A Micro-LED epitaxial structure and preparation method thereof
By depositing the insertion layers of AlN, GaSb and InGaN layers on the N-type doped GaN layer of Micro-LED, the stress and dislocation density problems caused by the heterogeneous substrate of GaN film are solved, and the inner quantum of Micro-LED is improved Efficiency and luminous performance.
Patent Information
- Application Number
- CN202411297495.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-18
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-09-18
AI Technical Summary
When growing Micro-LED, GaN films are lattice mismatch and stress problems caused by heterogeneous substrates, resulting in a decrease in crystal quality, high dislocation density, and affecting luminescence efficiency. The low-temperature growth of existing stress-regulating layer materials leads to additional increase in positions due to low temperature growth of existing stress-regulating layer materials, resulting in additional increases in positions. The wrong density is difficult to meet the high efficiency needs of Micro-LED.
The insertion layer of the AlN layer, the patterned GaSb layer, the Al metal layer and the InGaN layer are sequentially deposited on the N-type doped GaN layer, and the nanoscale Al metal particles and the patterned GaSb layer are formed by annealing to reduce the multi-quantum well layer. stress and dislocation density improve crystal quality.
It effectively reduces the stress and dislocation density of the multi-quantum well layer, improves the internal quantum efficiency of Micro-LED, improves the luminous brightness and anti-static properties, reduces lattice mismatch, and has good uniformity of luminous wavelengths.
Smart Images

Figure CN118825159B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of semiconductor materials, and in particular to a Micro-LED epitaxial structure and a preparation method thereof. Background Art
[0002] GaN material has the advantages of low heat generation efficiency, radiation resistance, high breakdown voltage, large electron saturation drift velocity and small dielectric constant. It has been widely used in high-frequency, high-temperature and high-voltage electronic devices, light-emitting diodes (LEDs) and semiconductor lasers (LDs), and has become a hot topic in current research.
[0003] There are many technical difficulties in the process of LED epitaxial growth. Due to the lack of substrate materials that match GaN, GaN films are currently mainly grown on SiC, Si, and patterned sapphire (PSS) substrates through heteroepitaxial methods. There are large lattice mismatches and thermal mismatches between heterogeneous substrates and GaN films. For example, the lattice mismatch between sapphire substrates and GaN is 17%, and the thermal mismatch is 34%. The lattice mismatch between Si substrates and GaN is 20%, and the thermal mismatch is 56%. When GaN-based LEDs are grown on sapphire substrates through heteroepitaxial methods, there is a large lattice mismatch between GaN and the sapphire substrate, which causes a large amount of stress to accumulate in the epitaxial layer. The stress caused by the lattice mismatch will cause the crystal quality of GaN films to deteriorate, and the dislocation density of GaN films can reach as high as 10 8 ~10 10 cm -2 , high-density dislocations may form leakage channels and non-radiative recombination centers in GaN-based devices, resulting in a decrease in the luminous efficiency of LEDs. In addition, due to the lattice mismatch, there is a polarization electric field between the well barriers, which causes the energy bands of the well barriers to tilt, the electron-hole distribution in the quantum wells to be uneven, the electron-hole wave function overlap rate to decrease, and the radiative recombination efficiency to decrease, affecting the internal quantum efficiency, which seriously limits the performance and application of light-emitting diodes. In order to improve the luminous efficiency of LEDs, it is necessary to prepare epitaxial layer structures with high radiative recombination efficiency and high crystal quality.
[0004] In particular, due to the small size of Micro-LED and the low injection current density, its optoelectronic performance is very sensitive to dislocation density. Dislocations, as non-radiative recombination centers and leakage channels, will significantly affect the chip performance of Micro-LED. Under the same epitaxial structure and the same chip structure, the reduction in size and surface area of Micro-LED will lead to a decrease in single-core brightness, which puts higher requirements on luminous efficiency. Therefore, Micro-LED requires epitaxial wafers with lower defect density.
[0005] At present, the growth of GaN thin film on heterogeneous substrate by MOCVD method of Micro-LED will cause large stress due to lattice mismatch. Lattice mismatch will lead to the reduction of crystal quality of epitaxial layer, and will also introduce some dislocations and defects, which will eventually reduce the growth quality of InGaN quantum well, and then lead to the reduction of luminous efficiency of Micro-LED. Therefore, it is necessary to improve the stress of InGaN quantum well. Usually, a stress regulation layer is introduced between n-type doped GaN and InGaN light-emitting active area, which can effectively alleviate the stress and polarization of InGaN light-emitting active area caused by lattice mismatch between substrate and GaN, and provide a better epitaxial foundation for InGaN light-emitting active area, thereby improving the internal quantum efficiency of light-emitting diode. The stress regulation layer material of conventional method is low-temperature grown GaN / InGaN material, which releases the stress accumulated in the bottom layer by sacrificing the quality of GaN / InGaN crystal at low temperature growth. The poor crystal quality of low-temperature grown GaN / InGaN stress regulation layer itself will increase the dislocation density, so that the internal quantum efficiency of LED cannot reach the optimal state, and it is difficult to meet the application of Micro-LED. Summary of the invention
[0006] The technical problem to be solved by the present invention is to provide a Micro-LED epitaxial structure and a preparation method thereof, which can reduce the stress during the growth of InGaN quantum wells, improve the crystal quality of the multi-quantum well layer, and thus improve the internal quantum efficiency of the Micro-LED.
