu 2+ 、Ni 2+ 、Cd 2+ Cr 2+ , Mn 2+ 、Co 2+ , Fe 2+ ,Ge 2+ , Yb 2+ 、Eu 2+ One or more of the following, X is a halogen anion selected from Cl-, Br - , I-; B is an organic amine cation selected from CH3(CH2) n- 2NH3 + or [NH3(CH2) n NH3] 2+ , where n≥2.

10. A light emitting device, characterized in that: include: A stacked first electrode and a first carrier functional layer; A patterned functional layer, the patterned functional layer comprising a stacked insulating layer, a second electrode, and a second carrier functional layer, wherein the insulating layer and the second electrode are sequentially stacked on the first carrier functional layer, and the second carrier functional layer is arranged on a side surface of the second electrode and a surface of the second electrode away from the insulating layer; The light-emitting layer is disposed in the patterned gap in the patterned functional layer, and the thickness of the light-emitting layer is greater than the thickness of the insulating layer.

11. The light emitting device according to claim 10, characterized in that: The thickness of the light-emitting layer is less than or equal to the thickness of the patterned functional layer; or The light-emitting layer includes a first light-emitting portion and a plurality of second light-emitting portions, the first light-emitting portion having a first surface, the plurality of second light-emitting portions being arranged at intervals on the first surface and extending in a direction away from the first surface, the plurality of second light-emitting portions being filled in patterned gaps of the patterned functional layer, and an area of ​​the first surface where no second light-emitting portion is arranged is arranged on a surface of the second carrier functional layer away from the first carrier functional layer.

12. The light emitting device according to claim 10, characterized in that: The patterned functional layer further includes a barrier layer, and the barrier layer is arranged between the first carrier functional layer and the insulating layer.

13. The light emitting device according to claim 12, characterized in that: The material of the barrier layer includes one or more of palladium, platinum, rhodium, iridium and ruthenium; and / or The thickness of the barrier layer is 8 to 15 nm; and / or The thickness of the light emitting layer is greater than the sum of the thicknesses of the blocking layer and the insulating layer.

14. The light emitting device according to claim 10, characterized in that: The thickness of the first electrode is 90-110 nm; and / or The thickness of the first carrier functional layer is 20 to 40 nm; and / or The thickness of the insulating layer is 25 to 35 nm; and / or The thickness of the second carrier functional layer is 8 to 12 nm; and / or The thickness of the second electrode is 50-60 nm.