[0007] In order to solve the above technical problems, the first aspect of the present invention provides a Micro-LED epitaxial structure, comprising a substrate, a buffer layer, an undoped GaN layer, an N-type doped GaN layer, an insertion layer, a multi-quantum well layer, an electron blocking layer, a P-type doped GaN layer and a contact layer stacked sequentially on the substrate;
[0008] Wherein, the insertion layer comprises an AlN layer, a patterned GaSb layer, an Al metal layer and an InGaN layer which are sequentially arranged on the N-type doped GaN layer.
[0009] As an improvement of the above solution, the method for growing the insertion layer includes:
[0010] (1) Depositing an AlN layer, a GaSb layer, and an Al metal layer in sequence on the N-type doped GaN layer;
[0011] (2) performing a first annealing treatment to form a nano-scale Al metal particle layer;
[0012] (3) performing a second annealing process to decompose the exposed GaSb layer to form a patterned GaSb layer;
[0013] (4) Continue to deposit the InGaN layer to obtain.
[0014] As an improvement of the above solution, the temperature of the first annealing treatment is 970° C. to 1050° C., the annealing pressure is 50 torr to 100 torr, the annealing atmosphere is H2, and the annealing time is 10 s to 100 s.
[0015] As an improvement of the above solution, the temperature of the second annealing treatment is 770° C. to 830° C., the annealing pressure is 50 torr to 100 torr, the annealing atmosphere is H2, and the annealing time is 5 min to 10 min.
[0016] As an improvement of the above solution, the In composition in the InGaN layer is 0.1-0.5.
[0017] As an improvement of the above solution, the thickness of the AlN layer is less than the thickness of the GaSb layer;
[0018] The thickness of the GaSb layer is greater than the thickness of the Al metal layer.
[0019] As an improvement of the above solution, the thickness of the AlN layer is 1nm~10nm;
[0020] The thickness of the GaSb layer is 50nm~200nm;
[0021] The thickness of the Al metal layer is 1 nm to 5 nm.
[0022] As an improvement of the above solution, the thickness of the Al metal layer is less than the thickness of the InGaN layer;
[0023] The thickness of the InGaN layer is 50nm-200nm.
[0024] As an improvement of the above scheme, in step (1), the growth temperature of depositing the AlN layer is 1000° C. to 1100° C., and the growth pressure is 30 torr to 50 torr;
[0025] The growth temperature of depositing the patterned GaSb layer is 500° C. to 700° C., and the growth pressure is 50 torr to 100 torr;
[0026] The growth temperature of the Al metal layer is 700° C. to 800° C., and the growth pressure is 30 torr to 50 torr;
[0027] In step (4), the growth temperature for depositing the InGaN layer is 700° C. to 800° C., and the growth pressure is 50 torr to 100 torr.
[0028] The second aspect of the present invention further provides a method for preparing the epitaxial structure of the Micro-LED, comprising:
[0029] providing a substrate;
[0030] depositing a buffer layer on the substrate;
[0031] depositing an undoped GaN layer on the buffer layer;
[0032] Depositing an N-type doped GaN layer on the undoped GaN layer;
[0033] depositing an insertion layer on the N-type doped GaN layer;
[0034] depositing a multi-quantum well layer on the insertion layer;
[0035] depositing an electron blocking layer on the multiple quantum well layer;
[0036] depositing a P-type doped GaN layer on the electron blocking layer;
[0037] depositing a contact layer on the P-type doped GaN layer;
[0038] The insertion layer includes an AlN layer, a patterned GaSb layer, an Al metal layer and an InGaN layer which are sequentially arranged on the N-type doped GaN layer.
[0039] The implementation of the present invention has the following beneficial effects:
[0040] An insertion layer is arranged between the N-type doped GaN layer and the multi-quantum well layer, and the insertion layer includes an AlN layer, a patterned GaSb layer, an Al metal layer and an InGaN layer arranged in sequence on the N-type doped GaN layer, which can reduce the stress when growing the multi-quantum well layer, reduce the dislocation density of the multi-quantum well layer, and improve the crystal quality of the multi-quantum well layer, thereby improving the internal quantum efficiency of the Micro-LED. At the same time, it can also improve the ohmic contact, reduce the operating voltage, increase the luminous brightness, improve the antistatic performance, and reduce the lattice mismatch with the multi-quantum well layer, so that the luminous wavelength is controllable and the uniformity of the luminous wavelength is good. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 : A schematic diagram of the structure of a Micro-LED epitaxial structure in the present invention;
[0042] Figure 2 : Schematic diagram of the preparation of the insertion layer in the epitaxial structure of Micro-LED in the present invention;
[0043] Figure 3 : A schematic diagram of the structure of the epitaxial structure of the Micro-LED after step (2) in the present invention is completed;
[0044] Figure 4 : A schematic diagram of the structure of the epitaxial structure of the Micro-LED after step (3) of the present invention is completed;
[0045] Figure 5 : Schematic diagram of the structure of the epitaxial structure of the Micro-LED after step (4) in the present invention is completed.
[0046] Reference numerals:
[0047] 21-substrate; 22-buffer layer; 23-undoped GaN layer; 24-N-type doped GaN layer; 25-insertion layer; 251-AlN layer; 252-patterned GaSb layer; 253-Al metal layer; 254-InGaN layer; 26-multiple quantum well layer; 27-electron blocking layer; 28-P-type doped GaN layer; 29-contact layer. DETAILED DESCRIPTION
[0048] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is further described in detail with specific embodiments below.
[0049] At present, in order to make the epitaxial wafer meet the application of Micro-LED, a GaN layer with good crystal quality is also grown between the N-type doped GaN layer 24 and the multi-quantum well layer 26, and then the GaN layer is etched. However, the etching process will introduce etching damage and affect the crystal quality of the material. In addition, the etching process requires secondary epitaxy, which will also bring additional contamination particles.
[0050] To solve the above problems, the present invention provides a Micro-LED epitaxial structure in a first aspect, such as Figure 1 As shown, it includes a substrate 21, a buffer layer 22, an undoped GaN layer 23, an N-type doped GaN layer 24, an insertion layer 25, a multi-quantum well layer 26, an electron blocking layer 27, a P-type doped GaN layer 28 and a contact layer 29 stacked in sequence on the substrate 21;
[0051] The insertion layer 25 includes an AlN layer 251 , a patterned GaSb layer 252 , an Al metal layer 253 and an InGaN layer 254 which are sequentially arranged on the N-type doped GaN layer 24 .
[0052] In the present invention, an insertion layer 25 is provided between the N-type doped GaN layer 24 and the multi-quantum well layer 26, which can reduce the stress during the growth of the multi-quantum well layer 26, reduce the dislocation density of the multi-quantum well layer 26, and improve the crystal quality of the multi-quantum well layer 26, thereby improving the internal quantum efficiency of the Micro-LED.
[0053] Furthermore, a patterned GaSb layer 252 is provided in the insertion layer 25, which has a function similar to that of a patterned sapphire substrate (PSS), and can induce dislocations to bend toward the sidewalls of the pattern, thereby reducing dislocations propagating upward. In addition, the GaSb sublayer nanopattern causes the photons generated by the multi-quantum well layer 26 to be reflected multiple times through the microstructure, which can change the propagation path of the photons and increase the probability of photons escaping, so that the photons are more likely to be emitted to the outside, thereby enhancing the light output efficiency of the Micro-LED. The provision of the Al metal layer 253 is conducive to the formation of the patterned GaSb layer 252 and protects the patterned Ga The Sb layer 252 will not be decomposed in a high temperature environment. At the same time, the setting of the Al metal layer 253 can prevent electrons from being directly injected from the N-type doped GaN layer 24 into the P-type doped GaN layer 28, thereby reducing electron leakage, improving the brightness of the device, and reducing the operating voltage of the device. The AlN layer 251 can act as an isolation layer to protect the N-type doped GaN layer 24 from being decomposed. Finally, a layer of InGaN layer 254 can fill the graphic structure of the patterned GaSb layer 252, which is beneficial to the subsequent deposition of the multi-quantum well layer 26, while improving the ohmic contact, further reducing the operating voltage, and improving the luminous brightness.
[0054] Furthermore, in the present invention, the insertion layer 25 is prepared by the coordinated cooperation of the AlN layer 251, the patterned GaSb layer 252, the Al metal layer 253 and the InGaN layer 254 under the annealing process. Specifically, Figure 2~Figure 5 As shown, the method for growing the insertion layer 25 includes:
[0055] (1) depositing an AlN layer 251, a GaSb layer, and an Al metal layer 253 in sequence on the N-type doped GaN layer 24;
[0056] (2) performing a first annealing treatment to form a nano-scale Al metal particle layer;
[0057] (3) performing a second annealing process to decompose the exposed GaSb layer to form a patterned GaSb layer 252;
[0058] (4) Continue to deposit the InGaN layer 254 to obtain.
[0059] When growing the insertion layer 25, two annealing treatments are performed to form a patterned GaSb sublayer, which can reduce the stress accumulated on the N-type doped GaN layer 24, thereby reducing the stress during the growth of the multi-quantum well layer 26, and can reduce the dislocation density of the multi-quantum well layer 26, improve the crystal quality of the multi-quantum well layer 26, and increase the probability of photon reflection in the multi-quantum well layer 26, ultimately improving the luminous efficiency of the Micro-LED. The InGaN layer 254 can fill in the patterned GaSb sublayer after annealing and decomposition, and the smaller bandgap width of GaSb (0.73eV) can release the stress accumulated in the bottom GaN.