15. The light emitting device according to claim 10, characterized in that: The material of the insulating layer includes one or more of SiO2 and Al2O3; and / or The first electrode comprises one or more of a metal, a carbon material and a metal oxide; the metal comprises one or more of Al, Ag, Cu, Mo, Au, Ba, Ca, Yb and Mg; the carbon material comprises one or more of graphite, carbon nanotubes, graphene and carbon fiber; the metal oxide comprises a metal oxide electrode or a composite electrode in which a metal is sandwiched between doped or undoped transparent metal oxides, the material of the metal oxide electrode comprises one or more of ITO, FTO, ATO, AZO, GZO, IZO, MZO and AMO, and the composite electrode comprises one or more of AZO / Ag / AZO, AZO / Al / AZO, ITO / Ag / ITO, ITO / Al / ITO, ZnO / Ag / ZnO, ZnO / Al / ZnO, ZnS / Ag / ZnS, ZnS / Al / ZnS, TiO2 / Ag / TiO2 and TiO2 / Al / TiO2; and / or The first carrier functional layer includes a hole functional layer or an electron functional layer; the hole functional layer includes 4,4'-N,N'-dicarbazolyl-biphenyl, N,N'-diphenyl-N,N'-bis(1-naphthyl)-1,1'-biphenyl-4,4"-diamine, N,N'-diphenyl-N,N'-bis(3-methylphenyl)-(1,1'-biphenyl)-4,4'-diamine (TPD), N,N'-bis(3-methylphenyl)-N,N'-bis(phenyl)-spiro, N,N'-bis(4-(N,N'-diphenyl-amino)phenyl)-N,N'-diphenylbenzidine, 4,4',4'-tri(N-carbazolyl)-triphenylamine, 4,4',4'-tri(carbazol-9-yl)-triphenylamine, Triphenylamine, trichloroisocyanuric acid, terbium-doped phosphate-based green luminescent materials, 2,3,6,7,10,11-hexacyano-1,4,5,8,9,12-hexaazatriphenylene, 4,4',4'-tri(N-3-methylphenyl-N-phenylamino)triphenylamine, poly[(9,9'-dioctylfluorene-2,7-diyl)-co-(4,4'-(N-(4-sec-butylphenyl)diphenylamine))], poly(4-butylphenyl-diphenylamine), poly[bis(4-phenyl)(4-butylphenyl)amine], polyaniline, polypyrrole, poly(p-phenylene vinylene), poly(phenylene vinylene), poly[2-methoxy-5-(2-ethylhexyloxy)-1,4-phenylene vinylene], Poly[2-methoxy-5-(3',7'-dimethyloctyloxy)-1,4-phenylene vinylene], copper phthalocyanine, aromatic tertiary amines, polynuclear aromatic tertiary amines, 4,4'-bis(p-carbazolyl)-1,1'-biphenyl compounds, N,N,N',N'-tetraaryl benzidine, PEDOT, PEDOT:PSS and its derivatives, PEDOT:PSS derivatives doped with s-MoO3, poly(N-vinyl carbazole) and its derivatives, polymethacrylate and its derivatives, poly(9,9-octylfluorene) and its derivatives, poly(spirofluorene) and its derivatives, N,N'-di(naphthalene-1-yl)-N,N'-diphenyl benzidine, spiro NPB, nano-polycrystalline diamond, microcrystalline cellulose and tetra One or more of cyanoquinodimethane, doped graphene, undoped graphene, transition metal oxides, transition metal sulfides, and transition metal tinides; the material of the electronic functional layer includes inorganic materials and / or organic materials, and the inorganic material includes one or more of doped or undoped zinc oxide, barium oxide, nickel oxide, titanium oxide, tin oxide, tantalum oxide, zirconium oxide, nickel oxide, lithium titanium oxide, zinc aluminum oxide, zinc manganese oxide, zinc tin oxide, lithium zinc oxide, indium tin oxide, cadmium sulfide, zinc sulfide, molybdenum sulfide, tungsten sulfide, copper sulfide, zinc tin, indium phosphide, gallium phosphide, copper indium sulfide, copper gallium sulfide, and barium titanate; the doped elements include one or more of aluminum, magnesium, lithium, manganese, yttrium, lanthanum, copper, nickel, zirconium, cerium, and gadolinium;The organic material includes one or more of quinoxaline compounds, imidazole compounds, triazine compounds, fluorene compounds, and hydroxyquinoline compounds; and / or; The second carrier functional layer includes a hole functional layer or an electron functional layer. When the second carrier functional layer is a hole functional layer, the material of the second carrier functional layer includes NiO x , CuO x 、MoO x When the second carrier functional layer is an electronic functional layer, the material of the second carrier functional layer includes ZnO x 、TiO x SnO x One or more of; and / or The material of the second electrode includes one or more of Ni, Cu, Mo, Zn, Ti, and Sn; and / or The luminescent materials include 4,4'-bis(N-carbazole)-1,1'-biphenyl:tris[2-(p-tolyl)pyridine iridium(III)], 4,4',4"-tris(carbazole-9-yl)triphenylamine:tris[2-(p-tolyl)pyridine iridium], diarylanthracene derivatives, distilbene aromatic derivatives, pyrene derivatives, fluorene derivatives, TBPe fluorescent materials, TTPX fluorescent materials, TBRb fluorescent materials, DBP fluorescent materials, delayed fluorescent materials, TTA materials, TADF materials, polymers containing covalent bonding of BN, HLCT materials, Exciplex luminescent materials, CdS, CdSe, CdTe, ZnS, ZnSe, ZnTe, ZnO, HgS, HgSe, H gTe, CdSeS, CdSeTe, CdSTe, ZnSeS, ZnSeTe, ZnSTe, HgSeS, HgSeTe, HgSTe, CdZnS, CdZnSe, CdZnTe, CdHgS, CdHgSe, CdHgTe, HgZnS, HgZnSe, HgZnTe, CdZ nSeS, CdZnSeTe, CdZnSTe, CdHgSeS, CdHgSeTe, CdHgSTe, HgZnSeS, HgZnSeTe, HgZnSTe, SnS, SnSe, SnTe, PbS, PbSe, PbTe, SnSeS, SnSeTe, SnSTe, PbSeS , PbSeTe, PbSTe, SnPbS, SnPbSe, SnPbTe, SnPbSSe, SnPbSeTe, SnPbSTe, GaN, GaP, GaAs, GaSb, AlN, AlP, AlAs, AlSb, InN, InP, InAs, InSb, GaNP, GaNAs, GaNSb, GaPAs, GaPSb, AlNP, AlNAs, AlNSb, AlPAs, AlPSb, InNP, InNAs, InNSb, InPAs, InPSb, GaAlNP, GaAlNAs, GaAlNSb, GaAlPAs, GaAlPSb, GaInNP, Ga InNAs, GaInNSb, GaInPAs, GaInPSb, InAlNP, InAlNAs, InAlNSb, InAlPAs, InAlPSb, CuInS2, CuInSe2, AgInS2, CdSe / CdSeS / CdS, InP / ZnSeS / ZnS, CdZn One or more of Se / ZnSe / ZnS, CdSeS / ZnSeS / ZnS, CdSe / ZnS, CdSe / ZnSe / ZnS, ZnSe / ZnS, ZnSeTe / ZnS, CdSe / CdZnSeS / ZnS, InP / ZnSe / ZnS, AMX3 and BMX3, where A is Cs + ion, M is a divalent metal cation selected from Pb 2+ Sn 2+ , Cu 2+ 、Ni 2+ 、Cd 2+ Cr 2+ , Mn 2+ 、Co 2+ , Fe 2+ ,Ge 2+ , Yb 2+ 、Eu 2+ One or more of the following, X is a halogen anion selected from Cl-, Br - , I-; B is an organic amine cation selected from CH3(CH2) n- 2NH3 + or [NH3(CH2) n NH3] 2+ , where n≥2.

16. A display device, characterized in that: The invention comprises a light-emitting device prepared by the preparation method according to any one of claims 1 to 9, or a light-emitting device according to any one of claims 10 to 15.