[0060] In step (1), if Figure 2 As shown, the growth temperature for depositing the AlN layer 251 is 1000°C~1100°C, and the growth pressure is 30torr~50torr; the growth temperature for depositing the GaSb layer is 500°C~700°C, and the growth pressure is 50torr~100torr; the growth temperature for depositing the Al metal layer 253 is 700°C~800°C, and the growth pressure is 30torr~50torr.
[0061] Preferably, the thickness of the AlN layer 251 is less than that of the GaSb layer; during the annealing process, the AlN layer 251 can act as an isolation layer to prevent the bottom N-type doped GaN layer 24 from being decomposed during the annealing process. If the thickness of the AlN layer 251 is too thick, cracks will occur and affect the subsequent growth. The thickness of the AlN layer 251 is 1nm~10nm, exemplarily 1nm, 2nm, 3nm, 4nm, 5nm, 6nm, 7nm, 8nm, 9nm, 10nm, but not limited thereto; the thickness of the GaSb layer is 50nm~200nm, exemplarily 50nm, 75nm, 100nm, 125nm, 150nm, 175nm, 200nm, but not limited thereto.
[0062] Furthermore, the thickness of the patterned GaSb layer 252 is greater than the thickness of the Al metal layer 253. If the thickness of the Al metal layer 253 is too thick, the GaSb layer cannot be exposed in the first annealing process, and the patterned GaSb layer 252 cannot be formed; if the thickness of the Al metal layer 253 is too thin, it cannot play a masking role in the second annealing process, and the blocking effect on electrons is weakened, reducing the luminous brightness of the device. The thickness of the Al metal layer 253 is 1nm~5nm, and exemplarily 1nm, 2nm, 3nm, 4nm, 5nm, but not limited to this, specifically referring to the laying thickness of the Al metal layer 253.
[0063] In step (2), if Figure 3As shown. The temperature of the first annealing treatment is 970℃~1050℃, the annealing pressure is 50torr~100torr, the annealing atmosphere is H2, and the annealing time is 10s~100s. In the H2 atmosphere, the Al metal film is in an unstable state at a high temperature of 970℃~1050℃. The deposited Al metal film layer will break under the action of surface tension and shrink into a ball under a pressure of 50torr~100torr, eventually forming nano-scale Al metal particles on the surface of the material, exposing part of the underlying GaSb layer.
[0064] In step (3), if Figure 4 The temperature of the second annealing treatment is 770°C to 830°C, the annealing pressure is 50 torr to 100 torr, the annealing atmosphere is H2, and the annealing time is 5 min to 10 min. GaSb material will decompose above 700°C. When the temperature of the second annealing treatment is 770°C~830°C, the exposed GaSb layer will decompose, and the nano-scale Al metal particles formed by the first annealing treatment can be used as a mask to prevent the GaSb film covered by the nano-scale Al metal particles from decomposing, thereby forming a patterned GaSb layer 252. By controlling the annealing pressure to 50torr~100torr and the annealing time to 5min~10min, the decomposition thickness of the GaSb layer can be controlled, thereby controlling the formation of defects on the surface of the patterned GaSb layer 252. If the annealing time is too short, GaSb cannot be effectively decomposed and a pattern cannot be formed. The undecomposed GaSb will introduce defects in the subsequent epitaxial growth and affect the luminous efficiency. However, if the annealing time is too long, it will be over-decomposed or even completely decomposed, and a pattern cannot be formed, and ultimately the luminous efficiency cannot be improved.
[0065] In step (4), if Figure 5 As shown, the growth temperature of depositing the InGaN layer 254 is 700° C. to 800° C., and the growth pressure is 50 torr to 100 torr.
[0066] Furthermore, the In composition in the InGaN layer 254 is 0.1-0.5, which is beneficial to reducing the lattice mismatch with the multi-quantum well layer 26, making the emission wavelength controllable and having good uniformity of the emission wavelength.
[0067] Furthermore, the thickness of the Al metal layer 253 is less than that of the InGaN layer 254, which can not only fill the surface shape of the patterned GaSb layer 252, but also improve the light-emitting performance of the device. The thickness of the InGaN layer 254 is 50nm~200nm, and exemplary thicknesses are 50nm, 75nm, 100nm, 125nm, 150nm, 175nm, and 200nm, but are not limited thereto.
[0068] Accordingly, the present invention also provides a method for preparing the epitaxial structure of the Micro-LED, comprising:
[0069] S01, providing a substrate 21;
[0070] Preferably, the substrate 21 may be a sapphire substrate, a Si substrate or the like.
[0071] S02, depositing a buffer layer 22 on the substrate 21;
[0072] Preferably, the buffer layer 22 is an AlN buffer layer, and the thickness of the buffer layer 22 is 15 nm to 50 nm.
[0073] Furthermore, the buffer layer 22 is grown by PVD, the growth temperature is controlled to be 400° C. to 650° C., the sputtering power is controlled to be 2000W to 4000W, the growth pressure is controlled to be 1 torr to 10 torr, and Al source and N source are introduced for deposition.
[0074] Furthermore, after the growth of the buffer layer 22 is completed, an in-situ annealing treatment can be performed in MOCVD, the annealing atmosphere is H2, the annealing temperature is 1000°C~1200°C, the annealing pressure is 150torr~500torr, the annealing time is 5min~10min, and the subsequent deposition processes are all performed in MOCVD.
[0075] S03, depositing an undoped GaN layer 23 on the buffer layer 22;
[0076] Preferably, the undoped GaN layer 23 has a thickness of 1.0 μm to 3.0 μm.
[0077] Furthermore, in MOCVD, the growth temperature is controlled to be 1050° C. to 1200° C., the growth pressure is controlled to be 100 torr to 500 torr, and Ga source and N source are introduced for deposition.
[0078] S04, depositing an N-type doped GaN layer 24 on the undoped GaN layer 23;
[0079] Preferably, the doping element of the N-type doped GaN layer 24 is Si, and the doping concentration of Si is 1×10 19 cm -3 ~1×10 20 cm -3 The thickness of the N-type doped GaN layer 24 is 1.0 μm to 3.0 μm.
[0080] Furthermore, the growth temperature is controlled to be 1100° C. to 1200° C., the growth pressure is 100 torr to 300 torr, and Si source, Ga source and N source are introduced for deposition.
[0081] S05, depositing an insertion layer 25 on the N-type doped GaN layer 24;
[0082] The insertion layer 25 includes an AlN layer 251 , a patterned GaSb layer 252 , an Al metal layer 253 and an InGaN layer 254 which are sequentially disposed on the N-type doped GaN layer 24 .
[0083] (1) First, the growth temperature is controlled to be 1000° C. to 1100° C., the growth pressure is 30 torr to 50 torr, and an Al source and a N source are introduced to deposit the AlN layer 251. Exemplary growth temperatures are 1000° C., 1020° C., 1040° C., 1060° C., 1080° C., and 1100° C., but are not limited thereto; exemplary growth pressures are 30 torr, 35 torr, 40 torr, 45 torr, and 50 torr, but are not limited thereto.
[0084] Subsequently, the growth temperature is controlled to be 500° C. to 700° C., the growth pressure is 50 torr to 100 torr, and a Ga source and a Sb source are introduced to deposit the GaSb layer. Exemplary growth temperatures are 500° C., 525° C., 550° C., 575° C., 600° C., 625° C., 650° C., 675° C., and 700° C., but are not limited thereto; exemplary growth pressures are 50 torr, 60 torr, 70 torr, 80 torr, 90 torr, and 100 torr, but are not limited thereto.
[0085] Finally, the growth temperature is controlled to be 700° C. to 800° C., the growth pressure is 30 torr to 50 torr, and an Al source is introduced to deposit the Al metal layer 253 to form an Al layer. Exemplary growth temperatures are 700° C., 725° C., 750° C., 775° C., and 800° C., but not limited thereto; exemplary growth pressures are 30 torr, 35 torr, 40 torr, 45 torr, and 50 torr, but not limited thereto.
[0086] (2) performing a first annealing treatment to transform the Al layer into a nano-scale Al metal particle layer and expose a portion of the GaSb layer; the temperature of the first annealing treatment is 970° C. to 1050° C., the annealing pressure is 50 torr to 100 torr, the annealing atmosphere is H2, and the annealing time is 10 s to 100 s;
[0087] (2) performing a second annealing treatment to decompose the exposed patterned GaSb layer 252 to form a patterned GaSb layer 252; the temperature of the second annealing treatment is 770°C to 830°C, the annealing pressure is 50 torr to 100 torr, the annealing atmosphere is H2, and the annealing time is 5 min to 10 min.
[0088] (3) Controlling the growth temperature to 700° C.-800° C. and the growth pressure to 50 torr-100 torr, introducing In source, Ga source and N source to deposit the InGaN layer 254, exemplary growth temperatures are 700° C., 725° C., 750° C., 775° C., 800° C., but not limited thereto; exemplary growth pressures are 50 torr, 60 torr, 70 torr, 80 torr, 90 torr, 100 torr, but not limited thereto.
[0089] S06, depositing a multi-quantum well layer 26 on the insertion layer 25;
[0090] Preferably, the multi-quantum well layer 26 is a periodic structure of alternately stacked InGaN quantum well layers and GaN quantum barrier layers, with a stacking period number of 5 to 12. In a single period, the In component of the InGaN quantum well layer is 0.1 to 0.5, the thickness of the InGaN quantum well layer is 2 nm to 4 nm, and the thickness of the GaN quantum barrier layer is 8 nm to 20 nm.
[0091] Further, the growth temperature is controlled to be 800° C. to 900° C., the growth pressure is 100 torr to 300 torr, and the In source, Ga source and N source are introduced to deposit the InGaN quantum well layer; then, the growth temperature is controlled to be 900° C. to 1000° C., the growth pressure is 100 torr to 300 torr, and the Ga source and N source are introduced to deposit the GaN quantum barrier layer to complete one growth cycle, and then the InGaN quantum well layer and the GaN quantum barrier layer are continued to be repeatedly stacked and grown periodically.
[0092] S07, depositing an electron blocking layer 27 on the multi-quantum well layer 26;
[0093] Preferably, the electron blocking layer 27 is an AlGaN layer, the Al component is 0.1-0.5, and the thickness of the electron blocking layer 27 is 50nm-100nm.
[0094] Furthermore, the growth temperature is controlled to be 950° C. to 1050° C., the growth pressure is controlled to be 50 torr to 100 torr, and N source, Ga source and Al source are introduced to deposit the electron blocking layer 27 .
[0095] S08, depositing a P-type doped GaN layer 28 on the electron blocking layer 27;
[0096] Preferably, the doping element of the P-type doped GaN layer 28 is Mg, and the doping concentration of Mg is 1×10 19 cm -3 ~1×10 20 cm -3The thickness of the P-type doped GaN layer 28 is 30 nm to 100 nm.
[0097] Furthermore, the growth temperature is controlled to be 950° C. to 1050° C., the growth pressure is controlled to be 100 torr to 600 torr, and N source, Ga source and Mg source are introduced to deposit the P-type doped GaN layer 28 .
[0098] S09, depositing a contact layer 29 on the P-type doped GaN layer 28;
[0099] Preferably, the contact layer 29 is a P-type contact layer 29, and the doping element is Mg, and the doping concentration of Mg is 1×10 19 cm -3 ~1×10 20 cm -3 The thickness of the contact layer 29 is 10 nm to 30 nm.
[0100] Furthermore, the growth temperature is controlled to be 1000° C. to 1100° C., the growth pressure is controlled to be 100 torr to 300 torr, and Mg source, Ga source and N source are introduced to deposit the contact layer 29 .
[0101] In some preferred embodiments, the method for preparing the epitaxial structure of the Micro-LED further includes:
[0102] S10, after the epitaxial structure growth is completed, annealing treatment is performed and then cooled to room temperature.
[0103] Preferably, the annealing treatment is performed in a N2 atmosphere, the annealing treatment temperature is 700°C to 800°C, and the treatment time is 8min to 15min.
[0104] It should be noted that in the present invention, Veeco C4 MOCVD (Metal Organic Chemical Vapor Deposition) equipment is used to realize the growth method of epitaxial wafers during MOCVD deposition. A mixed gas of high-purity H2 (hydrogen) and high-purity N2 is used as a carrier gas; the N source is high-purity NH3, the Al source is TMAl (trimethylaluminum), the Ga source is TMGa (trimethylgallium) or TEGa (triethylgallium), the In source is TMIn (trimethylindium), the Sb source is SbH3 (antimonide), the Si source is SiH4, and the Mg source is CP2Mg.
[0105] The present invention will be further described below with specific embodiments:
[0106] Example 1
[0107] This embodiment provides a Micro-LED epitaxial structure, including a substrate, a buffer layer, an undoped GaN layer, an N-type doped GaN layer, an insertion layer, a multi-quantum well layer, an electron blocking layer, a P-type doped GaN layer and a contact layer stacked in sequence on the substrate;
[0108] Wherein, the insertion layer comprises an AlN layer, a patterned GaSb layer, an Al metal layer and an InGaN layer which are sequentially arranged on the N-type doped GaN layer.
[0109] The thickness of the AlN layer is 5 nm, the thickness of the GsSb layer is 80 nm; the laying thickness of the Al metal layer is 2 nm; the In component of the InGaN layer is 0.3, and the thickness is 80 nm.
[0110] It is prepared by the following preparation method:
[0111] S01, providing a substrate;
[0112] The substrate is a sapphire substrate.
[0113] S02, depositing a buffer layer on the substrate;
[0114] The buffer layer is an AlN buffer layer with a thickness of 50 nm.
[0115] The buffer layer was grown by PVD, with Al source and N source introduced, and the growth temperature was controlled to be 520°C, the sputtering power was 3000W, and the pressure was 5torr to grow the buffer layer. Subsequently, in MOCVD, under H2 atmosphere, the temperature was adjusted to 1100°C and the pressure was 300torr for annealing for 7 minutes.
[0116] S03, depositing an undoped GaN layer on the buffer layer;
[0117] The reaction temperature was adjusted to 1175° C. and the reaction pressure was adjusted to 250 torr. Ga source and N source were introduced to grow the undoped GaN layer with a thickness of 2.0 μm.
[0118] S04, depositing an N-type doped GaN layer on the undoped GaN layer;
[0119] The doping element of the N-type doped GaN layer is Si, and the doping concentration of Si is 5×10 19 cm -3 .
[0120] The reaction temperature was adjusted to 1150° C. and the reaction pressure was adjusted to 200 torr. Si source, Ga source and N source were introduced to grow the N-type doped GaN layer with a thickness of 2.0 μm.
[0121] S05, depositing an insertion layer on the N-type doped GaN layer;
[0122] (1) First, the reaction temperature was maintained at 1050°C and the reaction pressure was adjusted to 35 torr, and Al source and N source were introduced to grow an AlN layer; then, the reaction temperature was adjusted to 600°C and the reaction pressure was adjusted to 80 torr, and Ga source and Sb source were introduced to grow a GaSb layer; finally, the reaction temperature was adjusted to 750°C and the reaction pressure was adjusted to 35 torr, and Al source was introduced to grow an Al metal layer to form an Al layer;
[0123] (2) Raise the temperature to 1000°C, maintain the reaction pressure at 75 torr, and perform the first step of rapid annealing in a H2 annealing atmosphere for 30 seconds;
[0124] (3) The temperature was lowered to 800°C, the reaction pressure was maintained at 75 torr, and a second annealing treatment was performed in a H2 annealing atmosphere for 8 minutes to form a patterned GaSb layer.
[0125] (4) Maintaining the reaction temperature at 750°C and adjusting the reaction pressure to 80 torr, In source, In source and N source were introduced to grow the InGaN layer.
[0126] S06. Depositing a multi-quantum well layer on the insertion layer
[0127] The multi-quantum well layer is a periodic structure of alternately stacked InGaN quantum well layers and GaN quantum barrier layers, and the number of stacking periods is 8. In a single period, the In component of the InGaN quantum well layer is 0.3, the thickness of the InGaN quantum well layer is 3nm, and the thickness of the GaN quantum barrier layer is 15nm.
[0128] The reaction temperature is adjusted to 850° C. and the reaction pressure is adjusted to 200 torr. N source, Ga source and In source are introduced to grow the InGaN quantum well layer. Subsequently, the temperature of the reaction chamber is controlled to 950° C., the In source is turned off, and Ga source and N source are introduced to grow the GaN quantum barrier layer to complete one cycle of growth. Subsequently, the InGaN quantum well layer and the GaN quantum barrier layer are repeatedly stacked and grown periodically.
[0129] S07, depositing an electron blocking layer on the multi-quantum well layer;
[0130] The electron blocking layer is an AlGaN layer, and the Al composition is 0.3.
[0131] The reaction temperature was adjusted to 1000° C., the reaction pressure was adjusted to 75 torr, and N source, Ga source and Al source were introduced to grow the electron blocking layer with a thickness of 75 nm.
[0132] S08, depositing a P-type doped GaN layer on the electron blocking layer;
[0133] The doping element of the P-type doped GaN layer is Mg, and the doping concentration of Mg is 5×10 19 cm -3 .
[0134] The reaction temperature was maintained at 1000° C., the reaction pressure was adjusted to 350 torr, and N source, Ga source and Mg source were introduced to grow the P-type doped GaN layer with a thickness of 70 nm.
[0135] S09, depositing a contact layer on the P-type doped GaN layer;
[0136] The contact layer is a P-type contact layer, and the doping element is Mg, and the doping concentration of Mg is 5×10 19 cm -3 .
[0137] The reaction temperature was adjusted to 1050° C., the growth pressure was adjusted to 200 torr, and Mg source, Ga source and N source were introduced to grow the P-type contact layer with a thickness of 20 nm.
[0138] S10. After the epitaxial structure growth is completed, the temperature of the reaction chamber is lowered, and annealing is performed in a N2 atmosphere at a temperature of 750°C for 10 minutes, and then the temperature is cooled to room temperature to obtain the epitaxial structure of Micro-LED.
[0139] Embodiments 2 to 13 are basically the same as Embodiment 1, except for the correlation coefficients of the layers in the insertion layer. The relevant parameters of the specific insertion layer are shown in Table 1 below.
[0140] Table 1 Parameter settings of the insertion layer in Examples 1 to 13
[0141]
[0142] Comparative Example 1
[0143] This comparative example provides a Micro-LED epitaxial structure, which is basically the same as Example 1, except that no insertion layer is included.
[0144] Comparative Example 2
[0145] This comparative example provides a Micro-LED epitaxial structure, which is basically the same as that of Example 1, except that:
[0146] Wherein, the insertion layer comprises an AlN layer, an Al metal layer and an InGaN layer which are sequentially arranged on the N-type doped GaN layer.
[0147] Comparative Example 3
[0148] This comparative example provides a Micro-LED epitaxial structure, which is basically the same as Example 1, except that: wherein the insertion layer includes an AlN layer, a patterned GaSb layer and an InGaN layer sequentially disposed on the N-type doped GaN layer.
[0149] Comparative Example 4
[0150] This comparative example provides a Micro-LED epitaxial structure, which is basically the same as that of Example 1, except that:
[0151] Wherein, the insertion layer comprises a patterned GaSb layer, an Al metal layer and an InGaN layer which are sequentially arranged on the N-type doped GaN layer.
[0152] The photoelectric performance of the chip with a size of 9*11mil made of the epitaxial structure obtained in the embodiment and the comparative example was tested. The specific testing method of the chip is as follows: when a current of 60mA is passed, the luminous brightness, operating voltage, luminous wavelength and luminous uniformity of the obtained chip are tested;
[0153] Antistatic performance test: The antistatic performance of the base chip is tested using an electrostatic meter under the HBM (Human Body Model) model to test the pass rate of the chip that can withstand reverse 6kV static electricity.
[0154] The performance test results are shown in Table 2.
[0155] Table 2 Performance test results of examples and comparative examples
[0156]
[0157] From the above results, it can be seen that the insertion layer is set between the N-type doped GaN layer and the multi-quantum well layer, and the insertion layer includes an AlN layer, a patterned GaSb layer, an Al metal layer and an InGaN layer sequentially set on the N-type doped GaN layer, which can reduce the stress when growing the multi-quantum well layer and improve the internal quantum efficiency of the Micro-LED. At the same time, it can also reduce the operating voltage, increase the luminous brightness, improve the antistatic performance, and make the luminous wavelength uniform. By keeping the thickness of each layer in the insertion layer within a certain range and performing annealing treatment at a certain temperature range for a certain time, the various performances of the LED chip can be improved.
[0158] The above disclosure is only a preferred embodiment of the present invention, which certainly cannot be used to limit the scope of the present invention. Therefore, equivalent changes made according to the claims of the present invention are still within the scope of the present invention.
Claims
1. A Micro-LED epitaxial structure, characterized in that: It comprises a substrate, a buffer layer, an undoped GaN layer, an N-type doped GaN layer, an insertion layer, a multi-quantum well layer, an electron blocking layer, a P-type doped GaN layer and a contact layer which are sequentially stacked on the substrate; The insertion layer includes an AlN layer, a patterned GaSb layer, an Al metal layer and an InGaN layer which are sequentially arranged on the N-type doped GaN layer.
2. The epitaxial structure of Micro-LED according to claim 1, characterized in that: The method for growing the insertion layer comprises: (1) Depositing an AlN layer, a GaSb layer, and an Al metal layer in sequence on the N-type doped GaN layer; (2) performing a first annealing treatment to form a nano-scale Al metal particle layer; (3) performing a second annealing process to decompose the exposed GaSb layer to form a patterned GaSb layer; (4) Continue to deposit the InGaN layer to obtain.
3. The epitaxial structure of Micro-LED according to claim 2, characterized in that: The temperature of the first annealing treatment is 970° C. to 1050° C., the annealing pressure is 50 torr to 100 torr, the annealing atmosphere is H 2 , and the annealing time is 10 s to 100 s.
4. The epitaxial structure of a Micro-LED according to claim 2, wherein: The temperature of the second annealing treatment is 770° C. to 830° C., the annealing pressure is 50 torr to 100 torr, the annealing atmosphere is H2, and the annealing time is 5 min to 10 min.
5. The epitaxial structure of Micro-LED according to claim 1, characterized in that: The In composition of the InGaN layer is 0.1-0.
5.
6. The epitaxial structure of a Micro-LED according to claim 2, wherein: The thickness of the AlN layer is less than the thickness of the GaSb layer; The thickness of the GaSb layer is greater than the thickness of the Al metal layer.
7. The epitaxial structure of Micro-LED according to claim 6, characterized in that: The thickness of the AlN layer is 1 nm to 10 nm; The thickness of the GaSb layer is 50nm~200nm; The thickness of the Al metal layer is 1 nm to 5 nm.
8. The epitaxial structure of Micro-LED according to claim 7, characterized in that: The thickness of the Al metal layer is less than the thickness of the InGaN layer; The thickness of the InGaN layer is 50nm-200nm.
9. The epitaxial structure of Micro-LED according to claim 2, characterized in that: In step (1), the growth temperature of the AlN layer is 1000° C. to 1100° C., and the growth pressure is 30 torr to 50 torr; The growth temperature of depositing the patterned GaSb layer is 500° C. to 700° C., and the growth pressure is 50 torr to 100 torr; The growth temperature of the Al metal layer is 700° C. to 800° C., and the growth pressure is 30 torr to 50 torr; In step (4), the growth temperature for depositing the InGaN layer is 700° C. to 800° C., and the growth pressure is 50 torr to 100 torr.
10. A method for preparing a Micro-LED epitaxial structure according to any one of claims 1 to 9, characterized in that: include: providing a substrate; depositing a buffer layer on the substrate; depositing an undoped GaN layer on the buffer layer; Depositing an N-type doped GaN layer on the undoped GaN layer; depositing an insertion layer on the N-type doped GaN layer; depositing a multi-quantum well layer on the insertion layer; depositing an electron blocking layer on the multiple quantum well layer; depositing a P-type doped GaN layer on the electron blocking layer; depositing a contact layer on the P-type doped GaN layer; The insertion layer includes an AlN layer, a patterned GaSb layer, an Al metal layer and an InGaN layer which are sequentially arranged on the N-type doped GaN layer.
Citation Information
Patent Citations
Light emitting diode (LED) epitaxial wafer with N type insertion layer with trapezoidal structure and growth method thereof
CN103165777A